A kind of polymer sulphoaluminate cement repair mortar and its preparation method and application
By adding ore powder and calcium sulfosilicate to the polymer sulfaluminate cement repair mortar, and using La2O3 to adjust the hydration liquid phase, the problems of shrinkage and cracking of the mortar were solved in the later stage of hydration of the mortar were improved, and durability and bonding were improved performance.
Patent Information
- Application Number
- CN202310312446.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-11-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Polymer sulfaluminate cement repair mortar is prone to shrink and cracking in the later stage of hydration, resulting in the problem of reduced durability and shedding.
By adding ore powder and calcium sulfosilicate to the repair mortar and introducing La2O3, the SO42-concentration of the hydrated liquid phase is controlled, the formation and stability of ettringite are promoted, and the emergence of monosulfide calcium sulfosilicate hydrated is inhibited. , delay the condensation of sulfur aluminate cement.
It effectively reduces the shrinkage rate of repair mortar, prevents cracking, improves bonding performance and durability, and ensures the stability and bonding performance of repair mortar in the later service process.
Smart Images

Figure CN116444237B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete repair, and in particular to a polymer sulphoaluminate cement repair mortar, a preparation method and applications thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Sulphoaluminate cement has the characteristics of fast hardening, early strength and high bonding strength, and is often used for repairing and reinforcing concrete structures. The hydration of calcium sulfoaluminate minerals in sulphoaluminate cement is mainly concentrated in the first 7 days. In the later stage of hydration, the repair mortar still has a certain shrinkage, which is easy to cause cracking. In addition, the main hydration product of sulphoaluminate cement is calcium sulfoaluminate. The molar ratio of gypsum to calcium sulfoaluminate in sulphoaluminate cement is less than 2. After the gypsum is consumed, the SO4 2- The decrease in concentration provides conditions for the conversion of ettringite into monosulfide calcium sulfoaluminate hydrate. However, since the density of calcium sulfoaluminate is lower than that of monosulfide calcium sulfoaluminate hydrate, the appearance of monosulfide calcium sulfoaluminate hydrate increases the porosity of the repair mortar and reduces its durability. In addition, compared with ettringite, monosulfide calcium sulfoaluminate hydrate is more easily carbonized, causing shrinkage, cracking, and even shedding of the repair mortar. Summary of the invention
[0004] The purpose of the present invention is to control the late shrinkage of polymer sulphoaluminate cement repair mortar and improve the stability of the hydration product ettringite therein, so as to overcome the defects that this type of repair mortar is prone to shrinkage, cracking, and even falling off in the later stage. In view of this, the present invention provides a polymer sulphoaluminate cement repair mortar, a preparation method thereof, and an application thereof. To achieve the above purpose, the technical solution of the present invention is specifically as follows.
[0005] In the first aspect, the present invention discloses a polymer sulphoaluminate cement repair mortar, which comprises the following raw materials: 40-45 parts by weight of sulphoaluminate cement, 40-45 parts by weight of sand, 5.0-8.0 parts by weight of mineral powder, 5.0-8.0 parts by weight of calcium sulfosilicate, 1.0-2.0 parts by weight of polymer glue powder, 0.001-0.002 parts by weight of La2O3 powder, and 0.32-0.75 parts by weight of additives. The mineral powder contains 13-20wt.% of the active ingredient Al2O3.
[0006] Furthermore, the raw material composition of the repair mortar also includes water. Optionally, the water is added in a ratio of 0.14 to 0.16.
[0007] Furthermore, the polymer powder includes at least one of polyvinyl alcohol (PVA) powder, ethylene-vinyl acetate copolymer (EVA) powder, etc. In the present invention, the main functions of the polymer powder include two aspects: (1) enhancing the bonding performance with old concrete; (2) encapsulating cement hydration products and inhibiting the powdering of the surface of the hardened sulphoaluminate cement.
[0008] Furthermore, the mineral powder includes at least one of S95 mineral powder, S105 mineral powder, primary fly ash, etc. In the present invention, the mineral powder containing active aluminum component is used, which can not only cooperate with the calcium sulfosilicate to compensate for the shrinkage of the polymer sulfoaluminate cement repair mortar in the late hydration stage and prevent cracking, but also promote the stability of the formed ettringite and avoid its carbonization.
[0009] Furthermore, the auxiliary agent includes at least one of a water reducing agent, a defoaming agent, a retarder, etc.
[0010] Furthermore, the water reducing agent is added in an amount of 0.2 to 0.5 parts by weight. Optionally, the water reducing agent includes any one of a polycarboxylic acid water reducing agent, a naphthalene water reducing agent, an aliphatic water reducing agent, and the like.
[0011] Furthermore, the defoamer is added in an amount of 0.1 to 0.2 parts by weight. Optionally, the defoamer includes at least one of an organosilicon defoamer, a polyether defoamer, a polyether-modified silicon, tributyl phosphate, etc. In the present invention, the main function of the defoamer is to eliminate bubbles generated during the mixing process of the polymer sulphoaluminate cement repair mortar.
[0012] Furthermore, the retarder is added in an amount of 0.02 to 0.05 parts by weight. Optionally, the retarder includes at least one of tartaric acid, sodium citrate, glucose, etc. In the present invention, the main function of the retarder is to delay the coagulation of sulphoaluminate cement and facilitate the construction of polymer sulphoaluminate cement repair mortar.
[0013] In a second aspect, the present invention discloses a method for preparing polymer sulphoaluminate cement repair mortar, comprising the following steps:
[0014] (1) The above-mentioned sulphoaluminate cement, sand, mineral powder, calcium sulphosilicate, polymer rubber powder, La2O3 and additives are mixed and stirred evenly to obtain a dry mix for standby use.
[0015] (2) Add the water to the dry mix and stir evenly to obtain the repair mortar.
[0016] In a third aspect, the present invention discloses the application of the polymer sulphoaluminate cement repair mortar in the fields of construction, bridges, highways, etc.
[0017] Compared with the prior art, the technical solution of the present invention has at least the following beneficial effects:
[0018] The present invention has found that the shrinkage and cracking of the conventional polymer sulphoaluminate cement repair mortar mainly occurs in the late stage of hydration of sulphoaluminate cement. To this end, the polymer sulphoaluminate cement repair mortar of the present invention adds mineral powder and calcium sulphosilicate, thereby: firstly, utilizing the SO4 2- The concentration is high, which strongly inhibits the hydration of calcium sulfosilicate. As the reaction continues, the SO4 in the hydrated liquid phase after the gypsum is consumed 2- The reduced concentration creates conditions for the dissolution and hydration of calcium sulfosilicate, which can enable the calcium sulfosilicate to be hydrated in the later stage of hydration of sulfoaluminate cement, and then the gypsum produced by the hydration can be reacted with the mineral powder to form calcium sulfoaluminate with micro-expansion characteristics, thereby compensating for the shrinkage of the polymer sulfoaluminate cement repair mortar in the later stage of hydration.
[0019] However, the present invention further found that the hydration degree of calcium sulfosilicate is extremely low, and it is unable to produce sufficient gypsum to react with the mineral powder to form sufficient calcium sulfonate. Therefore, the present invention introduces La2O3 into the polymer sulfoaluminate cement repair mortar. The hydration of calcium sulfosilicate starts from dissolution. The early hydration liquid phase SO4 2- The high concentration inhibits its dissolution, and the gypsum is consumed in the late stage of hydration, and the hydrated liquid phase SO4 2- As the concentration increases, the special electronic structure of La2O3 promotes the dissolution of calcium sulfosilicate, which in turn promotes the hydration of calcium sulfosilicate to produce more dihydrate gypsum, which reacts with the active aluminum component in the mineral powder to form ettringite with micro-expansion characteristics, compensating for the shrinkage of the polymer sulfoaluminate cement repair mortar in the later stage of hydration, thereby inhibiting cracking. Tests show that the polymer sulfoaluminate cement repair mortar of the present invention shrinks less than 0.02% in the later stage (after 7 days), and no cracking occurs during the later service process.
[0020] When the active aluminum component in the mineral powder is consumed, the calcium sulfosilicate continues to hydrate under the action of La2O3 to produce dihydrate gypsum, so that SO4 in the hydrated liquid phase 2- The concentration increases, thereby inhibiting the conversion of ettringite to monosulfide calcium sulfoaluminate hydrate, ensuring the stability of ettringite. On the one hand, it avoids the problem of increased porosity in the repair mortar due to the presence of monosulfide calcium sulfoaluminate hydrate, which in turn leads to reduced durability. On the other hand, it avoids the carbonization of monosulfide calcium sulfoaluminate hydrate, so that the polymerized sulfoaluminate-free cement repair mortar of the present invention maintains good bonding properties for a long time and is not easy to fall off during the later service process. The test shows that the SO4 2-The concentration is kept above 1.5mmol / L all year round, the hydration product ettringite is stable for a long time without decomposition, and the bonding performance is kept above 1.8MPa for a long time with good bonding performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. The embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein:
[0022] Figure 1 This is a graph showing the shrinkage test results of the polymer sulphoaluminate cement repair mortar specimens prepared in Example 1 of the present invention at various ages.
[0023] Figure 2 The SO4 content of the hydrated liquid phase of the polymer sulphoaluminate cement repair mortar specimens prepared in Example 1 of the present invention at various ages is 2- Concentration test result graph.
[0024] Figure 3 This is a graph showing the tensile bond strength test results of the polymer sulphoaluminate cement repair mortar specimens prepared in Example 1 of the present invention at various ages. DETAILED DESCRIPTION
[0025] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0026] Unless otherwise defined, all professional and scientific terms used in the present invention have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. If not otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar to or equivalent to the described content can be applied to the method of the present invention. The preferred implementation methods and materials described in the present invention are for demonstration purposes only.
[0027] Example 1
[0028] A method for preparing polymer sulphoaluminate cement repair mortar comprises the following steps:
[0029] (1) Weigh the following raw materials: 40 parts by weight of sulphoaluminate cement, 45 parts by weight of sand (fineness between 0.7 and 2.2 mm), 8.0 parts by weight of S105 mineral powder (wherein the Al2O3 content is 16.74 wt.%), 5.0 parts by weight of calcium sulfosilicate, 2.0 parts by weight of PVA glue powder, 0.002 parts by weight of La2O3 powder, 0.5 parts by weight of polycarboxylic acid water reducer (water reduction rate 20%), 0.2 parts by weight of tributyl phosphate defoamer, and 0.05 parts by weight of tartaric acid retarder.
[0030] (2) The sulphoaluminate cement, calcium sulfosilicate, sand, mineral powder, PVA glue powder, water reducer, defoamer, retarder and La2O3 powder in the above raw materials are placed in a mixer and mixed for 5 minutes to obtain a dry mix, and then water is added at a water-to-material ratio of 0.16 and mixed for 10 minutes to obtain polymer sulphoaluminate cement repair mortar.
[0031] Performance test: The polymer sulphoaluminate cement repair mortar prepared in this example was poured into a mold to make a test piece, and the test piece was discarded and the length of the hydration age of 7 days was taken as the original length (recorded as A). Then the length of the test piece at 90 days (recorded as B) was tested, and the shrinkage rate was calculated as (AB) / A, and the result was 0.011%. In addition, the SO4 2- The concentration is 1.93mmol / L, the tensile bond strength is 1.81MPa, and the specific performance at each age is as follows: Figure 1 , Figure 2 , Figure 3 shown.
[0032] Example 2
[0033] A method for preparing polymer sulphoaluminate cement repair mortar comprises the following steps:
[0034] (1) Weigh the following raw materials: 42 parts by weight of sulphoaluminate cement, 43 parts by weight of sand with a fineness of 0.7 to 2.2 mm), 6.0 parts by weight of S105 mineral powder (wherein the Al2O3 content is 12.97 wt.%), 6.5 parts by weight of calcium sulfosilicate, 1.5 parts by weight of ethylene-vinyl acetate copolymer rubber powder, 0.002 parts by weight of La2O3 powder, 0.35 parts by weight of polycarboxylic acid water reducer (water reduction rate 20%), 0.15 parts by weight of organosilicon defoamer, and 0.03 parts by weight of tartaric acid retarder.
[0035] (2) The sulphoaluminate cement, calcium sulfosilicate, sand, mineral powder, ethylene-vinyl acetate copolymer rubber powder, water reducer, defoamer, retarder and La2O3 powder in the above raw materials are placed in a mixer and mixed for 5 minutes to obtain a dry mix, and then water is added at a water-to-material ratio of 0.15 and mixed for 10 minutes to obtain polymer sulphoaluminate cement repair mortar.
[0036] Performance test: The polymer sulphoaluminate cement repair mortar prepared in this example was poured into a mold to make a test piece, and the test piece was discarded and the length of the hydration age of 7 days was taken as the original length (recorded as A). Then the length of the test piece at 90 days (recorded as B) was tested, and the shrinkage rate was calculated as (AB) / A, and the result was 0.011%. In addition, the SO4 2- The concentration is 2.26mmol / L and the tensile bond strength is 2.41MPa.
[0037] Example 3
[0038] A method for preparing polymer sulphoaluminate cement repair mortar comprises the following steps:
[0039] (1) Weigh the following raw materials: 45 parts by weight of sulphoaluminate cement, 40 parts by weight of sand (fineness between 0.7 and 2.2 mm), 5.0 parts by weight of S95 mineral powder (wherein the Al2O3 content is 20.02 wt.%), 8.0 parts by weight of calcium sulfosilicate, 1.0 parts by weight of PVA glue powder, 0.001 parts by weight of La2O3 powder, 0.2 parts by weight of polycarboxylic acid water reducer (water reduction rate 20%), 0.1 parts by weight of triphosphate defoamer, and 0.02 parts by weight of glucose retarder.
[0040] (2) The sulphoaluminate cement, calcium sulfosilicate, sand, mineral powder, PVA glue powder, water reducer, defoamer, retarder and La2O3 powder in the above raw materials are placed in a mixer and mixed for 5 minutes to obtain a dry mix, and then water is added at a water-to-material ratio of 0.14 and mixed for 10 minutes to obtain polymer sulphoaluminate cement repair mortar.
[0041] Performance test: The polymer sulphoaluminate cement repair mortar prepared in this example was poured into a mold to make a test piece, and the test piece was discarded and the length of the hydration age of 7 days was taken as the original length (recorded as A). Then the length of the test piece at 90 days (recorded as B) was tested, and the shrinkage rate was calculated as (AB) / A, and the result was 0.009%. In addition, the SO4 2- The concentration is 2.14mmol / L and the tensile bond strength is 2.27MPa.
[0042] Example 4
[0043] A method for preparing polymer sulphoaluminate cement repair mortar comprises the following steps:
[0044] (1) Weigh the following raw materials: 40 parts by weight of sulphoaluminate cement, 45 parts by weight of sand (fineness between 0.7 and 2.2 mm), 8.0 parts by weight of S105 mineral powder (wherein the Al2O3 content is 16.74 wt.%), 5.0 parts by weight of calcium sulfosilicate, 2.0 parts by weight of PVA glue powder, 0.5 parts by weight of polycarboxylic acid water reducer (water reduction rate 20%), 0.2 parts by weight of tributyl phosphate defoamer, and 0.05 parts by weight of tartaric acid retarder.
[0045] (2) The sulphoaluminate cement, calcium sulfosilicate, sand, mineral powder, PVA glue powder, water reducer, defoamer and retarder in the above raw materials are placed in a mixer and mixed for 5 minutes to obtain a dry mix, and then water is added at a water-to-material ratio of 0.16 and mixed for 10 minutes to obtain polymer sulphoaluminate cement repair mortar.
[0046] Performance test: The polymer sulphoaluminate cement repair mortar prepared in this example was poured into a mold to make a test piece, and the test piece was discarded and the length of the hydration age of 7 days was taken as the original length (recorded as A). Then the length of the test piece at 90 days (recorded as B) was tested, and the shrinkage rate was calculated as (AB) / A, and the result was 0.035%. In addition, the SO4 2- The concentration is 0.87mmol / L and the tensile bond strength is 1.21MPa.
[0047] Example 5
[0048] A method for preparing polymer sulphoaluminate cement repair mortar comprises the following steps:
[0049] (1) Weigh the following raw materials: 40 parts by weight of sulphoaluminate cement, 45 parts by weight of sand (fineness between 0.7 and 2.2 mm), 8.0 parts by weight of S105 mineral powder (wherein the Al2O3 content is 16.74 wt.%), 5.0 parts by weight of calcium sulfosilicate, 2.0 parts by weight of PVA glue powder, 0.002 parts by weight of Ce2O3 powder, 0.5 parts by weight of polycarboxylic acid water reducer (water reduction rate 20%), 0.2 parts by weight of tributyl phosphate defoamer, and 0.05 parts by weight of tartaric acid retarder.
[0050] (2) The sulphoaluminate cement, calcium sulfosilicate, sand, mineral powder, PVA glue powder, water reducer, defoamer, retarder and Ce2O3 powder in the above raw materials are placed in a mixer and mixed for 5 minutes to obtain a dry mix, and then water is added at a water-to-material ratio of 0.16 and mixed for 10 minutes to obtain polymer sulphoaluminate cement repair mortar.
[0051] Performance test: The polymer sulphoaluminate cement repair mortar prepared in this example was poured into a mold to make a test piece, and the test piece was discarded and the length of the hydration age of 7 days was taken as the original length (recorded as A). Then the length of the test piece at 90 days (recorded as B) was tested, and the shrinkage rate was calculated as (AB) / A, and the result was 0.047%. In addition, the SO4 2- The concentration is 0.92mmol / L and the tensile bond strength is 1.33MPa.
[0052] Example 6
[0053] A method for preparing polymer sulphoaluminate cement repair mortar comprises the following steps:
[0054] (1) Weigh the following raw materials: 42 parts by weight of sulphoaluminate cement, 43 parts by weight of sand (fineness between 0.7 and 2.2 mm), 6.0 parts by weight of S105 mineral powder (wherein the Al2O3 content is 12.97 wt.%), 6.5 parts by weight of calcium sulfosilicate, 1.5 parts by weight of ethylene-vinyl acetate copolymer rubber powder, 0.002 parts by weight of Y2O3 powder, 0.35 parts by weight of polycarboxylic acid water reducer (water reduction rate 20%), 0.15 parts by weight of organosilicon defoamer, and 0.03 parts by weight of tartaric acid retarder.
[0055] (2) The sulphoaluminate cement, calcium sulfosilicate, sand, mineral powder, ethylene-vinyl acetate copolymer rubber powder, water reducer, defoamer, retarder, and Y2O3 powder in the above raw materials are placed in a mixer and mixed for 5 minutes to obtain a dry mix, and then water is added at a water-to-material ratio of 0.15 and mixed for 10 minutes to obtain polymer sulphoaluminate cement repair mortar.
[0056] Performance test: The polymer sulphoaluminate cement repair mortar prepared in this example was poured into a mold to make a test piece, and the test piece was discarded and the length of the hydration age of 7 days was taken as the original length (recorded as A). Then the length of the test piece at 90 days (recorded as B) was tested, and the shrinkage rate was calculated as (AB) / A, and the result was 0.041%. In addition, the SO4 2- The concentration is 0.76mmol / L and the tensile bond strength is 1.02MPa.
[0057] Example 7
[0058] A method for preparing polymer sulphoaluminate cement repair mortar comprises the following steps:
[0059] (1) Weigh the following raw materials: 45 parts by weight of sulphoaluminate cement, 40 parts by weight of sand (fineness between 0.7 and 2.2 mm), 5.0 parts by weight of S95 mineral powder (wherein the Al2O3 content is 20.02 wt.%), 1.0 parts by weight of PVA glue powder, 0.001 parts by weight of La2O3 powder, 00.2 parts by weight of polycarboxylic acid water reducer (water reduction rate 20%), 0.1 parts by weight of triphosphate defoamer, and 0.02 parts by weight of glucose retarder.
[0060] (2) The sulphoaluminate cement, sand, mineral powder, PVA glue powder, water reducer, defoamer, retarder and La2O3 powder in the above raw materials are placed in a mixer and mixed for 5 minutes to obtain a dry mix, and then water is added at a water-to-material ratio of 0.14 and mixed for 10 minutes to obtain polymer sulphoaluminate cement repair mortar.
[0061] Performance test: The polymer sulphoaluminate cement repair mortar prepared in this example was poured into a mold to make a test piece, and the test piece was discarded and the length of the hydration age of 7 days was taken as the original length (recorded as A). Then the length of the test piece at 90 days (recorded as B) was tested, and the shrinkage rate was calculated as (AB) / A, and the result was 0.052%. In addition, the SO4 2- The concentration is 0.56mmol / L and the tensile bond strength is 0.94MPa.
[0062] Example 8
[0063] A method for preparing polymer sulphoaluminate cement repair mortar comprises the following steps:
[0064] (1) Weigh the following raw materials: 45 parts by weight of sulphoaluminate cement, 40 parts by weight of sand (fineness between 0.7 and 2.2 mm), (wherein the Al2O3 content is 20.02 wt.%), 8.0 parts by weight of calcium sulphosilicate, 1.0 parts by weight of PVA glue powder, 0.001 parts by weight of La2O3 powder, 0.2 parts by weight of polycarboxylic acid water reducer (water reduction rate 20%), 0.1 parts by weight of triphosphate defoamer, and 0.02 parts by weight of glucose retarder.
[0065] (2) The sulphoaluminate cement, calcium sulfosilicate, sand, PVA glue powder, water reducer, defoamer, retarder and La2O3 powder in the above raw materials are placed in a mixer and mixed for 5 minutes to obtain a dry mix, and then water is added at a water-to-material ratio of 0.14 and mixed for 10 minutes to obtain polymer sulphoaluminate cement repair mortar.
[0066] Performance test: The polymer sulphoaluminate cement repair mortar prepared in this example was poured into a mold to make a test piece, and the test piece was discarded and the length of the hydration age of 7 days was taken as the original length (recorded as A). Then the length of the test piece at 90 days (recorded as B) was tested, and the shrinkage rate was calculated as (AB) / A, and the result was 0.039%. In addition, the SO4 2- The concentration is 1.14mmol / L and the tensile bond strength is 1.46MPa.
[0067] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A polymer sulphoaluminate cement repair mortar, characterized in that: The repair mortar comprises the following raw materials: 40-45 parts by weight of sulphoaluminate cement, 40-45 parts by weight of sand, 5.0-8.0 parts by weight of mineral powder, 5.0-8.0 parts by weight of calcium sulfosilicate, 1.0-2.0 parts by weight of polymer glue powder, 0.001-0.002 parts by weight of La2O3 powder, and 0.32-0.75 parts by weight of additives; wherein the mineral powder contains 13-20wt.% of the active ingredient Al2O3.
2. The polymer sulphoaluminate cement repair mortar according to claim 1, characterized in that: The raw material composition of the repair mortar also includes water.
3. The polymer sulphoaluminate cement repair mortar according to claim 2, characterized in that: The addition ratio of the water is: the water-to-material ratio is 0.14~0.
16.
4. The polymer sulphoaluminate cement repair mortar according to claim 1, characterized in that: The mineral powder includes at least one of S95 mineral powder and S105 mineral powder.
5. The polymer sulphoaluminate cement repair mortar according to claim 1, characterized in that: The polymer rubber powder includes at least one of polyvinyl alcohol rubber powder and ethylene-vinyl acetate copolymer.
6. The polymer sulphoaluminate cement repair mortar according to claim 1, characterized in that: The auxiliary agent includes at least one of a water reducing agent, a defoaming agent and a retarder.
7. The polymer sulphoaluminate cement repair mortar according to claim 6, characterized in that: The water reducing agent is added in an amount of 0.2 to 0.5 parts by weight.
8. The polymer sulphoaluminate cement repair mortar according to claim 6, characterized in that: The water reducer includes any one of a polycarboxylate water reducer, a naphthalene water reducer, and an aliphatic water reducer.
9. The polymer sulphoaluminate cement repair mortar according to claim 6, characterized in that: The defoamer is added in an amount of 0.1 to 0.2 parts by weight.
10. The polymer sulphoaluminate cement repair mortar according to claim 6, characterized in that: The defoaming agent includes at least one of silicone defoaming agent, polyether defoaming agent, polyether modified silicon, and tributyl phosphate.
11. The polymer sulphoaluminate cement repair mortar according to claim 6, characterized in that: The retarder is added in an amount of 0.02 to 0.05 parts by weight.
12. The polymer sulphoaluminate cement repair mortar according to claim 6, characterized in that: The retarder includes at least one of tartaric acid, sodium citrate and glucose.
13. A method for preparing polymer sulphoaluminate cement repair mortar, comprising the following steps: (1) Mix the sulphoaluminate cement, sand, mineral powder, calcium sulfosilicate, polymer glue powder, La2O3 and additives in the polymer sulphoaluminate cement repair mortar according to any one of claims 1 to 12, stir evenly, and obtain a dry mix for later use; (2) Add the water to the dry mix and stir evenly to obtain the repair mortar.
14. Use of the polymer sulphoaluminate cement repair mortar according to any one of claims 1 to 12, or the polymer sulphoaluminate cement repair mortar obtained by the preparation method according to claim 13 in the fields of construction, bridges or highways.