Catalytic layer for fuel cell and preparation method of membrane electrode of catalytic layer

By using materials such as sulfonated lignin conductive polymer nanoparticles and polytetrafluoroethylene in the fuel cell catalytic layer, a stable conductive network and gas transmission channel is formed, and the water management and conductivity of fuel cells under low humidity conditions is solved. The problem of insufficient problems significantly improves the performance and efficiency of the battery.

CN119069730AActive Publication Date: 2024-12-03SICHUAN QINGLV TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411537564.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-31
Publication Date
2024-12-03
Estimated Expiration
2044-10-31

AI Technical Summary

Technical Problem

Fuel cells have difficulty in water management under low humidity or unhumidified conditions, poor moisture management effect of the catalytic layer affects battery performance, and insufficient conductivity of existing water management materials.

Method used

An anode catalyst layer including Pt-C catalyst, high dielectric small molecule alcohol, sulfonated lignin-doped conductive polymer nanoparticles, hydrophilic adhesives and deionized water, as well as catalysts, polytetrafluoroethylene, The cathodic catalytic layer of high dielectric small molecule alcohol and deionized water forms a stable conductive network and gas transmission channel through the combination of hydrophilic and hydrophobic materials, optimizing water management and conductivity.

Benefits of technology

Support efficient water management under low humidity conditions, improve the overall conductivity and electrochemical performance of the catalytic layer, ensure the water distribution and transmission efficiency of the proton exchange membrane, avoid water flooding, and improve the temperature and power performance of the fuel cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069730A_ABST
    Figure CN119069730A_ABST
Patent Text Reader

Abstract

The invention discloses a catalyst layer for a fuel cell and a preparation method of a membrane electrode of the catalyst layer, the catalyst layer comprises an anode catalyst and a cathode catalyst, the anode catalyst layer comprises a Pt-C catalyst, high-dielectric micromolecular alcohol, sulfonated lignin doped conductive polymer nanoparticles, a hydrophilic adhesive, an ionomer solution and deionized water; the cathode catalyst layer comprises a catalyst, an ionomer solution, high-dielectric micromolecular alcohol, polytetrafluoroethylene and deionized water; the technical problems that an existing catalyst layer for a fuel cell is poor in water management effect, and an adopted water management material is poor in conductivity can be solved. According to the preparation method, in the preparation process, a hydrophilic conductive adhesive and a relatively hydrophobic conductive adhesive are adopted for adhesive dispensing on the cathode and the anode respectively, the diffusion layer is fixed under the condition that conductivity is not lost, meanwhile, hydrophilic management and hydrophobic management are conducted on the two sides of the square packaging structure respectively, and the performance is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of fuel cells, and specifically relates to a catalyst layer for a fuel cell and a method for preparing a membrane electrode thereof. Background Art

[0002] As an efficient and clean energy conversion device, fuel cells have received extensive attention and research in recent years. Fuel cells directly generate electricity through the chemical reaction of hydrogen and oxygen, and have the advantages of high energy conversion efficiency and low environmental pollution. In fuel cells, the catalyst layer is one of the key components and directly affects the performance and efficiency of the battery. The main function of the catalyst layer is to promote the electrochemical reaction of fuel and oxidant on the electrode surface, thereby improving the output power and stability of the battery.

[0003] Water management in fuel cells is particularly difficult under low humidity or non-humidification conditions. The water loss of the proton exchange membrane during operation will not only cause deformation of the catalyst layer, but also affect the proton transfer efficiency. At the same time, most of the water management materials currently used have poor electrical conductivity, which affects the establishment of the electron transfer network in the catalyst layer, thereby affecting the performance of the battery. Summary of the invention

[0004] In order to overcome the defects of the prior art, the present invention provides a catalyst layer for a fuel cell and a method for preparing the membrane electrode thereof, which can solve the technical problems that the catalyst layer for a fuel cell currently has poor water management effect and the water management material used has poor conductivity.

[0005] The object of the present invention is achieved through the following technical solutions: In the first aspect, the present invention provides a catalytic layer for a fuel cell, including an anode catalyst and a cathode catalyst, wherein the anode catalyst layer includes: a Pt-C catalyst, a high dielectric small molecule alcohol, sulfonated lignin-doped conductive polymer nanoparticles, a hydrophilic adhesive, an ionomer solution, and deionized water; the cathode catalyst layer includes a catalyst, an ionomer solution, a high dielectric small molecule alcohol, polytetrafluoroethylene, and deionized water.

[0006] The main beneficial effects of the present invention are as follows: hydrophilic substances are added to the anode catalyst slurry of the present invention, which can still support efficient water management under high current density even under low humidity conditions or non-humidified conditions; sulfonated lignin-doped conductive polymer nanoparticles are added to the anode catalyst, sulfonated lignin has good hydrophilicity, and due to its highly branched three-dimensional structure, it can form a stable conductive network with nano-conductive particles, thereby improving the overall conductivity of the catalyst layer, forming an effect of one plus one greater than two; and polytetrafluoroethylene has good hydrophobic properties. When the battery is running at a high current density, a large amount of water will be generated on the cathode side. PTFE can ensure that the water is quickly discharged to avoid the cathode catalyst layer being flooded by water, thereby maintaining a good gas transmission channel. The hydrophilic treatment of the diffusion layer is conducive to controlling the content of free water inside the battery and avoiding high temperature and power drop caused by water blockage.

[0007] In one embodiment, the high dielectric small molecule alcohol includes at least one of ethanol, ethylene glycol, n-propanol, and isopropanol.

[0008] The main beneficial effects of the present invention are as follows: high dielectric small molecule alcohol can not only improve the conductivity of the catalyst layer, thereby improving the electrochemical performance of the battery, but also act as a solvent or dispersant to help the catalyst to be evenly dispersed in the slurry, thereby improving the uniformity and stability of the catalyst layer.

[0009] In one embodiment, the ionomer solution includes at least one of a sulfonated polyetheretherketone solution, a sulfonated polystyrene solution, a sulfonated polysulfone solution, a sulfonated polyethylene solution, and a perfluorosulfonic acid resin solution.

[0010] In one embodiment, the hydrophilic binder comprises glycerol and / or PEG.

[0011] The hydrophilic binder can not only act as a dispersant to help the catalyst particles disperse evenly in the slurry, thereby improving the uniformity and stability of the catalyst layer, but also improve the water management performance of the catalyst layer to ensure the water distribution and transmission of the proton exchange membrane under low humidity or non-humidification conditions. In one embodiment, in the anode catalyst layer, in the Pt-C catalyst, the Pt loading is 0.03-0.3 mg / cm 2The mass of the effective component in the ionomer solution is 20-80% of the mass of C in the Pt-C catalyst, the mass of the Pt-C catalyst is 5-20% of the mass of the deionized water, the mass ratio of the deionized water to the high dielectric small molecule alcohol is 1:(1-4), the mass of the sulfonated lignin-doped conductive polymer nanoparticles is 0.5-5% of the mass of the Pt-C catalyst, and the mass of the hydrophilic adhesive is 2-5% of the mass of the deionized water; in the cathode catalyst layer, the catalyst is at least one of a Pt-C catalyst and a Ni-Fe catalyst, and in the Pt-C catalyst, the Pt loading is 0.3-0.7 mg / cm 2 The mass of the effective ingredient in the ionomer solution is 30-80% of the mass of C in the Pt-C catalyst, the mass of the Pt-C catalyst is 5-20% of the mass of the deionized water, the mass ratio of the deionized water to the high dielectric small molecule alcohol is 1:(1-4), and the mass of the polytetrafluoroethylene is 1-5% of the mass of the deionized water.

[0012] By using sulfonated lignin doped conductive polymer nanoparticles in the above-mentioned mass range, the hydrophilic effect and conductive effect of the sulfonated lignin doped conductive polymer nanoparticles in the anode catalyst layer can be effectively improved, and the sulfonated lignin doped conductive polymer nanoparticles can be more stably present in the anode catalyst. If the mass used is not within this range, the conductive properties and hydrophilic properties of the sulfonated lignin doped conductive polymer nanoparticles will decrease.

[0013] By using polytetrafluoroethylene in the above mass range, the hydrophobic effect of polytetrafluoroethylene in the cathode catalyst layer can be effectively improved, and polytetrafluoroethylene can be more stably present in the cathode catalyst. If the mass used is not within this range, the hydrophobic performance of polytetrafluoroethylene will decrease.

[0014] In a second aspect, the present invention provides a method for preparing a membrane electrode for a fuel cell, comprising the following steps: S1, preparing an anode catalyst layer: mixing the raw materials contained in the anode catalyst layer and preparing it on one side of a proton exchange membrane; preparing a cathode catalyst layer: mixing the raw materials contained in the cathode catalyst layer and preparing it on the other side of the proton exchange membrane; S2, sealing the anode catalyst layer and the cathode catalyst layer with a PEN frame with hot melt adhesive, and the edges of the anode catalyst layer and the cathode catalyst layer are respectively 0.5 to 1 cm; use the initial flat plate hot pressing method to bond the PEN frame; S3, prepare the anode side adhesion layer: apply conductive polymer-sulfonated lignin hydrogel to the edge of the surface of the anode catalyst layer to form an anode side adhesion layer for adhering the anode catalyst layer; prepare the cathode side adhesion layer: apply nafion-PEDOT conductive polymer to the edge of the surface of the cathode catalyst layer to form a cathode side adhesion layer for adhering the cathode diffusion layer; S4, paste the anode diffusion layer on the surface of the anode side adhesion layer, and paste the cathode diffusion layer on the surface of the cathode side adhesion layer; S5, use the secondary flat plate hot pressing method to treat, that is, obtain the membrane electrode for the fuel cell; the cathode diffusion layer and the anode diffusion layer respectively include a double-layer composite structure of carbon fiber and graphite and nano-silicon dioxide, and the nano-silicon dioxide is coated on the double-layer composite structure of carbon fiber and graphite.

[0015] The preparation method uses hydrophilic and relatively hydrophobic conductive adhesives to dispense glue on the anode and cathode, respectively, to fix the diffusion layer without losing conductivity. At the same time, the "mouth"-shaped packaging structure is hydrophilic and hydrophobic on both sides, respectively, to effectively improve performance; wherein nano-silicon dioxide is attached to the surface of the double-layer composite structure of carbon fiber and graphite by dipping or spraying to form a thin film coating; wherein the raw materials are mixed by at least one of ultrasonic mixing, high-speed shear mixing, ball milling mixing, and high-pressure homogenization mixing. The above mixing method can make the structures of the anode catalyst layer and the cathode catalyst layer more stable and avoid material precipitation.

[0016] In one embodiment, the mass of the nano-silicon dioxide is 10-40% of the mass of the double-layer composite structure of carbon fiber and graphite, the thickness of the carbon fiber is 150-310 μm, and the thickness of the graphite is 20-40 μm.

[0017] In one embodiment, the total thickness of the PEN frame is 40-80 μm.

[0018] The thickness range of the PEN frame can ensure improved hydrophilicity and water transport management performance while also avoiding waste of raw materials, saving materials and reducing costs.

[0019] In one embodiment, the pressure of the initial flat plate hot pressing method is less than 0.3 MPa, the temperature is less than 120°C, and the time is 30 s to 1 min; the pressure of the secondary flat plate hot pressing method is less than 0.3 MPa, the temperature is 130 to 140°C, and the time is 30 s to 2 min.

[0020] In one embodiment, the thickness of the anode catalyst layer and the cathode catalyst layer are 5-10 μm respectively.

[0021] This thickness range can ensure that the anode catalyst layer and the cathode catalyst layer have good catalytic efficiency while not causing waste of raw materials.

[0022] The beneficial effects of the present invention are: The present invention achieves efficient water management by adding a hydrophilic conductive polymer (sulfonated lignin-doped conductive polymer nanoparticles) to the anode catalyst slurry and a hydrophobic material (PTFE) to the cathode catalyst slurry. Specifically, the addition of the hydrophilic conductive polymer can absorb and retain moisture, reduce the drying phenomenon of the proton exchange membrane, and ensure sufficient moisture on the anode side; while the addition of the hydrophobic material PTFE can effectively prevent flooding, ensure rapid discharge of moisture on the cathode side, and maintain a good gas transmission channel.

[0023] In addition, the present invention improves the conductivity of the catalyst layer by optimizing the formula of the catalyst slurry, thereby improving the electrochemical performance of the battery. The hydrophilic conductive polymer and the nano-conductive particles can form a stable conductive network and improve the transmission efficiency of electrons and protons; the addition of high-dielectric small molecule alcohol can promote the conduction of protons and improve the ion conductivity of the proton exchange membrane, thereby improving the overall performance of the battery. By adding a hydrophilic binder (such as glycerol, PEG) to the catalyst slurry, the present invention ensures the uniform dispersion of the catalyst particles in the slurry and improves the uniformity and stability of the catalyst layer. The hydrophilic binder can reduce the interaction force between the catalyst particles, prevent the particles from agglomerating, and ensure the uniform distribution of the catalyst in the catalyst layer, thereby ensuring the thickness and uniformity of the catalyst layer and improving the performance of the catalyst layer.

[0024] In addition, during the preparation process, the present invention uses hydrophilic and relatively hydrophobic conductive adhesives to dispense the anode and cathode respectively, and fixes the diffusion layer without losing conductivity. At the same time, the "mouth"-shaped packaging structure is hydrophilic and hydrophobic on both sides, effectively improving performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The temperature of the fuel cells prepared in Examples 1 to 3 and Comparative Examples 1 to 2 in the test examples of the present invention varies with time; Figure 2This is a graph showing the power variation over time of the fuel cells prepared in Examples 1 to 3 and Comparative Examples 1 to 2 in the test examples of the present invention. DETAILED DESCRIPTION

[0026] The present invention will be further described below in conjunction with the accompanying drawings. Example

[0027] This embodiment provides a catalyst layer for a fuel cell and a method for preparing the membrane electrode thereof: The ingredients are as follows: Cationic catalyst layer: deionized water 100 g, ethanol 100 g, Pt-C catalyst 15 g (Pt loading is 0.03 mg / cm 2 ), 0.075 g of sulfonated lignin-doped conductive polymer nanoparticles, 2 g of glycerol, and 40 g of sulfonated polyetheretherketone solution (containing 10 wt% of sulfonated polyetheretherketone); Cathode catalyst: deionized water 100 g, ethylene glycol 100 g, Pt-C catalyst 15 g (Pt loading is 0.3 mg / cm 2 ), 1 g of polytetrafluoroethylene, and 31.5 g of sulfonated polystyrene solution (containing 10 wt% of sulfonated polystyrene).

[0028] Here are the steps: S1, mixing the slurries of the anode catalyst layer and the cathode catalyst layer respectively, by ultrasonic mixing; S2, applying the dispersed anode catalyst slurry on one side of the proton exchange membrane by screen printing; preparing a membrane layer with a dry film thickness of 5 μm; S3, applying the dispersed cathode catalyst slurry to the other side of the proton exchange membrane by screen printing; preparing a membrane layer with a dry film thickness of 5 μm; S4. Use ultrasound (40 Hz, 10°C, 10 min) to disperse 20 nm silica and acetylacetone in isopropanol. The mass ratio of silica, acetylacetone and isopropanol is 2%:5%:93%. Then add concentrated sulfuric acid until the pH is less than 1, and continue ultrasound (40 Hz, 5°C) for 30 min.

[0029] S5. Immerse the anode diffusion layer / cathode diffusion layer (double-layer composite structure of carbon fiber and graphite, with a carbon fiber thickness of 150 μm and a graphite thickness of 20 μm) in a silica suspension for 10 s by dipping, dry at 140°C for 10 min, and repeat the dipping process 4 to 5 times until the silica content in the diffusion layer reaches 10%.

[0030] S6, using a PEN frame with hot melt adhesive to seal the anode catalyst layer and the cathode catalyst layer, the edges of the anode catalyst layer and the cathode catalyst layer are 0.5 cm away from the PEN frame; using the initial flat plate hot pressing method (pressure of 0.2 MPa, temperature of 100° C., time of 0.5 min) to bond the PEN frame; S7, pasting the anode side diffusion layer: applying a conductive polymer-sulfonated lignin hydrogel to the edge of the surface of the anode catalyst layer to form an anode side diffusion layer, and the anode side diffusion layer is adhered to the edge of the anode catalyst layer; pasting the cathode side diffusion layer: applying a nafion-PEDOT conductive polymer to the edge of the surface of the cathode catalyst layer to form a cathode side diffusion layer, and the cathode side diffusion layer is adhered to the edge of the cathode catalyst layer; S8. The catalyst layer for the fuel cell is obtained by treating the catalyst by a secondary flat plate hot pressing method (pressure of 0.2 MPa, temperature of 130°C, time of 0.5 min). Example

[0031] This embodiment provides a catalyst layer for a fuel cell and a method for preparing the membrane electrode thereof: The ingredients are as follows: Cationic catalyst layer: 100 g deionized water, 400 g ethanol, 20 g Pt-C catalyst (Pt loading is 0.3 mg / cm 2 ), sulfonated lignin-doped conductive polymer nanoparticles 1 g, PEG 5 g, sulfonated polysulfone solution 56 g (containing 20wt% sulfonated polysulfone); Cathode catalyst: 100 g deionized water, 400 g ethylene glycol, 20 g Pt-C catalyst (Pt loading is 0.7 mg / cm 2 ), 5 g of polytetrafluoroethylene, and 48 g of sulfonated polyethylene solution (containing 10 wt% of sulfonated polyethylene).

[0032] Here are the steps: S1, mixing the slurries of the anode catalyst layer and the cathode catalyst layer respectively, using high-speed shear mixing; S2, preparing the dispersed anode catalyst slurry on one side of the proton exchange membrane by spraying; preparing the membrane layer with a dry film thickness of 10 μm; S3, applying the dispersed cathode catalyst slurry to the other side of the proton exchange membrane by wire rod coating, scraper coating, or slit coating; preparing a membrane layer with a dry film thickness of 10 μm; S4. Use ultrasound (40 Hz, 10°C, 10 min) to disperse 20 nm silica and acetylacetone in isopropanol. The mass ratio of silica, acetylacetone and isopropanol is 2%:5%:93%. Then add concentrated sulfuric acid until the pH is less than 1, and continue ultrasound (40 Hz, 5°C) for 30 min.

[0033] S5. Immerse the anode diffusion layer / cathode diffusion layer (double-layer composite structure of carbon fiber and graphite, with a carbon fiber thickness of 310 μm and a graphite thickness of 40 μm) in a silica suspension for 10 s by dipping, dry at 140°C for 10 min, and repeat the dipping process 4 to 5 times until the silica content in the diffusion layer reaches 40%.

[0034] S6, using a PEN frame with hot melt adhesive to seal the anode catalyst layer and the cathode catalyst layer, the edges of the anode catalyst layer and the cathode catalyst layer are 1 cm away from the PEN frame respectively; using the initial flat plate hot pressing method (pressure of 0.28 MPa, temperature of 118° C., time of 1 min) to bond the PEN frame; S7, pasting the anode side diffusion layer: applying the conductive polymer-sulfonated lignin hydrogel on the edge of the surface of the anode catalyst layer by dispensing, and pasting the anode side diffusion layer; pasting to prepare the cathode side diffusion layer: applying the nafion-PEDOT conductive polymer on the edge of the surface of the cathode catalyst layer by dispensing, and pasting the cathode side diffusion layer; S8. The catalyst layer for the fuel cell is obtained by using a secondary flat plate hot pressing method (pressure of 0.28 MPa, temperature of 140°C, and time of 2 min). Example

[0035] This embodiment provides a catalyst layer for a fuel cell and a method for preparing the membrane electrode thereof: The ingredients are as follows: Cationic catalyst layer: deionized water 100 g, ethanol 200 g, Pt-C catalyst 18 g (Pt loading is 0.2 mg / cm 2 ), 0.36 g of sulfonated lignin-doped conductive polymer nanoparticles, 4 g of a mixture of PEG and glycerol, and 43.2 g of a mixed solution of sulfonated polysulfone and sulfonated polystyrene (containing 10 wt% of sulfonated polysulfone and 10 wt% of sulfonated polystyrene); Cathode catalyst: deionized water 100 g, ethylene glycol 300 g, Pt-C catalyst 16 g (Pt loading is 0.5 mg / cm 2 ), 4 g of polytetrafluoroethylene, and 28 g of a mixed solution of sulfonated polyethylene and sulfonated polyetheretherketone (containing 10 wt% of sulfonated polyethylene and 10 wt% of sulfonated polyetheretherketone).

[0036] Here are the steps: S1, mixing the slurries of the anode catalyst layer and the cathode catalyst layer respectively, by ball milling; S2, applying the dispersed anode catalyst slurry to one side of the proton exchange membrane by a transfer printing method; preparing a membrane layer with a dry film thickness of 8 μm; S3, applying the dispersed cathode catalyst slurry to the other side of the proton exchange membrane by transfer printing; the prepared membrane layer has a dry film thickness of 8 μm; S4. Use ultrasound (40 Hz, 10°C, 10 min) to disperse 20 nm silica and acetylacetone in isopropanol. The mass ratio of silica, acetylacetone and isopropanol is 2%:5%:93%. Then add concentrated sulfuric acid until the pH is less than 1, and continue ultrasound (40 Hz, 5°C) for 30 min.

[0037] S5. Immerse the anode diffusion layer / cathode diffusion layer (double-layer composite structure of carbon fiber and graphite, with a carbon fiber thickness of 220 μm and a graphite thickness of 30 μm) in a silica suspension for 10 s by dipping, dry at 140°C for 10 min, and repeat the dipping process 4 to 5 times until the silica content on the diffusion layer reaches 30%.

[0038] S6, using a PEN frame with hot melt adhesive to seal the anode catalyst layer and the cathode catalyst layer, the edges of the anode catalyst layer and the cathode catalyst layer are respectively 1 cm away from the PEN frame; using the initial flat plate hot pressing method (pressure 0.25 MPa, temperature 110° C., time 1.5 min) to bond the PEN frame; S7, pasting the anode side diffusion layer: applying a conductive polymer-sulfonated lignin hydrogel to the edge of the surface of the anode catalyst layer to form an anode side adhesion layer, and the anode side diffusion layer adheres to the edge of the anode catalyst layer; pasting the cathode side diffusion layer: applying a nafion-PEDOT conductive polymer to the edge of the surface of the cathode catalyst layer to form a cathode side adhesion layer, and the cathode side diffusion layer adheres to the edge of the cathode catalyst layer; S8. The catalyst layer for the fuel cell is obtained by treating the catalyst by a secondary flat plate hot pressing method (pressure of 0.25 MPa, temperature of 135°C, and time of 1.5 min).

[0039] Comparative Example 1 The sulfonated lignin doping was removed and only conductive polymer nanoparticles were used, and the rest was the same as in Example 2.

[0040] Comparative Example 2 The polytetrafluoroethylene is removed, and the rest is the same as in Example 2.

[0041] Test example The catalyst layers of Examples 1-3 and Comparative Examples 1-2 were cut into 5 cm×5 cm single pieces, which were plastic-sealed by hot-melt plastic sealing and matched with a 180 μm diffusion layer to prepare 30 membrane electrodes, which were stacked, activated and tested for performance.

[0042] Activation conditions: hydrogen 0.1 MPa, air 0.1 MPa, flow rate of 700 mL / min, 2800 mL / min, 60% humidification, 50°C, 4 A, constant current discharge for 30 min every 2 A, 10 A, constant current discharge for 30 min every 5 A, 19 A, constant current discharge for 30 min every 2 A).

[0043] Constant current discharge conditions: hydrogen 0.1 MPa, air 0.1 MPa, flow rate 700 mL / min, 2800 mL / min, 60% humidification, 50°C, 15 A constant current discharge for 110 h. The stack power and temperature were continuously recorded.

[0044] according to Figure 1 The results show that the temperature of the fuel cell prepared by the technical solutions of Examples 1 to 3 is significantly lower than that of the fuel cell prepared in Comparative Examples 1 to 2, which shows that the fuel cell catalyst layer and membrane electrode prepared by the present invention have a good effect in reducing the temperature of the fuel cell. Figure 2 The results show that the power of the fuel cell prepared by the technical solutions of Examples 1 to 3 is significantly higher than the power of the fuel cell prepared in Comparative Examples 1 to 2. It can be seen that the fuel cell catalyst layer and membrane electrode prepared by the present invention have a good effect in improving the temperature power of the fuel cell.

[0045] In the description of the present invention, it is necessary to understand that the terms "upper", "lower", "bottom", "top", "front", "back", "inside", "outside", "left", "right", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0046] Although the present invention is described herein with reference to specific embodiments, it should be understood that these embodiments are merely examples of the principles and applications of the present invention. It should therefore be understood that many modifications may be made to the exemplary embodiments and that other arrangements may be devised without departing from the spirit and scope of the present invention as defined by the appended claims. It should be understood that the various dependent claims and features described herein may be combined in a manner different from that described in the original claims. It should also be understood that features described in conjunction with individual embodiments may be used in other described embodiments.

Claims

1. A catalyst layer for a fuel cell, characterized in that: It includes an anode catalyst and a cathode catalyst, wherein the anode catalyst layer includes: a Pt-C catalyst, a high dielectric small molecule alcohol, sulfonated lignin-doped conductive polymer nanoparticles, a hydrophilic adhesive, an ionomer solution, and deionized water; The cathode catalyst layer comprises a catalyst, an ionomer solution, a high dielectric small molecule alcohol, polytetrafluoroethylene and deionized water.

2. The fuel cell catalyst layer according to claim 1, characterized in that: The high dielectric small molecule alcohol includes at least one of ethanol, ethylene glycol, n-propanol and isopropanol.

3. The fuel cell catalyst layer according to claim 1, characterized in that: The ionomer solution includes at least one of a sulfonated polyetheretherketone solution, a sulfonated polystyrene solution, a sulfonated polysulfone solution, a sulfonated polyethylene solution, and a perfluorosulfonic acid resin solution.

4. The fuel cell catalyst layer according to claim 1, characterized in that: The hydrophilic binder includes glycerol and / or PEG.

5. The fuel cell catalyst layer according to claim 1, characterized in that: In the anode catalyst layer, in the Pt-C catalyst, the Pt loading is 0.03-0.3 mg / cm 2 , the mass of the effective component in the ionomer solution is 20-80% of the mass of C in the Pt-C catalyst, the mass of the Pt-C catalyst is 5-20% of the mass of the deionized water, the mass ratio of the deionized water to the high dielectric small molecule alcohol is 1:(1-4), the mass of the sulfonated lignin-doped conductive polymer nanoparticles is 0.5-5% of the mass of the Pt-C catalyst, and the mass of the hydrophilic adhesive is 2-5% of the mass of the deionized water; In the cathode catalyst layer, the catalyst in the cathode catalyst layer is at least one of a Pt-C catalyst and a Ni-Fe catalyst, and in the Pt-C catalyst, the loading amount of Pt is 0.3-0.7 mg / cm 2 The mass of the effective ingredient in the ionomer solution is 30-80% of the mass of C in the Pt-C catalyst, the mass of the Pt-C catalyst is 5-20% of the mass of the deionized water, the mass ratio of the deionized water to the high dielectric small molecule alcohol is 1:(1-4), and the mass of the polytetrafluoroethylene is 1-5% of the mass of the deionized water.

6. A method for preparing a membrane electrode having a catalyst layer for a fuel cell according to any one of claims 1 to 5, characterized in that: The steps include: S1. preparing an anode catalyst layer: mixing raw materials contained in the anode catalyst layer and preparing the anode catalyst layer on one side of a proton exchange membrane; Prepare the cathode catalyst layer: mix the raw materials contained in the cathode catalyst layer and prepare it on the other side of the proton exchange membrane; S2, seal the anode catalyst layer and the cathode catalyst layer with a PEN frame with hot melt adhesive, and the edges of the anode catalyst layer and the cathode catalyst layer are respectively 0.5-1 cm away from the PEN frame; use the initial flat plate hot pressing method to bond the PEN frame; S3, preparing an anode side adhesion layer: applying a conductive polymer-sulfonated lignin hydrogel to the edge of the surface of the anode catalyst layer to form an anode side adhesion layer for adhering the anode catalyst layer; Preparation of cathode side adhesion layer: dispensing nafion-PEDOT conductive polymer on the edge of the cathode catalyst layer surface to form a cathode side adhesion layer for adhering the cathode diffusion layer; S4, pasting the anode diffusion layer on the surface of the anode side adhesion layer, and pasting the cathode diffusion layer on the surface of the cathode side adhesion layer; S5, using a secondary flat plate hot pressing method to obtain the membrane electrode for the fuel cell; The cathode diffusion layer and the anode diffusion layer respectively include a double-layer composite structure of carbon fiber and graphite and nano silicon dioxide, and the nano silicon dioxide is coated on the double-layer composite structure of carbon fiber and graphite.

7. The method for preparing a membrane electrode having a catalyst layer for a fuel cell according to claim 6, characterized in that: The mass of the nano-silicon dioxide is 10-40% of the mass of the double-layer composite structure of carbon fiber and graphite, the thickness of the carbon fiber is 150-310 μm, and the thickness of the graphite is 20-40 μm.

8. The method for preparing a membrane electrode having a catalyst layer for a fuel cell according to claim 6, characterized in that: The total thickness of the PEN frame is 40-80 μm.

9. The method for preparing a membrane electrode having a catalyst layer for a fuel cell according to claim 6, characterized in that: The pressure of the primary flat plate hot pressing method is less than 0.3 MPa, the temperature is less than 120°C, and the time is 30 s to 1 min; the pressure of the secondary flat plate hot pressing method is less than 0.3 MPa, the temperature is 130 to 140°C, and the time is 30 s to 2 min.

10. The method for preparing a membrane electrode having a catalyst layer for a fuel cell according to claim 6, characterized in that: The thickness of the anode catalyst layer and the cathode catalyst layer are 5-10 μm respectively.

Citation Information

Patent Citations

  • Membrane electrode containing hydrophilic high polymer in anode catalytic layer and preparation method thereof

    CN102437343A

  • Self-humidifying membrane electrode and preparation method thereof

    CN116759586A

  • Membrane electrode of fuel cell and preparation method of membrane electrode

    CN117810498A

  • Preparation method of fuel cell membrane electrode CCM

    CN118281241A

  • Catalytic layer for fuel cell and preparation method thereof

    CN119153717A

Cited By

  • Catalytic layer for fuel cell and preparation method thereof

    CN119153717A

  • Catalytic layer for fuel cell and preparation method thereof

    CN119153717B