A medical material containing decellularized biological tissue material
By combining blocking agents and cross-linking agents, the problem of degradation time and three-dimensional structure regulation of decellularized biological tissue materials in existing technologies has been solved, achieving efficient and simple antigen blocking and degradation cycle regulation, and reducing immune risks.
Patent Information
- Application Number
- CN202310074159.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-01-14
- Filing Date
- 2023-01-13
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-01-13
AI Technical Summary
Existing technologies for controlling the degradation time and three-dimensional structure of decellularized biological tissue materials have problems such as cumbersome operation, long time consumption, high cost, or decreased antigen blocking rate and increased immune risk.
By using a combination of blocking and cross-linking agents, and adjusting the molar ratio of the blocking and cross-linking agents as well as the reaction conditions, the degree of cross-linking of decellularized biological tissues can be regulated, maintaining a high antigen blocking rate and adjusting the degradation cycle.
It effectively regulates the degradation cycle of decellularized biological tissues, improves reaction efficiency, avoids the decrease in antigen blocking rate caused by simply changing the temperature, time, and concentration of the cross-linking agent, reduces the risk of immunity, and simplifies the process.
Smart Images

Figure CN116440312B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of biomedical materials, and in particular relates to a medical material containing decellularized biological tissue material. Background Art
[0002] Decellularized biological tissue materials are a new type of biomaterial that uses physical or chemical methods to decellularize allogeneic or xenogeneic tissues, thereby removing the related antigens that cause rejection reactions during tissue transplantation, and are used to repair damaged tissues. Due to their low immunogenicity and good biocompatibility, they are widely used in the field of medical devices, such as biological patches, wound dressings, tissue fillings, engineering scaffolds, etc.
[0003] When the decellularized materials in the prior art are used as repair materials or scaffolds, their own safety, biocompatibility, and mechanical strength need to be considered. Due to the inherent structure of the material, it is difficult to control the degradation time and three-dimensional structure, and the mechanical strength is poor. In order to adjust the degradation time, it is generally achieved by changing the cross-linking degree.
[0004] Patent document CN 105999410 A discloses a decellularized tissue matrix composite material and a preparation method thereof, wherein the composite material is prepared by crushing the decellularized tissue matrix, adding water or digestion fluid, mixing with polyelectrolytes, and freeze-drying. However, the material does not solve the problem of antigen blocking rate of the material.
[0005] Patent document CN 109498830 A discloses changing the degree of cross-linking by changing the temperature. Although this method can make the degree of cross-linking of decellularized biological tissues adjustable, the antigen blocking rate of decellularized biological tissues decreases as the degree of cross-linking decreases, increasing the risk of immune response caused by antigen exposure.
[0006] Patent document CN 109833119 A discloses a cross-linking method for improving the biocompatibility of a decellularized matrix, wherein the cleaned decellularized matrix is immersed in a glycidyl methacrylate solution for cross-linking. This method has a complex process, is time-consuming, and has relatively low production efficiency.
[0007] Patent document CN 105935454 A discloses a method of first using a strong hydrogen bonding agent to thoroughly remove antigens from biological tissues, then using an epoxy compound for cross-linking, and then adjusting the degradation cycle of decellularized biological tissues by changing the concentration and reaction time of the epoxy compound. Although this method avoids the disadvantage of reducing the antigen blocking rate of biological tissues due to reducing the degree of cross-linking, its process is complicated and time-consuming. It can be seen from the above-mentioned prior art that most of the methods for adjusting the degradation cycle of decellularized biological tissues to make them suitable for multiple indications still have the defects of cumbersome operation, long time consumption, high cost, reduced antigen blocking rate, increased immune risk, etc. Summary of the invention
[0008] In order to solve the above-mentioned deficiencies of the prior art, the present invention provides a medical material containing acellular biological tissue material.
[0009] The purpose of the present invention is achieved through the following technical solutions:
[0010] The present invention provides a medical material containing a cell-free biological tissue material, wherein the cell-free biological tissue material is prepared by the following method, which comprises: after the biological tissue is decellularized and defatted, a cross-linking treatment is performed, wherein the cross-linking step is performed by adding a blocking agent and a cross-linking agent to a reaction solution;
[0011] The molar ratio of the blocking agent to the cross-linking agent is 0-40:0-20, and the molar ratio of the blocking agent to the cross-linking agent is 0 when the blocking agent and the cross-linking agent are not used.
[0012] The blocking agent and the cross-linking agent have the same site that mainly reacts with the amino group or carboxyl group of the amino acid.
[0013] The blocking agent has a single reaction site that mainly reacts with the amino group or carboxyl group of the amino acid, and the cross-linking agent has two or more reaction sites that mainly react with the amino group or carboxyl group of the amino acid.
[0014] The antigenicity of biological tissues is mainly caused by certain amino acid residues in proteins, such as -OH, -NH 2 , -COOH, etc., the active groups in collagen can be blocked by adding active reagents that react with these groups (such as acid anhydrides, alkyl halides and epoxides, etc.), thereby achieving the purpose of effectively removing antigens.
[0015] Preferably, the medical materials include materials used for repairing, filling and replacing human tissues;
[0016] The materials used for tissue repair include: wound dressings, dental repair materials, bone or cartilage repair materials, chest and / or abdominal wall repair patches, anal fistula repair patches, gastric or lung resection repair patches, dura mater patches, spinal dura mater patches, scleral repair patches, anti-adhesion patches, and nerve conduits;
[0017] Materials used for tissue filling include: rhinoplasty filling materials, breast filling materials, facial filling materials, hand filling materials, buttock filling materials, genital filling materials, filling materials after otitis media surgery, and filling materials after thyroid surgery;
[0018] Materials used for tissue replacement include: biological valves, artificial blood vessels, artificial tear ducts, artificial organs, artificial tendons, and artificial corneas.
[0019] More preferably, the medical materials include: wound dressings, dental repair materials, chest and / or abdominal wall repair patches, dura mater patches, spinal dura mater patches, sclera repair patches, breast filling materials, facial filling materials, and hand filling materials.
[0020] Further, the reaction solution comprises any one of component I and component II;
[0021] The component I comprises: a blocking agent I and a cross-linking agent I;
[0022] The component II includes: a blocking agent II and a cross-linking agent II;
[0023] The sealing agent I is an epoxy compound I, and the epoxy compound I is selected from one or more of glycidol, 2-(oxetane-3-yl)ethane-1-ol, epichlorohydrin, and butyl glycidyl ether;
[0024] The crosslinking agent I is a polyepoxy epoxy compound, which contains 2 to 4 epoxy groups and is selected from one or more of 1,4-butanediol diglycidyl ether, ethylene glycol diglycidyl ether, glycerol triglycidyl ether, and pentaerythritol glycidyl ether; preferably, the polyepoxy epoxy compound contains 2 epoxy groups.
[0025] The blocking agent II is an aldehyde compound selected from: one or more of acetaldehyde, n-propionaldehyde, and n-valeraldehyde;
[0026] The crosslinking agent II is a polyaldehyde compound containing 2 to 4 aldehyde groups, selected from one or more of glutaraldehyde, adipaldehyde, 1,3-butanedialdehyde, trimesic acid, and 1,2,4,5-pyromellitic acid; preferably, the polyaldehyde compound contains 2 aldehyde groups.
[0027] In the component I, the blocking agent is glycidol, and the cross-linking agent is 1,4-butanediol diglycidyl ether;
[0028] In the component II, the blocking agent is acetaldehyde, and the cross-linking agent is 1,4-butanediol diglycidyl ether.
[0029] Furthermore, the reaction solution further comprises a solvent, and the solvent comprises: a combination of one or more of water, dimethyl sulfoxide, N,N-dimethylformamide, tetrahydrofuran, diethyl ether, dioxane, pyridine, acetonitrile, ethyl acetate, diethyl ether, isopropyl ether, dichloromethane, chloroform, ethyl bromide, benzene, chloropropane, toluene, carbon tetrachloride, carbon disulfide, cyclohexane, hexane, heptane or kerosene.
[0030] In the component I, the molar ratio of the blocking agent I to the cross-linking agent I is 0-25:0-20, and the blocking agent and the cross-linking agent are not zero at the same time;
[0031] And / or, the ratio of the epoxy group molar concentration of the blocking agent I or the crosslinking agent I in the component I to the total epoxy group molar concentration (the sum of the epoxy group molar concentrations of the blocking agent and the crosslinking agent) is in the range of 0 to 100%; and the blocking agent and the crosslinking agent are not simultaneously 0.
[0032] Preferably, in the component I, the molar ratio of the blocking agent I to the cross-linking agent I is 0 to 20:0:10;
[0033] Preferably, in the component I, the molar ratio of the blocking agent I to the crosslinking agent I is 1:10 to 25:1;
[0034] More preferably, in the component I, the molar ratio of the blocking agent I to the crosslinking agent I is 1:5 to 20:1;
[0035] In a specific embodiment of the present invention, the molar ratio of the blocking agent I to the cross-linking agent I can be 1:1, 1:5, 2:1, 12:1, or 20:1.
[0036] In the component II, the molar ratio of the blocking agent II to the crosslinking agent II is 0-25:0-20;
[0037] And / or, the ratio of the aldehyde group molar concentration of the blocking agent II or the crosslinking agent II in the component II to the total aldehyde group molar concentration (the sum of the epoxy group molar concentrations of the blocking agent and the crosslinking agent) is in the range of 0 to 100%; and the blocking agent and the crosslinking agent are not simultaneously 0.
[0038] Preferably, in the component II, the molar ratio of the blocking agent II to the crosslinking agent II is 0-20:0-10;
[0039] Preferably, in the component II, the molar ratio of the blocking agent II to the crosslinking agent II is 1:10 to 25:1;
[0040] More preferably, in the component II, the molar ratio of the blocking agent II to the crosslinking agent II is 1:5 to 20:1;
[0041] In a specific embodiment of the present invention, the molar ratio of blocking agent II to cross-linking agent II can be 1:1, 1:5, 2:1, 12:1, or 20:1.
[0042] and / or, in the component I, the epoxy group molar ratio of the blocking agent I and the crosslinking agent I is 1:10 to 10:1;
[0043] For example, the molar ratio of epoxy groups of the blocking agent I and the crosslinking agent I can be 1:10, 1:9, 1:8, 1:7, 1:6, 1:5, 1:4, 1:3, 1:2, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, and 10:1.
[0044] In the component II, the molar ratio of the aldehyde groups of the blocking agent II and the cross-linking agent II is 1:10 to 10:1;
[0045] For example, the molar ratio of the aldehyde groups of the blocking agent II and the cross-linking agent II can be 1:10, 1:9, 1:8, 1:7, 1:6, 1:5, 1:4, 1:3, 1:2, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, and 10:1.
[0046] When the molar concentration ratio of the crosslinking agent I in the component I accounts for 90% to 100% of the total concentration ratio, the medical material is selected from a scleral repair patch and a biological valve.
[0047] When the molar concentration ratio of the crosslinking agent I in the component I accounts for 10% to 90% of the total concentration ratio, the medical material is selected from dura mater patches, spinal dura mater patches, hernia patches, breast plastic surgery patches, and facial filling materials.
[0048] When the molar concentration ratio of the crosslinking agent I in the component I accounts for 0% to 10% of the total concentration ratio, the medical material is selected from wound dressings or oral filling materials.
[0049] When the molar concentration ratio of the crosslinking agent II in the component II accounts for 90% to 100% of the total concentration ratio, the medical material is selected from a scleral repair patch and a biological valve.
[0050] When the molar concentration ratio of the crosslinking agent II in the component II accounts for 10% to 90% of the total concentration ratio, the medical material is selected from dura mater patches, spinal dura mater patches, hernia patches, breast plastic surgery patches, and facial filling materials.
[0051] When the molar concentration ratio of the crosslinking agent II in the component II accounts for 0% to 10% of the total concentration ratio, the medical material is selected from wound dressings or oral filling materials.
[0052] Further, the solvent of component I is an alkaline solvent, and the solvent I further comprises one or more of the following components: sodium hydroxide, potassium hydroxide, calcium hydroxide, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, sodium sulfite, potassium sulfite, preferably, the solvent further comprises sodium carbonate;
[0053] And / or, the solvent of component II is an alkaline solvent, the pH value of the solvent of component II is 6-9, preferably, the pH value of the solvent is 7-8.
[0054] The total epoxy group molar concentration in the component I is 0.1M to 3M;
[0055] Preferably, the total epoxy group molar concentration in the component I is 0.5 to 2M;
[0056] The crosslinking treatment soaking temperature of the component I is 25-45°C,
[0057] Preferably, the cross-linking treatment immersion temperature of component I is 30-40°C;
[0058] The crosslinking treatment soaking time of component I is 5 to 72 hours;
[0059] Preferably, the cross-linking treatment immersion time of component I is 15 to 30 hours.
[0060] The total aldehyde molar concentration in the component II is 0.01M to 2M;
[0061] Preferably, the total aldehyde molar concentration in the component II is 0.1 to 1 M;
[0062] The crosslinking treatment soaking temperature of the component II is 20 to 45°C;
[0063] Preferably, the crosslinking treatment immersion temperature of component II is 25 to 30°C;
[0064] The crosslinking treatment soaking time of component II is 10 to 96 hours;
[0065] Preferably, the cross-linking treatment immersion time of component II is 24 to 48 hours.
[0066] Further, the biological tissue includes dermal tissue, blood vessels, digestive tract, organ membrane, body cavity membrane, amniotic membrane, biological valve, cartilage tissue, bone tissue, muscle tissue, adipose tissue, tendon, organ; preferably, the biological tissue is animal pericardium;
[0067] And / or, the cross-linking treatment process is: immersing the animal pericardium in a mixed cross-linking solution.
[0068] The present invention also provides a method for preparing a medical material, the method comprising:
[0069] A. Material collection: Select biological tissue materials.
[0070] B Pretreatment: destroy the cells of biological tissue materials through freeze-thaw technology; trim and remove impurities and irregular parts on the biological tissue materials.
[0071] C Alkaline treatment: The biological tissue material is treated with an alkaline solution, neutralized with a weak acid, and washed.
[0072] D Deproteinization: Use surfactants and protein solubilizers to remove water-soluble and lipid proteins from biological tissue materials
[0073] Soluble proteins;
[0074] E. Removal of lipid impurities: Use medium polarity organic solvents to remove residual lipids in the tissue;
[0075] F Cross-linking: Cross-linking biological tissue materials with a reaction solution, the reaction solution contains a cross-linking agent and a blocking agent, wherein the more the cross-linking agent is used, the higher the degree of cross-linking;
[0076] G. Remove residual reagents: Use water to repeatedly soak and clean the tissue to remove residual reagents.
[0077] H Sterilization: Sterilize the tissue after cutting and packaging.
[0078] Preferably, in step C, the alkaline solution is sodium hydroxide, the weak acid is citric acid, and the washing times are 3 times;
[0079] Preferably, the medium polar organic solvent in step E is ethanol or ethyl acetate;
[0080] Preferably, the water in step G is purified water, water for injection or physiological saline;
[0081] Preferably, the sterilization in step H is gamma-ray irradiation sterilization (cobalt-60), and step H also includes a packaging process.
[0082] In step D, the surfactant includes one or more components selected from surfactants, buffer salts, inorganic salts, thiol compounds, etc. The surfactant includes, but is not limited to, one or more selected from sodium dodecyl sulfate, sodium dodecyl sulfate, Tween-20, Tween-40, Tween-60, Tween-80, Triton X-100, etc.
[0083] The protein solubilizing agent includes but is not limited to at least one of urea and guanidine hydrochloride.
[0084] The present invention provides an application of a biological tissue material in preparing a medical material for repairing, filling and replacing human tissue.
[0085] Furthermore, the present invention uses decellularized biological tissue for tissue repair, and the process for preparing chest and / or abdominal wall repair patches, dura mater patches, spinal dura mater patches, and sclera repair patches includes: taking biological tissue materials, freeze-thaw trimming, alkali treatment, protein removal, removal of lipid impurities, medium to high degree cross-linking, removal of residual reagents and sterilization.
[0086] Furthermore, the present invention uses decellularized biological tissue to repair tissue defects with a faster reconstruction speed, and the process for preparing wound dressings and oral filling materials includes: taking biological tissue materials, freeze-thaw trimming, alkali treatment, protein removal, lipid impurity removal, thickening, low-degree cross-linking, removal of residual reagents, freeze-drying and sterilization.
[0087] Furthermore, the present invention uses decellularized biological tissue for tissue filling, and the process for preparing breast filling materials, facial filling materials and hand filling materials generally includes: taking biological tissue materials, freeze-thaw trimming, alkali treatment, protein removal, removal of lipid impurities, medium and low degree cross-linking, removal of residual reagents, granulation, sterilization, and preparation.
[0088] Beneficial effects of the present invention:
[0089] 1. The present invention adopts a compound of a blocking agent and a cross-linking agent to cross-link the decellularized biological tissue, keeps the total molar concentration of reactive groups in the system unchanged, and can maintain a relatively high antigen blocking rate. By changing the molar concentration ratio of reactive groups contained in the cross-linking agent component in the system, the cross-linking degree of the decellularized biological tissue is regulated, so that the degradation cycle of the decellularized biological tissue can be regulated while maintaining a relatively high antigen blocking rate, thereby avoiding the problem of a decrease in the antigen blocking rate of the biological tissue and an increase in the immune risk caused by simply changing the reaction temperature, time, concentration and other factors of the cross-linking agent, and also avoiding the problem of increased process complexity and time consumption caused by first completely removing the antigen and then adjusting the cross-linking degree.
[0090] 2. The present invention adds the blocking agent and the cross-linking agent at the same time, and the cross-linking agent and the blocking agent can enter the decellularized biological tissue at the same time. The concentrations of the cross-linking agent and the blocking agent in the microenvironment inside the decellularized biological tissue are relatively high, which is conducive to the reaction. Compared with adding them separately, the reaction efficiency can be effectively improved; if the cross-linking agent is added first, the pores of the decellularized biological tissue become smaller after being cross-linked, which will increase the difficulty of the blocking agent entering, resulting in a decrease in the antigen blocking rate; if the blocking agent is added first, the blocking agent preferentially occupies the reaction sites. When the cross-linking agent enters, the cross-linking efficiency will also be reduced due to the length of the cross-linking agent carbon chain and the reduction in reaction sites.
[0091] 3. The simultaneous addition of the blocking agent and the cross-linking agent can not only regulate the degradation cycle of the decellularized tissue, but also increase the concentration difference between the inside and outside of the initial membrane, which is more conducive to the penetration of the cross-linking agent and the blocking agent and accelerates the reaction process. In addition, since the cross-linking agent and the blocking agent are activated in the reaction system and are in an unstable state, they can quickly penetrate into the reaction, so that the cross-linking agent and the blocking agent can react at a relatively high concentration, thereby improving the utilization rate of the cross-linking agent and the blocking agent. BRIEF DESCRIPTION OF THE DRAWINGS
[0092] Figure 1 This is the degradation curve of the pericardium after cross-linking with different molar concentration ratios of propylene oxide and BDDE. DETAILED DESCRIPTION
[0093] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.
[0094] In the present invention, the term "crosslinking" refers to the process of converting a linear polymer with chemical reactivity into a three-dimensional network (body) polymer through a chemical reaction. It is often used for polymer modification.
[0095] In the present invention, the term "BDDE" refers to 1,4-butanediol diglycidyl ether, which is a water-soluble epoxy resin. It is a yellow transparent liquid with an epoxy value of 0.63-0.74 and a viscosity of 15-20 mPa·s. It is prepared by polycondensation of 1,4-butanediol and epichlorohydrin. It is often used in combination with bisphenol A epoxy resin to prepare low-viscosity composites, casting plastics, impregnation solutions, adhesives, coatings and resin modifiers.
[0096] In the present invention, the term "crosslinking agent" refers to an agent that can generate chemical bonds between linear molecules to connect the linear molecules to form a network structure, and is used to improve the strength of polymer materials.
[0097] In the present invention, the term "blocking agent" refers to a reagent that can block the active groups in collagen to achieve the purpose of effectively removing antigens.
[0098] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0099] Example
[0100] Example 1: Crosslinking agent is epoxy
[0101] The ratio of the molar concentration of epoxy groups in glycidol to the molar concentration of total epoxy groups is 100% (sample group 1): the pericardium after decellularization and defatting was taken and placed in a 0.1 M sodium carbonate aqueous solution with a glycidol concentration of 1.5 M, and immersed at 35° C. for 30 h.
[0102] The molar concentration ratio of epoxy groups of propylene oxide to BDDE was 1:1 (sample group 2): the pericardium after decellularization and defatting was taken and placed in a 0.001 M sodium hydroxide aqueous solution with a propylene oxide concentration of 0.75 M and a BDDE concentration of 0.375 M, and immersed at 35°C for 24 h.
[0103] The molar concentration ratio of epoxy groups of propylene oxide to BDDE was 1:2 (sample group 3): the pericardium after decellularization and defatting was taken and placed in a 0.01 M sodium hydroxide aqueous solution with a glycidol concentration of 0.5 M and a BDDE concentration of 0.5 M, and immersed at 35°C for 15 h.
[0104] The molar concentration ratio of epoxy groups of propylene oxide to BDDE was 1:3 (sample group 4): the pericardium after decellularization and defatting was placed in a 0.2 M sodium carbonate aqueous solution with a propylene oxide concentration of 0.375 M and a BDDE concentration of 0.563 M, and immersed at 35°C for 30 h.
[0105] The molar concentration of epoxy groups of BDDE accounts for 100% of the molar concentration of total epoxy groups (sample group 5): the pericardium after decellularization and defatting was taken and placed in a 0.01M sodium carbonate aqueous solution with a BDDE concentration of 0.75M, and immersed at 35°C for 19h.
[0106] The molar concentration ratio of epoxy groups of propylene oxide to BDDE was 10:1 (sample group 6): the pericardium after decellularization and defatting was placed in a 0.001 M sodium hydroxide solution with a propylene oxide concentration of 1.36 M and a BDDE concentration of 0.068 M, and immersed at 35°C for 24 h.
[0107] The molar concentration ratio of epoxy groups of propylene oxide to BDDE is 6:1 (sample group 7): the pericardium after decellularization and defatting was taken and placed in a 0.001M sodium hydroxide solution with a propylene oxide concentration of 1.29M and a BDDE concentration of 0.107M, and immersed at 35°C for 24h.
[0108] The molar concentration ratio of epoxy groups of propylene oxide to BDDE was 1:10 (sample group 8): the pericardium after decellularization and defatting was placed in a 0.001 M sodium hydroxide solution with a propylene oxide concentration of 0.136 M and a BDDE concentration of 0.68 M, and immersed at 35° C. for 24 h.
[0109] The molar concentration ratio of epichlorohydrin to ethylene glycol diglycidyl ether epoxy group was 1:10 (sample group 9): the pericardium after decellularization and defatting was placed in a 0.001 M sodium hydroxide solution with a concentration of 0.136 M of propylene oxide and 0.68 M of ethylene glycol diglycidyl ether, and immersed at 35°C for 24 h.
[0110] 1.1 Degradation performance
[0111] The pericardium prepared according to the conditions in Example 1 was cut into pieces and then degraded in vitro using type I collagenase. The degradation rate of each sample at different times was recorded. The results are shown in Table 1.
[0112] Table 1 Degradation rate of each sample at different enzymatic hydrolysis times in Example 1
[0113]
[0114]
[0115] The pericardium contains a large amount of type I collagen. Under alkaline conditions, epoxy compounds are easy to open the ring and react with primary amino groups, carboxyl groups, secondary amines, etc. with strong nucleophilic ability in collagen amino acids, thereby causing cross-linking reactions. From the data in Table 1, it can be seen that the degradation rate of the pericardium treated with a single sealing agent, propylene glycol, is still relatively fast even if the total epoxy group molar concentration remains unchanged. The decellularized biological tissue prepared under this condition is suitable for repairing tissue defects with a fast reconstruction speed, such as wound dressings or oral filling materials; with the increase of BDDE content, the degradation rate of the pericardium gradually decreases. When the pericardium is treated with a single cross-linking agent, BDDE, its degradation rate is extremely slow. The decellularized biological tissue prepared under this condition is suitable for replacing tissue protective membranes that degrade slowly or even do not need to be degraded in vivo, such as the posterior sclera of ophthalmology; and the pericardium cross-linked within the two extreme conditions can be used in dura mater patches, spinal dura mater patches, hernia patches, breast plastic surgery patches, etc. according to their different degradation times.
[0116] 1.2 Antigen blocking rate
[0117] The pericardium prepared according to the conditions in Example 1 was cut into pieces and then the antigen blocking rate was tested. The results are shown in Table 2.
[0118] Table 2 Antigen blocking rate of each sample
[0119] Cross-linking conditions Antigen blocking rate Sample set 1 97.89% Sample set 2 97.54% Sample set 3 98.12% Sample set 4 97.56% Sample set 5 98.35%
[0120] As can be seen from Table 2, the decellularized biological tissues prepared by the present invention have high antigen blocking rates, all reaching more than 97%, even though the cross-linking degrees are different. The decellularized biological tissues prepared by the present invention have good biocompatibility, and the same raw materials can be adapted to the needs of different indications by adjusting the degradation cycle.
[0121] 1.3 Degradation rate of pericardium at different immersion temperatures
[0122] The pericardium of sample group 2 that had been decellularized and defatted was taken and placed in a 0.001 M sodium hydroxide solution with a glycidol concentration of 0.75 M and a BDDE concentration of 0.375 M, and immersed at 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, and 50°C for 24 h, respectively.
[0123] Each pericardium was taken, cut into pieces, and then degraded in vitro using type I collagenase. The degradation rate of each sample at different times was recorded. The results are shown in Table 3.
[0124] Table 3 Degradation rate of each sample at different enzymatic hydrolysis time
[0125] Temperature is one of the main factors affecting the reaction between decellularized biological tissue and epoxy compounds. The increase in temperature can increase the frequency of intermolecular collisions, so that the molecules quickly have the activation energy required for the reaction, thereby accelerating the reaction. However, too high a temperature can also cause the epoxy compounds themselves to open their rings, resulting in a decrease in the reaction rate. From the data in Table 3, it can be seen that when the immersion temperature is 30-40°C, the degradation trend of the pericardium is basically the same, and its degradation rate is relatively slow under the conditions of the cross-linking liquid ratio, indicating that within this temperature range, the cross-linking degree of the pericardium is consistent and it is the optimal immersion temperature; when the immersion temperatures are 25°C and 45°C, respectively, the former has a slightly lower temperature and a slightly decreased reaction rate, resulting in a relatively slightly accelerated degradation rate under the condition of the same cross-linking time, while the latter has a slightly higher temperature than the optimal temperature, which causes a few epoxy compounds to open their rings, resulting in a slightly reduced reaction rate, so the degradation rate is slightly accelerated; and when the immersion temperature is lower than 25°C or higher than 45°C, the degradation rate of the pericardium is significantly accelerated.
[0126] Example 2: Crosslinking agent is aldehyde
[0127] The ratio of the molar concentration of acetaldehyde to the total molar concentration of aldehydes is 100% (sample group 1): the pericardium after decellularization and defatting was taken and placed in an aqueous solution with an acetaldehyde concentration of 0.6 M and a pH of 7, and immersed at 30° C. for 48 hours.
[0128] The molar concentration ratio of aldehyde groups of acetaldehyde to glutaraldehyde was 1:1 (sample group 2): the pericardium after decellularization and defatting was placed in an aqueous solution with an acetaldehyde concentration of 0.3 M, a glutaraldehyde concentration of 0.15 M, and a pH of 7.4, and immersed at 30°C for 48 h.
[0129] The molar concentration ratio of aldehyde groups of acetaldehyde to glutaraldehyde was 1:2 (sample group 3): the pericardium after decellularization and defatting was taken and placed in an aqueous solution with an acetaldehyde concentration of 0.2 M, a glutaraldehyde concentration of 0.2 M, and a pH of 8, and immersed at 30°C for 24 h.
[0130] The ratio of the molar concentration of aldehyde groups of glutaraldehyde to the molar concentration of total aldehyde groups is 100% (sample group 4): the pericardium after decellularization and defatting was taken and placed in an aqueous solution with a glutaraldehyde concentration of 0.3 M and a pH of 7, and immersed at 30° C. for 24 hours.
[0131] The ratio of the molar concentration of glutaraldehyde to the total molar concentration of aldehydes was 100% (sample group 5): the pericardium after decellularization and defatting was placed in an aqueous solution with a glutaraldehyde concentration of 0.3 M and a pH of 7, and immersed at 20° C. for 24 h.
[0132] The ratio of the molar concentration of aldehyde groups of glutaraldehyde to the molar concentration of total aldehyde groups is 100% (sample group 6): the pericardium after decellularization and defatting was taken and placed in an aqueous solution with a glutaraldehyde concentration of 0.3 M and a pH of 7, and immersed at 45° C. for 24 hours.
[0133] The molar concentration ratio of aldehyde groups of acetaldehyde to glutaraldehyde was 10:1 (sample group 7): the pericardium after decellularization and defatting was placed in a solution with an acetaldehyde concentration of 1.36 M, a glutaraldehyde concentration of 0.068 M, and a pH of 7.4, and immersed at 30°C for 48 h.
[0134] The molar concentration ratio of aldehyde groups of acetaldehyde to glutaraldehyde was 6:1 (sample group 8): the pericardium after decellularization and defatting was placed in a solution with an acetaldehyde concentration of 1.29 M, a glutaraldehyde concentration of 0.107 M, and a pH of 7.4, and immersed at 30°C for 48 h.
[0135] The molar concentration ratio of aldehyde groups of acetaldehyde to glutaraldehyde was 1:10 (sample group 9): the pericardium after decellularization and defatting was placed in a solution with an acetaldehyde concentration of 0.136 M, a glutaraldehyde concentration of 0.68 M, and a pH of 7.4, and immersed at 30°C for 48 h.
[0136] The molar concentration ratio of propionaldehyde to adipaldehyde was 1:10 (sample group 10): the pericardium after decellularization and defatting was placed in a solution with a propionaldehyde concentration of 0.136 M, an adipaldehyde concentration of 0.68 M, and a pH of 7.4, and immersed at 30°C for 48 h.
[0137] 2.1 Degradation performance
[0138] The pericardium prepared according to the conditions in Example 2 was cut into pieces and then degraded in vitro using type I collagenase. The degradation rate of each sample at different times was recorded. The results are shown in Table 4.
[0139] Table 4 Degradation rate of each sample at different enzymatic hydrolysis time
[0140]
[0141] From the data in Table 4, it can be seen that the degradation trend of the pericardium treated with epoxy crosslinkers is similar to that of the pericardium treated with a single sealer, acetaldehyde. The degradation rate of the pericardium is faster, and as the glutaraldehyde content increases, the degradation rate of the pericardium gradually decreases. When the pericardium is treated with a single crosslinker, glutaraldehyde, the degradation rate is relatively slow overall. In addition, when the immersion temperature is 20°C and 45°C, respectively, the degradation rate is faster than that of the sample group with an immersion temperature of 30°C.
[0142] Example 3: Multi-component mixed sealant or cross-linker
[0143] 1) Sample Group 1: The decellularized and defatted pericardium was placed in a 0.1 M sodium carbonate aqueous solution containing 0.75 M 2-(oxetane-3-yl)ethane-1-ol, 0.2 M BDDE and 0.175 M ethylene glycol diglycidyl ether, and immersed at 37°C for 24 h.
[0144] 2) Sample Group 2: The pericardium after decellularization and defatting was placed in an aqueous solution with a pH of 7.4 and a concentration of 0.2 M propionaldehyde, 0.15 M glutaraldehyde, and 0.15 M adipaldehyde, and was immersed at 25° C. for 36 h.
[0145] 3.1 Degradation performance
[0146] The pericardium prepared according to the conditions in Examples 1-2 was cut into pieces and then degraded in vitro using type I collagenase. The degradation rate of each sample at different times was recorded. The results are shown in Table 5.
[0147] Table 5 Degradation rate of each sample at different enzymatic hydrolysis time
[0148]
[0149] Embodiment 4:
[0150] The crosslinking agent is epoxy type:
[0151] Sample Group 1: The preparation method is similar to that of Sample Group 2 in Example 1.
[0152] Sample group 2: The pericardium after decellularization and defatting was placed in a 0.001 M sodium hydroxide aqueous solution with a BDDE concentration of 0.375 M and immersed at 35° C. for 24 h.
[0153] Crosslinking agent is aldehyde
[0154] Sample group 3: Preparation method refers to sample group 2 in Example 2;
[0155] Sample group 4: The pericardium after decellularization and defatting was placed in an aqueous solution with a glutaraldehyde concentration of 0.15 M and a pH of 7.4 and immersed at 30° C. for 48 h.
[0156] 4.1 Degradation performance
[0157] The pericardium prepared according to the conditions in Example 4 was cut into pieces and then degraded in vitro using type I collagenase. The degradation rate of each sample at different times was recorded. The results are shown in Table 6.
[0158] Table 6 Degradation rate of each sample at different enzymatic hydrolysis time
[0159]
[0160] 4.2 Antigen blocking rate
[0161] The pericardium prepared according to the conditions in Example 4 was cut into pieces and then the antigen blocking rate was tested. The results are shown in Table 7.
[0162] Table 7 Antigen blocking rate of each sample
[0163] Cross-linking conditions Antigen blocking rate Sample set 1 97.54% Sample set 2 70.12% Sample set 3 98.01% Sample set 4 72.33%
[0164] From the data in Tables 6 and 7, it can be seen that no matter which type of cross-linking agent is used, when the concentration of the cross-linking agent component remains consistent, the degradation trend of the prepared pericardium is basically the same; and when the blocking agent component is added, the antigen blocking rate of the pericardium treated with the mixed cross-linking agent is higher.
[0165] Example 5
[0166] 5.1. Crosslinking agent is epoxy
[0167] Sample Group 1: Sample Group 1 of Example 4 (ie, Sample Group 2 of Example 1) was used.
[0168] Sample group 2: The decellularized and defatted pericardium was placed in a 0.001M sodium hydroxide aqueous solution with a glycidol concentration of 0.75M and immersed at 35°C for 24h; the pericardium was taken out and washed, and then placed in a 0.001M sodium hydroxide aqueous solution with a BDDE concentration of 0.375M and immersed at 35°C for 24h.
[0169] Sample group 3: Take the decellularized and defatted pericardium, put it into a 0.001M sodium hydroxide aqueous solution with a glycidol concentration of 0.75M, and soak it at 35°C for 12 hours; take it out, wash it, and then put it into a 0.001M sodium hydroxide aqueous solution with a BDDE concentration of 0.375M, and soak it at 35°C for 12 hours.
[0170] Sample group 4: The pericardium after decellularization and defatting was placed in a 0.001M sodium hydroxide aqueous solution with a BDDE concentration of 0.375M, and immersed at 35°C for 12h; taken out and washed, and then immersed in a 0.001M sodium hydroxide aqueous solution with a propylene oxide concentration of 0.75M, and immersed at 35°C for 12h.
[0171] 5.2. Crosslinking agent is aldehyde
[0172] Sample Group 5: Sample Group 3 of Example 4 (ie, Sample Group 2 of Example 2) was used.
[0173] Sample Group 6: The decellularized and defatted pericardium was placed in an aqueous solution of 0.3 M acetaldehyde and pH 7.4, and immersed at 30°C for 48 h; the pericardium was taken out and washed, and then placed in an aqueous solution of 0.15 M glutaraldehyde and pH 7.4, and immersed at 30°C for 48 h.
[0174] Sample Group 7: The decellularized and defatted pericardium was placed in an aqueous solution of 0.3 M acetaldehyde and pH 7.4, and soaked at 30°C for 12 h; taken out, washed, and then placed in an aqueous solution of 0.15 M glutaraldehyde and pH 7.4, and soaked at 30°C for 12 h.
[0175] Sample Group 8: The decellularized and defatted pericardium was placed in an aqueous solution of 0.15 M glutaraldehyde and pH 7.4, and immersed at 30°C for 12 h; the pericardium was taken out and washed, and then placed in an aqueous solution of 0.3 M acetaldehyde and pH 7.4, and immersed at 30°C for 12 h.
[0176] 5.3 Degradation performance
[0177] The pericardium prepared according to the conditions in Example 5 was cut into pieces and then degraded in vitro using type I collagenase. The degradation rate of each sample at different times was recorded. The results are shown in Table 8.
[0178] Table 8 Degradation rate of each sample at different enzymatic hydrolysis time
[0179]
[0180]
[0181] 5.4 Antigen blocking
[0182] The pericardium prepared according to the conditions in Example 5 was cut into pieces and then tested for antigen blocking rate. The results are shown in Table 7.
[0183] Table 9 Antigen blocking rate of each sample
[0184] Cross-linking conditions Antigen blocking rate Sample set 1 97.54% Sample set 2 96.13% Sample set 3 81.66% Sample set 4 77.12% Sample set 5 98.01% Sample set 6 91.33% Sample set 7 85.12% Sample set 8 75.18%
[0185] As can be seen from Tables 8-9, in sample group 1 and sample group 5, the antigen blocking rate of sample group 1 in which the blocking agent and the cross-linking agent were added simultaneously was higher and the degradation rate was lower.
[0186] This is because the concentrations of the crosslinker and the blocking agent in the reaction system are relatively high, which is more conducive to the penetration of the crosslinker and the blocking agent into the decellularized biological tissue and accelerates the reaction process; in addition, since the crosslinker and the blocking agent are activated in the reaction system and are in an unstable state, the rapid penetration of the two allows the crosslinker and the blocking agent to react at a relatively high concentration, thereby improving the utilization rate of the crosslinker and the blocking agent.
[0187] In sample groups 2 and 6, the blocking agent and the cross-linking agent were added separately. Compared with sample groups 1 and 5, the concentrations inside and outside the membrane of sample groups 2 and 6 were relatively low, resulting in relatively slow permeation rates. The epoxy groups in sample group 2 were unstable in alkaline aqueous solution and easily opened, and the aldehydes in sample group 6 were unstable under neutral and alkaline conditions and easily oxidized, resulting in the loss of blocking agent and cross-linking agent. Therefore, the antigen blocking rates of sample groups 2 and 6 were lower than those of sample groups 1 and 5. In addition, since the blocking agent was added to sample groups 2 and 6 first, it occupied the reaction sites first, and then the cross-linking agent was added. The carbon chain length of the cross-linking agent was limited, and the cross-linking efficiency was lower than that of sample groups 1 and 5, so the degradation rate was faster.
[0188] Although the total reaction time of sample groups 3 and 7 is the same as that of sample groups 1 and 5, respectively, the blocking reaction and cross-linking reaction are not sufficient due to the short step reaction time, and the blocking rate and cross-linking rate are reduced. Therefore, compared with sample groups 1 and 5, the antigen blocking rate is low and the degradation rate is fast.
[0189] The cross-linking agent was added to sample groups 4 and 8 first. Since there was no competition with the sealing agent, there were more sites suitable for cross-linking, so the degree of cross-linking was relatively large, resulting in a relatively slow degradation rate. In addition, the pores of the pericardium became smaller after cross-linking, which increased the difficulty of the sealing agent entering the pericardium. The speed of entering the pericardium was slow, resulting in lower antigen blocking rates relative to sample groups 1 and 5, respectively. In addition, the epoxy group in sample group 4 was unstable in alkaline aqueous solution and easily opened, and the aldehyde group in sample group 8 was unstable in neutral and alkaline aqueous solutions and easily oxidized, which was also one of the reasons for the relatively low antigen blocking rates in sample groups 4 and 8.
[0190] Example 6 Preparation of medical materials
[0191] Sample 1: Preparation of dural brain patch: obtain biological tissue material, freeze-thaw trimming, alkali treatment, protein removal, lipid impurities removal, medium to high degree cross-linking, removal of residual reagents and sterilization.
[0192] Its tensile strength is greater than 1MPa, elastic modulus is greater than 10MPa, and suture strength is greater than 2N.
[0193] Sample 2: Wound dressing and oral filling materials: biological tissue materials are obtained, freeze-thawed and trimmed, alkali treated, protein removed, lipid impurities removed, thickened, cross-linked to a low degree, residual reagents removed, freeze-dried and sterilized.
[0194] Its extensibility is ≤4.0N / cm, permanent deformation is ≤5%, thickness is >1mm, and porosity is >60%.
[0195] Sample Group 3: Preparation of facial and hand filling materials: biological tissue materials, freeze-thaw trimming, alkali treatment, protein removal, lipid impurities removal, low- to medium-level cross-linking, residual reagent removal, granulation, sterilization, preparation. Its sealing rate is > 90%, with good biosafety.
[0196] It can be seen from the above data that the product of the present invention is applicable to surgical operations and has good mechanical strength.
[0197] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A medical material containing decellularized biological tissue material, It is characterized in that The decellularized biological tissue material is prepared by the following method, which includes: after the biological tissue material is decellularized and defatted, cross-linking treatment is performed, and the biological tissue material is cross-linked with a reaction solution, wherein the reaction solution contains a blocking agent and a cross-linking agent; The molar ratio of the blocking agent to the cross-linking agent is: 0-40: 0-20, and both the blocking agent and the cross-linking agent are not 0; The reaction solution comprises any one of component I and component II; The component I comprises a blocking agent I and a cross-linking agent I; The component II includes a blocking agent II and a cross-linking agent II; The blocking agent I is an epoxy compound, the blocking agent II is an aldehyde compound, and the blocking agent has a single reaction site that mainly reacts with the amino group or carboxyl group of the amino acid in the biological tissue material; The crosslinking agent I is a polyepoxy epoxy compound, and the crosslinking agent II is a polyaldehyde compound.
2. The medical material according to claim 1, It is characterized in that The medical materials include materials used for repairing, filling and replacing human tissues; The materials used for tissue repair include: wound dressings, dental repair materials, bone or cartilage repair materials, chest and / or abdominal wall repair patches, anal fistula repair patches, gastric or lung resection repair patches, dura mater patches, spinal dura mater patches, scleral repair patches, anti-adhesion patches, and nerve conduits; Materials used for tissue filling include: rhinoplasty filling materials, breast filling materials, facial filling materials, hand filling materials, buttock filling materials, genital filling materials, filling materials after otitis media surgery, and filling materials after thyroid surgery; Materials used for tissue replacement include: biological valves, artificial blood vessels, artificial tear ducts, artificial tendons, and artificial corneas.
3. The medical material according to claim 2, It is characterized in that The medical materials include: wound dressings, dental repair materials, chest and / or abdominal wall repair patches, dura mater patches, spinal dura mater patches, sclera repair patches, breast filling materials, facial filling materials, and hand filling materials.
4. The medical material according to claim 1, It is characterized in that The epoxy compound of the blocking agent I is selected from one or more of glycidol, 2-(oxetane-3-yl)ethane-1-ol, epichlorohydrin, and butyl glycidyl ether; The polyepoxy epoxy compound of the crosslinking agent I contains 2-4 epoxy groups and is selected from: one or more of 1,4-butanediol diglycidyl ether, ethylene glycol diglycidyl ether, glycerol triglycidyl ether, and pentaerythritol glycidyl ether; The aldehyde compound of the blocking agent II is selected from one or more of acetaldehyde, n-propionaldehyde, and n-valeraldehyde; The polyaldehyde compound of the crosslinking agent II contains 2 to 4 aldehyde groups, and is selected from one or more of glutaraldehyde, adipaldehyde, 1,3-succinaldehyde, trimesic acid, and 1,2,4,5-pyromellitic acid.
5. The medical material according to claim 4, It is characterized in that In component I, the blocking agent I is glycidol, and the cross-linking agent I is 1,4-butanediol diglycidyl ether; In component II, the blocking agent II is acetaldehyde, and the cross-linking agent II is glutaraldehyde.
6. The medical material according to claim 1, It is characterized in that The reaction solution further comprises a solvent, which is selected from the group consisting of one or more combinations of water, dimethyl sulfoxide, N,N-dimethylformamide, tetrahydrofuran, dioxane, pyridine, acetonitrile, ethyl acetate, ether, isopropyl ether, dichloromethane, ethyl bromide, carbon tetrachloride, cyclohexane, hexane, heptane or kerosene.
7. The medical material according to any one of claims 1 to 6, It is characterized in that In the component I, the molar ratio of the blocking agent I to the cross-linking agent I is 0-25:0-20.
8. The medical material according to claim 7, It is characterized in that In the component I, the molar ratio of the blocking agent I to the cross-linking agent I is 0-20:0-10.
9. The medical material according to claim 8, It is characterized in that In the component I, the molar ratio of the blocking agent I to the cross-linking agent I is 1-20:1-10.
10. The medical material according to claim 9, It is characterized in that In the component I, the molar ratio of the blocking agent I to the cross-linking agent I is 1-20:1-5.
11. The medical material according to any one of claims 1 to 6, It is characterized in that In the component II, the molar ratio of the blocking agent II to the cross-linking agent II is 0-25:0-20.
12. The medical material according to claim 11, It is characterized in that In the component II, the molar ratio of the blocking agent II to the cross-linking agent II is 0-20:0-10.
13. The medical material according to claim 12, It is characterized in that In the component II, the molar ratio of the blocking agent II to the cross-linking agent II is 1-20:1-10.
14. The medical material according to claim 13, It is characterized in that In the component II, the molar ratio of the blocking agent II to the cross-linking agent II is 1-20:1-5.
15. The medical material according to claim 9 or 13, It is characterized in that In the component I, the epoxy group molar ratio of the blocking agent I and the crosslinking agent I is 1-10:1-10; In the component II, the molar ratio of the aldehyde groups of the blocking agent II and the cross-linking agent II is 1-10:1-10.
16. The medical material according to claim 1, It is characterized in that The solvent of component I is an alkaline solvent, and the alkaline solvent comprises one or more of the following components: sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, sodium sulfite, potassium sulfite; And / or, the solvent of component II is an alkaline solvent with a pH value of 7-9.
17. The medical material according to any one of claims 1 to 6, It is characterized in that The total epoxy group molar concentration in the component I is 0.1 to 3M; The crosslinking treatment immersion temperature of the component I is 25-45°C; The cross-linking treatment immersion time of the component I is 5 to 72 hours.
18. The medical material according to claim 17, It is characterized in that The total epoxy group molar concentration in the component I is 0.5 to 2M; The crosslinking treatment immersion temperature of the component I is 30-40°C; The crosslinking treatment immersion time of the component I is 15 to 30 hours.
19. The medical material according to any one of claims 1 to 6, It is characterized in that The total aldehyde molar concentration in the component II is 0.01 to 2 M; The crosslinking treatment immersion temperature of the component II is 20-45°C; The cross-linking treatment immersion time of the component II is 10 to 96 hours.
20. The medical material according to claim 19, It is characterized in that The total aldehyde molar concentration in the component II is 0.1 to 1 M; The crosslinking treatment immersion temperature of the component II is 25-30°C; The cross-linking treatment immersion time of the component II is 24 to 48 hours.
21. The medical material according to claim 1, It is characterized in that The biological tissue material includes dermal tissue, blood vessels, digestive tract, organ membrane, body cavity membrane, amniotic membrane, biological valve, cartilage tissue, bone tissue, muscle tissue, fat tissue, tendon or animal pericardium.
22. The medical material according to claim 21, It is characterized in that The biological tissue material is animal pericardium.
23. The method for preparing the medical material according to any one of claims 1 to 22, wherein the method include: A. Material collection: Select biological tissue materials; B Pretreatment: destroying cells of biological tissue materials by freeze-thaw technique; Trimming, removing impurities and irregularities from biological tissue materials; C Alkaline treatment: The biological tissue material is treated with an alkaline solution, neutralized with a weak acid, and washed; D. Protein removal: Use surfactants and protein solubilizers to remove water-soluble and fat-soluble proteins from biological tissue materials; E. Removal of lipid impurities: Use medium polarity organic solvents to remove residual lipids in biological tissue materials; F Cross-linking: cross-linking biological tissue materials with reaction solution; G. Removal of residual reagents: Use water to repeatedly soak and clean the cross-linked biological tissue material to remove residual reagents; H Sterilization: Sterilize the cross-linked biological tissue material after cutting and packaging.
24. Use of the medical material according to any one of claims 1 to 22 or the medical material obtained by the preparation method according to claim 23 in the preparation of materials for repairing, filling and replacing human tissues.