A PS composite material with good antibacterial and VOC performance and a preparation method thereof
Through the combination of mesoporous La2O3/gallic acid/polystyrene hydrogel and antioxidants, the problem of insufficient antibacterial and VOC performance of PS composite materials is solved, significantly improving its performance and expanding the application field.
Patent Information
- Application Number
- CN202310474817.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-04-28
AI Technical Summary
The lack of antibacterial properties and VOC properties of polystyrene (PS) composites limit their application in specific fields.
Mesoporous La2O3/gallic acid/polystyrene hydrogel is used to combine with antioxidants, and a PS composite material with good antibacterial and VOC performance is prepared through specific preparation methods and component ratios.
The antibacterial properties and VOC properties of PS composite materials have been significantly improved, greatly expanding its application potential in automotive interiors and other fields.
Smart Images

Figure BDA0004205138040000091 
Figure BDA0004205138040000101
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite materials, and in particular to a PS composite material with good antibacterial performance and VOC performance and a preparation method thereof. Background Art
[0002] Polystyrene (PS) is a widely used polymer polyester resin. PS has the advantages of good fatigue resistance, good heat resistance, excellent dimensional stability, etc. However, the antibacterial and VOC properties of PS are average, which limits the application of PS composites in some specific fields.
[0003] In view of this situation, the present invention innovatively produces a PS composite material, which has excellent antibacterial and VOC properties. This material has not been reported so far, which has very important practical significance for expanding the application of PS composite materials. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a PS composite material with good antibacterial and VOC performance and a preparation method thereof, which has excellent antibacterial and VOC performance, which is of great significance.
[0005] The technical problem to be solved by the present invention is achieved through the following technical solutions:
[0006] A PS composite material with good antibacterial and VOC performance comprises the following components in parts by weight: 80-100 parts of polystyrene (PS), 8-12 parts of mesoporous La2O3 / gallic acid / polystyrene hydrogel and 0.1-0.5 parts of antioxidant.
[0007] Preferably, the following components are included in weight: 90 parts of polystyrene (PS), 10 parts of mesoporous La2O3 / gallic acid / polystyrene hydrogel and 0.3 parts of antioxidant.
[0008] Preferably, the mesoporous La2O3 / gallic acid / polystyrene hydrogel is prepared by the following method:
[0009] (1) Lanthanum nitrate, ammonia water, and deionized water are placed in a reaction vessel and stirred at 30-50° C. for 6-8 hours to prepare solution A;
[0010] (2) Filtering, washing, and drying solution A, and calcining in a muffle furnace at 720-760° C. for 10-16 h to obtain mesoporous La2O3;
[0011] (3) placing mesoporous La2O3, initiator ammonium persulfate, solvent ether, gallic acid, and styrene in a reaction vessel, reacting in a water bath at 50-70°C for 10-14 hours, filtering, washing, and drying to obtain a mesoporous La2O3 / gallic acid / polystyrene hydrogel.
[0012] Preferably, in step (1), the mass ratio of lanthanum nitrate, ammonia water and deionized water is (30-40): (50-60): (90-110).
[0013] Preferably, in step (3), the mass ratio of mesoporous La2O3, initiator ammonium persulfate, solvent ether, gallic acid and styrene is (30-40): (0.1-0.3): (80-90): (20-30): (16-18).
[0014] Preferably, the antioxidant is one or a mixture of tris(2,4-di-tert-butyl)phenyl phosphite (Irganox 168 for short), pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (Irganox 1010 for short) and 1,3,5-trimethyl-2,4,6-(3,5-di-tert-butyl-4-hydroxybenzyl)benzene (Irganox 1330 for short) produced by BASF.
[0015] A method for preparing a PS composite material with good antibacterial performance and VOC performance comprises the following steps:
[0016] S1. Weigh 80-100 parts of polystyrene (PS), 8-12 parts of mesoporous La2O3 / gallic acid / polystyrene hydrogel, and 0.1-0.5 parts of antioxidant, mix and stir evenly to obtain a mixture;
[0017] Among them, the mesoporous La2O3 / gallic acid / polystyrene hydrogel was prepared by the following method:
[0018] (1) Lanthanum nitrate, ammonia water, and deionized water are placed in a reaction vessel at a mass ratio of (30-40): (50-60): (90-110), and stirred at 30-50° C. for 6-8 hours to prepare solution A;
[0019] (2) Filtering, washing, and drying solution A, and calcining in a muffle furnace at 720-760° C. for 10-16 h to obtain mesoporous La2O3;
[0020] (3) placing mesoporous La2O3, initiator ammonium persulfate, solvent ether, gallic acid, and styrene in a reaction vessel at a mass ratio of (30-40):(0.1-0.3):(80-90):(20-30):(16-18), reacting in a 50-70°C water bath for 10-14 hours, filtering, washing, and drying to obtain a mesoporous La2O3 / gallic acid / polystyrene hydrogel;
[0021] S2, extruding the mixed material obtained in step S1 from an extruder and granulating it to obtain a PS composite material.
[0022] Preferably, step S2 specifically includes:
[0023] The extruder in step S1 is a twin-screw extruder, wherein the twin-screw extruder includes six temperature zones arranged in sequence, with a temperature of 160-180°C in zone one, a temperature of 210-250°C in zone two, a temperature of 210-250°C in zone three, a temperature of 210-250°C in zone four, a temperature of 210-250°C in zone five, a temperature of 210-250°C in zone six, a die head temperature of 210-250°C, and a screw speed of 200-280r / min.
[0024] Preferably, the antioxidant is one or a mixture of tris(2,4-di-tert-butyl)phenyl phosphite, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and 1,3,5-trimethyl-2,4,6-(3,5-di-tert-butyl-4-hydroxybenzyl)benzene.
[0025] Application of PS composite material in automobile interior decoration.
[0026] The above technical solution of the present invention has the following beneficial effects:
[0027] (1) The preparation process of the mesoporous La2O3 / gallic acid / polystyrene hydrogel in this patent is as follows:
[0028] La(NO3)3+NH3·H2O→La(OH)3+NH4NO3;
[0029] 2La(OH)3→La2O3+3H2O.
[0030] (2) The excellent antibacterial properties of the PS composite material prepared in this patent are mainly attributed to the catechol structure of gallic acid. The catechol group can be adsorbed on the surface of the bacterial cell wall, destroying the cell wall structure and the permeability of the cell membrane, and then killing the bacteria.
[0031] (3) The excellent VOC performance of the PS composite material prepared in this patent is mainly attributed to the fact that the mesoporous La2O3 can adsorb small molecules in VOCs, thereby improving the VOC performance of the PS composite material.
[0032] (4) Compared with other substances that improve VOC and antibacterial properties, the mesoporous La2O3 / gallic acid / polystyrene hydrogel prepared in this patent has better compatibility with the PS matrix, and has better VOC performance and antibacterial properties. DETAILED DESCRIPTION
[0033] Various exemplary embodiments of the present invention will now be described in detail. It should be noted that the relative arrangement of components and steps, numerical expressions and numerical values set forth in these embodiments do not limit the scope of the present invention unless otherwise specifically stated.
[0034] The raw materials used in the embodiments of the present invention are as follows:
[0035] PS (model 2002U), Polyplastics, Japan; lanthanum nitrate, Hubei Xinrunde Chemical Co., Ltd.; ammonia water, Shandong Ruijiang Chemical Co., Ltd.; deionized water, Jinan Hairuibao Chemical Co., Ltd.; ammonium persulfate, Shandong Yushuo Chemical Co., Ltd.; ether, Jinan Guangyu Chemical Co., Ltd.; gallic acid, Jiangsu Jiujia Biotechnology Co., Ltd.; styrene, Shandong Qiyuan Chemical Co., Ltd.; antioxidants (models Irganox168, Irganox1010, Irganox1330), BASF, Germany.
[0036] The testing instrument used in the present invention is as follows:
[0037] ZSK30 twin-screw extruder, W&P, Germany; JL-1000 tensile testing machine, Guangzhou Guangcai Experimental Instrument Co., Ltd.; HTL900-T-5B injection molding machine, Haitai Plastic Machinery Co., Ltd.; XCJ-500 impact testing machine, Chengde Testing Machine Factory; QT-1196 tensile tester, Dongguan Gaotai Testing Instrument Co., Ltd.; QD-GJS-B12K high-speed mixer, Beijing Hengaode Instrument Co., Ltd.
[0038] Example 1
[0039] (I) Preparation of mesoporous La2O3 / gallic acid / polystyrene hydrogel:
[0040] (1) Weigh 300 g of lanthanum nitrate, 500 g of ammonia water, and 900 g of deionized water, place them in a reaction vessel, and stir at 30° C. for 6 h to prepare solution A;
[0041] (2) Filtering, washing, and drying solution A, and calcining it at 720° C. in a muffle furnace for 10 h to obtain mesoporous La2O3;
[0042] (3) Weigh 300 g of mesoporous La2O3, 1 g of initiator ammonium persulfate, 800 g of solvent ether, 200 g of gallic acid, and 160 g of styrene, place them in a reaction vessel, react in a 50°C water bath for 10 h, filter, wash, and dry to obtain mesoporous La2O3 / gallic acid / polystyrene hydrogel M1.
[0043] (II) Preparation of PS composite materials with good antibacterial and VOC performance:
[0044] S1, weigh 80 parts of PS, 8 parts of mesoporous La2O3 / gallic acid / polystyrene hydrogel M1, and 0.1 parts of Irganox1010, mix and stir evenly to obtain a mixture;
[0045] S2, extruding the mixed material obtained in step S1 from an extruder and granulating it to obtain a PS composite material P1.
[0046] The temperatures and screw speeds of each zone of the twin-screw extruder are: zone 1 temperature 160°C, zone 2 temperature 210°C, zone 3 temperature 210°C, zone 4 temperature 210°C, zone 5 temperature 210°C, zone 6 temperature 210°C, die head temperature 210°C, and screw speed 200r / min.
[0047] Example 2
[0048] (I) Preparation of mesoporous La2O3 / gallic acid / polystyrene hydrogel:
[0049] (1) Weigh 350 g of lanthanum nitrate, 550 g of ammonia water, and 1.0 kg of deionized water, place in a reaction vessel, and stir at 40° C. for 7 h to prepare solution A;
[0050] (2) Filtering, washing, and drying solution A, and calcining it at 740° C. in a muffle furnace for 13 h to obtain mesoporous La2O3;
[0051] (3) Weigh 350 g of mesoporous La2O3, 2 g of initiator ammonium persulfate, 850 g of solvent ether, 250 g of gallic acid, and 170 g of styrene, place them in a reaction vessel, react in a 60°C water bath for 12 h, filter, wash, and dry to obtain mesoporous La2O3 / gallic acid / polystyrene hydrogel M2.
[0052] (II) Preparation of PS composite materials with good antibacterial and VOC performance:
[0053] S1, weigh 90 parts of PS, 10 parts of mesoporous La2O3 / gallic acid / polystyrene hydrogel M2, 0.1 parts of Irganox1010, and 0.2 parts of Irganox168, mix and stir evenly to obtain a mixture;
[0054] S2, extruding the mixed material obtained in step S1 from an extruder and granulating it to obtain a PS composite material P2.
[0055] The temperatures and screw speeds of each zone of the twin-screw extruder are: zone 1 temperature 180°C, zone 2 temperature 250°C, zone 3 temperature 250°C, zone 4 temperature 250°C, zone 5 temperature 250°C, zone 6 temperature 250°C, die head temperature 250°C, and screw speed 280r / min.
[0056] Example 3
[0057] (I) Preparation of mesoporous La2O3 / gallic acid / polystyrene hydrogel:
[0058] (1) Weigh 400 g of lanthanum nitrate, 600 g of ammonia water, and 1.1 kg of deionized water, place them in a reaction vessel, and stir at 50° C. for 8 h to prepare solution A;
[0059] (2) Filtering, washing, and drying solution A, and calcining it at 760° C. in a muffle furnace for 16 h to obtain mesoporous La2O3;
[0060] (3) Weigh 400 g of mesoporous La2O3, 3 g of initiator ammonium persulfate, 900 g of solvent ether, 300 g of gallic acid, and 180 g of styrene, place them in a reaction vessel, react in a 70°C water bath for 14 h, filter, wash, and dry to obtain mesoporous La2O3 / gallic acid / polystyrene hydrogel M3.
[0061] (II) Preparation of PS composite materials with good antibacterial and VOC performance:
[0062] S1, weigh 100 parts of PS, 12 parts of mesoporous La2O3 / gallic acid / polystyrene hydrogel M3, 0.2 parts of Irganox1330, 0.1 parts of Irganox168, and 0.2 parts of Irganox1010, mix and stir evenly to obtain a mixture;
[0063] S2, extruding the mixed material obtained in step S1 from an extruder and granulating it to obtain a PS composite material P3.
[0064] The temperatures and screw speeds of each zone of the twin-screw extruder are: zone 1 temperature 170°C, zone 2 temperature 230°C, zone 3 temperature 230°C, zone 4 temperature 230°C, zone 5 temperature 230°C, zone 6 temperature 230°C, die head temperature 230°C, and screw speed 240r / min.
[0065] Example 4
[0066] (I) Preparation of mesoporous La2O3 / gallic acid / polystyrene hydrogel:
[0067] (1) Weigh 325 g of lanthanum nitrate, 545 g of ammonia water, and 985 g of deionized water, place them in a reaction vessel, and stir and react at 45° C. for 7 h to prepare solution A;
[0068] (2) Filtering, washing, and drying solution A, and calcining it at 745° C. in a muffle furnace for 15 h to obtain mesoporous La2O3;
[0069] (3) Weigh 315 g of mesoporous La2O3, 2.5 g of initiator ammonium persulfate, 865 g of solvent ether, 295 g of gallic acid, and 175 g of styrene, place them in a reaction vessel, react in a 55°C water bath for 13 h, filter, wash, and dry to obtain mesoporous La2O3 / gallic acid / polystyrene hydrogel M4.
[0070] (II) Preparation of PS composite materials with good antibacterial and VOC performance:
[0071] S1, weigh 95 parts of PS, 11 parts of mesoporous La2O3 / gallic acid / polystyrene hydrogel M4, 0.1 parts of Irganox1010, and 0.2 parts of Irganox1330, mix and stir evenly to obtain a mixture;
[0072] S2. Extruding the mixed material obtained in step S1 from an extruder and granulating it to obtain a PS composite material P4.
[0073] The temperatures and screw speeds of each zone of the twin-screw extruder are: zone 1 temperature 165°C, zone 2 temperature 215°C, zone 3 temperature 215°C, zone 4 temperature 215°C, zone 5 temperature 215°C, zone 6 temperature 215°C, die head temperature 215°C, and screw speed 260r / min.
[0074] Example 5
[0075] (I) Preparation of mesoporous La2O3 / gallic acid / polystyrene hydrogel:
[0076] (1) Weigh 335 g of lanthanum nitrate, 515 g of ammonia water, and 995 g of deionized water, place them in a reaction vessel, and stir and react at 45° C. for 8 h to prepare solution A;
[0077] (2) Solution A was filtered, washed, dried, and calcined in a muffle furnace at 755° C. for 15 h to obtain mesoporous La2O3.
[0078] (3) Weigh 385 g of mesoporous La2O3, 1.5 g of initiator ammonium persulfate, 865 g of solvent ether, 285 g of gallic acid, and 165 g of styrene, place them in a reaction vessel, react in a 68°C water bath for 13 h, filter, wash, and dry to obtain mesoporous La2O3 / gallic acid / polystyrene hydrogel M5.
[0079] (II) Preparation of PS composite materials with good antibacterial and VOC performance:
[0080] S1, weigh 85 parts of PS, 9 parts of mesoporous La2O3 / gallic acid / polystyrene hydrogel M5, 0.1 parts of Irganox1010, and 0.1 parts of Irganox168, mix and stir evenly to obtain a mixture;
[0081] S2. Extruding the mixed material obtained in step S1 from an extruder and granulating it to obtain a PS composite material P5.
[0082] The temperatures and screw speeds of each zone of the twin-screw extruder are: zone 1 temperature 170°C, zone 2 temperature 230°C, zone 3 temperature 225°C, zone 4 temperature 225°C, zone 5 temperature 225°C, zone 6 temperature 225°C, die head temperature 225°C, and screw speed 250r / min.
[0083] Comparative Example 1
[0084] (1) Weigh 85 parts of PS, 0.1 parts of Irganox 1010, and 0.2 parts of Irganox 168, mix and stir evenly to obtain a mixture;
[0085] (2) The mixed material obtained in step (1) is extruded from an extruder and granulated to obtain a PS composite material D1.
[0086] The temperatures and screw speeds of each zone of the twin-screw extruder are: zone 1 temperature 170°C, zone 2 temperature 230°C, zone 3 temperature 225°C, zone 4 temperature 225°C, zone 5 temperature 225°C, zone 6 temperature 225°C, die head temperature 225°C; screw speed 250r / min.
[0087] Comparative Example 2
[0088] (1) Weigh 85 parts of PS, 9 parts of mesoporous La2O3, 0.1 parts of Irganox1010, and 0.1 parts of Irganox1330, mix and stir to obtain a mixture;
[0089] (2) The mixed material obtained in step (1) is extruded from an extruder and granulated to obtain a PS composite material D2.
[0090] The temperatures and screw speeds of each zone of the twin-screw extruder are: zone 1 temperature 170°C, zone 2 temperature 230°C, zone 3 temperature 225°C, zone 4 temperature 225°C, zone 5 temperature 225°C, zone 6 temperature 225°C, die head temperature 225°C; screw speed 250r / min.
[0091] Comparative Example 3
[0092] (1) Weigh 85 parts of PS, 5 parts of mesoporous La2O3, 4 parts of gallic acid, 0.1 parts of Irganox1010, and 0.1 parts of Irganox168, mix and stir to obtain a mixture;
[0093] (2) The mixed material obtained in step (1) is extruded from an extruder and granulated to obtain a PS composite material D3.
[0094] The temperatures and screw speeds of each zone of the twin-screw extruder are: zone 1 temperature 170°C, zone 2 temperature 230°C, zone 3 temperature 225°C, zone 4 temperature 225°C, zone 5 temperature 225°C, zone 6 temperature 225°C, die head temperature 225°C; screw speed 250r / min.
[0095] The PS composite materials prepared in the above Examples 1-5 and Comparative Examples 1-3 were made into strips by injection molding and tested. The test data are shown in the following table:
[0096]
[0097]
[0098] From the data in the above table, we can see that;
[0099] In summary, compared with Comparative Examples 1-3, Examples 1-5 have better antibacterial properties and VOC properties, which indicates that the antibacterial properties and VOC properties of the PS in the present invention are greatly improved compared with conventional PS. This greatly expands the application field of PS composite materials and is of great significance.
[0100] Although the present invention has been disclosed as above by the embodiments, it is not intended to limit the present invention. Any person skilled in the art may make various choices and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention is limited by the claims and their equivalents.
Claims
1. A PS composite material with good antibacterial and VOC performance, characterized in that: The invention comprises the following components in parts by weight: 80-100 parts of polystyrene (PS), 8-12 parts of mesoporous La2O3 / gallic acid / polystyrene hydrogel and 0.1-0.5 parts of antioxidant; The mesoporous La2O3 / gallic acid / polystyrene hydrogel is prepared as follows: (1) Lanthanum nitrate, ammonia water and deionized water are placed in a reaction vessel and stirred at 30-50°C for 6-8 hours to prepare solution A; (2) Filter, wash and dry solution A, and calcine it in a muffle furnace at 720-760°C for 10-16 hours to obtain mesoporous La2O3; (3) Place mesoporous La2O3, initiator ammonium persulfate, solvent ether, gallic acid, and styrene in a reaction vessel, react in a 50-70°C water bath for 10-14 hours, filter, wash, and dry to obtain mesoporous La2O3 / gallic acid / polystyrene hydrogel.
2. The PS composite material with good antibacterial performance and VOC performance according to claim 1, characterized in that: The invention comprises the following components in parts by weight: 90 parts of polystyrene (PS), 10 parts of mesoporous La2O3 / gallic acid / polystyrene hydrogel and 0.3 parts of antioxidant.
3. The PS composite material with good antibacterial performance and VOC performance according to claim 1, characterized in that: In step (1), the mass ratio of lanthanum nitrate, ammonia water and deionized water is (30-40): (50-60): (90-110).
4. The PS composite material with good antibacterial performance and VOC performance according to claim 1, characterized in that: In step (3), the mass ratio of mesoporous La2O3, initiator ammonium persulfate, solvent ether, gallic acid, and styrene is (30-40): (0.1-0.3): (80-90): (20-30): (16-18).
5. The PS composite material with good antibacterial performance and VOC performance according to claim 1, characterized in that: The antioxidant is one or a mixture of tris(2,4-di-tert-butyl)phenyl phosphite, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and 1,3,5-trimethyl-2,4,6-(3,5-di-tert-butyl-4-hydroxybenzyl)benzene.
6. The method for preparing a PS composite material with good antibacterial performance and VOC performance according to any one of claims 1, 3-5, characterized in that: The following steps are involved: S1. Weigh 80-100 parts of polystyrene (PS), 8-12 parts of mesoporous La2O3 / gallic acid / polystyrene hydrogel, and 0.1-0.5 parts of antioxidant, mix and stir evenly to obtain a mixture; Among them, the mesoporous La2O3 / gallic acid / polystyrene hydrogel was prepared by the following method: (1) Place lanthanum nitrate, ammonia water, and deionized water in a reaction vessel at a mass ratio of (30-40): (50-60): (90-110), and stir at 30-50°C for 6-8 hours to prepare solution A; (2) Filter, wash and dry solution A, and calcine it in a muffle furnace at 720-760°C for 10-16 hours to obtain mesoporous La2O3; (3) placing mesoporous La2O3, initiator ammonium persulfate, solvent ether, gallic acid, and styrene in a reaction vessel in a mass ratio of (30-40): (0.1-0.3): (80-90): (20-30): (16-18), reacting in a 50-70°C water bath for 10-14 hours, filtering, washing, and drying to obtain a mesoporous La2O3 / gallic acid / polystyrene hydrogel; S2, extruding the mixed material obtained in step S1 from an extruder and granulating it to obtain a PS composite material.
7. The method for preparing a PS composite material with good antibacterial and VOC performance according to claim 6, characterized in that: Step S2 is specifically as follows: The extruder of step S2 is a twin-screw extruder, wherein the twin-screw extruder includes six temperature zones arranged in sequence, with a temperature of 160-180°C in zone one, a temperature of 210-250°C in zone two, a temperature of 210-250°C in zone three, a temperature of 210-250°C in zone four, a temperature of 210-250°C in zone five, a temperature of 210-250°C in zone six, a die head temperature of 210-250°C, and a screw speed of 200-280r / min.
8. The method for preparing a PS composite material with good antibacterial performance and VOC performance according to claim 6, characterized in that: The antioxidant is one or a mixture of tris(2,4-di-tert-butyl)phenyl phosphite, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and 1,3,5-trimethyl-2,4,6-(3,5-di-tert-butyl-4-hydroxybenzyl)benzene.
9. Use of the PS composite material according to any one of claims 1 to 5 or the PS composite material prepared according to any one of claims 6 to 8 in automobile interior decoration.
Citation Information
Patent Citations
Heat oxygen aging resistance high polymer material and preparation method and application thereof
CN101633789A
Modified polymers and compositions containing the same
CN101696248A
Preparation method of intercalated composite heat stabilizer for PVC
CN107245244A
Antibacterial magnetic composite coating material used for fabric, preparation method thereof and antibacterial fabric