Wide temperature range, high load-bearing 4D printing nickel-titanium-based alloy based on self-locking functional primitives and its preparation method and application
By combining NiTiCuZr alloy with NiTi alloy and using hot extrusion technology to form self-locking primitives, it solves the problem of limited service capabilities of existing shape memory alloys in extreme environments and achieves wide temperature range and high load-bearing 4D nickel printing. Titanium-based alloy with excellent superelastic properties and wider service temperature range.
Patent Information
- Application Number
- CN202310267657.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-20
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-03-20
AI Technical Summary
Existing shape memory alloys have limited service capabilities in extreme environments. They have a narrow superelastic temperature window and insufficient yield stress, making it difficult to combine a wide temperature range and high load-bearing capacity.
A wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on self-locking functional primitives is used. By combining NiTiCuZr alloy with NiTi alloy, hot extrusion technology is used to consolidate the honeycomb skeleton and amorphous powder to achieve metallurgical bonding of the two phases. Matching with the lattice strain, a self-locking unit is formed to improve the superelastic properties of the material.
It achieves good functional properties of the material under a wider temperature range and greater external force levels, expands the superelastic service temperature range, enhances the load-bearing capacity, and overcomes the limitations of plastic deformation at high temperatures and recovery capabilities at low temperatures of a single shape memory alloy. problem.
Smart Images

Figure CN116445796B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of shape memory alloys and composite materials, and specifically relates to a wide temperature range, high load-bearing 4D printing nickel-titanium-based alloy based on a self-locking functional element, and a preparation method and application thereof. Background Art
[0002] The superelasticity of shape memory alloys refers to the reversible martensitic phase transformation of the B2 austenite parent phase under the drive of the stress field, thereby showing large deformation and high recovery rate, which can be applied to medical devices, automotive industry, aerospace, construction and civil engineering and other fields. In order to meet the stringent service requirements in extreme environments, such as aviation or marine engineering, it is urgent to develop shape memory alloys with a wider service temperature window and higher load-bearing capacity. However, most shape memory alloys do not have this feature (Encyclopedia of Smart Materials 4 (2022) 239-253). Taking the most widely used NiTi shape memory alloy as an example, NiTi alloy has significant phase transformation strain, excellent deformation recovery rate and good functional stability, but its superelasticity is limited by both phase transformation temperature and yield stress (Int. J. Mater. Res. 70 (1979) 113-117), and its superelastic temperature window is about 50 ° C, which is around room temperature (Scripta Metal. 15 (1981) 287-292). In essence, only when the temperature is higher than A f (B2 austenite transformation end temperature), that is, in the temperature range where the B2 austenite phase is stable, superelasticity can achieve deformation recovery through spontaneous martensitic reverse phase transformation; when the temperature is between A f and A s (B2 austenite transformation starting temperature), superelastic recovery is incomplete; when the temperature is lower than A s When the superelasticity is completely lost, the superelasticity is completely lost. Therefore, lowering the phase transition temperature and increasing the stable range of the B2 austenite phase can expand the lower temperature limit of superelastic service. On the other hand, due to the critical stress σ of the stress-induced martensitic phase transformation of shape memory alloys SIM Following the Clausius-Clapeyron relationship, σ SIM It increases with the increase of temperature; when the service temperature increases to the point that causes σ SIMWhen the yield strength is higher than that of the B2 austenite phase, the material will undergo plastic deformation first, and dislocation slip will replace stress-induced martensitic transformation as the main deformation mechanism of the material, thereby introducing a large amount of irrecoverable deformation. Therefore, enhancing the yield strength of the B2 austenite phase is a way to increase the upper temperature limit of superelastic service. For a single shape memory alloy, although alloying, grain refinement, precipitation phase strengthening and other means can achieve a certain degree of superelasticity enhancement, the effect is limited, and it is difficult to have the above characteristics at the same time. For example, by cold rolling and aging treatment, the grain size of nickel-titanium alloy is reduced, and the matrix is strengthened by introducing nano-precipitation phase to obtain stable superelasticity, but its recovery stress is only 650MPa, and the service temperature window is about 40℃ (Scripta Mater.162(2019)230–234).
[0003] In order to break through the performance limitations of a single shape memory alloy and enrich the service scenarios of shape memory alloys, a composite strategy can be adopted to combine shape memory alloys with lower phase transition temperature and higher yield strength with nickel-titanium shape memory alloys with excellent superelasticity. However, how to combine the two, how to ensure good interface bonding quality, and how to coordinate the deformation of the two are problems that need to be solved. Summary of the invention
[0004] In order to overcome the shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on a self-locking functional element.
[0005] The second object of the present invention is to provide a method for preparing the above-mentioned wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on self-locking functional elements.
[0006] The third object of the present invention is to provide the application of the above-mentioned wide temperature range, high load-bearing 4D printing nickel-titanium-based alloy based on the self-locking functional element.
[0007] The primary purpose of the present invention is achieved through the following technical solutions:
[0008] A wide temperature range, high load-bearing 4D printing nickel-titanium-based alloy based on self-locking functional primitives, including the following features:
[0009] (1) Microstructural characteristics: The wide temperature range, high load-bearing nickel-titanium-based alloy based on the self-locking functional unit includes a regular hexagonal unit with a self-locking function. The regular hexagonal self-locking functional unit consists of a circular bolt in the center and a hexagonal nut on the periphery;
[0010] (2) Composition characteristics: The bolt phase region composition of the self-locking functional unit is a NiTiCuZr alloy with 35-40at.% Ni, 35-40at.% Ti, 10-15at.% Cu and 10-15at.% Zr, and the nut phase region composition is a NiTi alloy with 50-52at.% Ni and 48-50at.% Ti;
[0011] (3) Phase characteristics: The circular bolt of the self-locking functional unit is the low-temperature phase of NiTiCuZr shape memory alloy, and the hexagonal nut is the high-temperature phase of NiTi shape memory alloy. Both are in the B2 austenite phase at room temperature.
[0012] (4) Functional characteristics: The hardness and critical stress of phase transition of the bolt phase and nut phase of the self-locking functional element are different. During the loading process, the nut phase self-locks the bolt phase.
[0013] Preferably, the cross-sectional diameter of the bolt phase region of the self-locking functional element in the feature (1) is 200-750 μm, and it is composed of round rod-shaped grains with a grain diameter of 0.5-30 μm and an aspect ratio of 5-20; the cross-sectional hexagon height of the nut phase region is 400-950 μm, and it is composed of columnar crystals with a grain diameter of 10-100 μm and an aspect ratio of 10-30.
[0014] Preferably, the phase transition temperature of the bolt phase region of the self-locking functional element in the feature (3) is -160 to -120°C, and the phase transition temperature of the nut phase region is 10 to 40°C.
[0015] Preferably, the Vickers hardness of the self-locking functional element in the feature (4) in the bolt phase region is 450-650HV, and the Vickers hardness of the nut phase region is 150-300HV; the critical stress of phase transformation in the bolt phase region is 1000-1200MPa, and the critical stress of phase transformation in the nut phase region is 450-550MPa; the superelastic response temperature range of the nickel-titanium based alloy is -100-100°C, and the bearing stress is 1400-1600MPa.
[0016] The second object of the present invention is achieved by the following technical solutions:
[0017] A method for preparing a wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on a self-locking functional primitive comprises the following steps:
[0018] (1) Honeycomb skeleton 4D printing: NiTi alloy powder is printed into a honeycomb shape using a 4D printing system, residual stress is removed by annealing post-treatment, and surface bonding powder is removed by abrasive flow polishing to obtain a NiTi honeycomb skeleton;
[0019] (2) Preparation of extruded blank: placing the NiTi honeycomb skeleton obtained in step (1) in a copper sheath, filling the through holes of the honeycomb skeleton with NiTiCuZr amorphous alloy powder, sealing the sheath after compaction, and cold pressing to obtain an extruded blank;
[0020] (3) Hot extrusion molding: hot extrusion is performed on the extruded billet obtained in step (2) to consolidate the NiTiCuZr amorphous alloy powder to achieve metallurgical bonding of NiTiCuZr and NiTi alloy, followed by air cooling to obtain a wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on a self-locking functional unit.
[0021] Preferably, the process parameters of the 4D printing in step (1) are: laser power 180-250W, scanning rate 800-1400mm / s, scanning spacing 80-120μm, powder layer thickness 30-40μm; the annealing temperature of the annealing post-treatment is 900-1050°C, and the annealing time is 1-1.5h; the abrasive of the abrasive flow polishing treatment is silicon carbide, the pressure is 80-100kg, and the treatment time is 6-8h; the NiTi honeycomb skeleton is a cylindrical through hole containing hexagonal close-packed holes, any circular hole is closely surrounded by another 6 regular hexagonal circular holes, the pore diameter is 0.5-2mm, and the porosity is 25-75%.
[0022] Preferably, the NiTi alloy powder is prepared by an atomization method, and has a particle size of 15 to 53 μm; the NiTiCuZr amorphous alloy powder is prepared by an atomization method, and has a particle size of 15 to 38 μm.
[0023] Preferably, the extrusion temperature of the hot extrusion in step (3) is 850-980° C., the extrusion pressure is 600-1200 MPa, the extrusion speed is 2-6 mm / s, and the extrusion ratio is (4-8):1.
[0024] The third object of the present invention is achieved by the following technical solutions:
[0025] A wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on self-locking functional elements for use in medical devices, automotive industry, construction, civil engineering, and aerospace fields.
[0026] Preferably, the medical device products include cardiovascular stents, intestinal stents, spinal orthopedic rods, pressurized saddle staples, orthopedic spring environmentally friendly internal fixators; the automotive industry products include radiator mask valves, brake energy storage devices, and fan clutches; the construction and civil engineering products include elastic heat coolers, temperature control springs, elastic dampers, and shock absorbers; the aerospace products include tire radial reinforcements, space truss assembly structures, self-deployed satellite antennas, exhaust automatic regulating nozzles, flexible wings, and pipe joints.
[0027] The principle of the present invention is:
[0028] The present invention combines a NiTiCuZr alloy with a lower phase transition temperature, higher hardness, and stronger anti-slip ability with a NiTi alloy with a large phase transition strain and a high recovery rate, so that the material has both characteristics and exhibits good functional characteristics in a larger temperature range and under a larger external force level. The NiTi honeycomb skeleton and the NiTiCuZr powder are consolidated by hot extrusion technology. Under the action of thermal coupling, the density is greatly improved through large plastic deformation and element diffusion, and a good interface metallurgical bonding is obtained. During the hot extrusion process, the NiTiCuZr amorphous in-situ crystallizes into a B2-NiTiCuZr phase that can undergo stress-induced phase transition, while achieving the purpose of controlling the grain size.
[0029] The NiTi skeleton of the wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on self-locking functional elements prepared by the present invention is arranged in a honeycomb shape, has good structural stability, high stacking density, and outstanding compressive resistance, and can improve the load-bearing capacity of the nickel-titanium-based shape memory alloy; and the honeycomb structure is isotropic and uniformly stressed, which helps to disperse the stress along the honeycomb skeleton and ensure the coordinated deformation of multiple self-locking elements; the honeycomb holes are designed to be circular rather than regular hexagons, which can reduce stress concentration at the nodes and avoid damage to the honeycomb skeleton during hot extrusion.
[0030] When the wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on the self-locking functional unit prepared by the present invention is subjected to external force, the soft NiTi honeycomb skeleton outside the self-locking unit preferentially undergoes stress-induced phase transformation and buckles on both sides, uniformly transferring stress to the NiTiCuZr inside the self-locking unit, so that it further withstands external force and undergoes phase transformation at a higher stress level. Since the B2-NiTi and B2-NiTiCuZr two-phase lattice structures are the same, the lattice constants are close, and the two-phase interface has good lattice strain matching, even outside the NiTi superelastic temperature range or stress range, the lattice strain generated by the deformation recovery of NiTiCuZr will force the NiTi phase to recover synergistically, thereby showing good superelasticity.
[0031] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0032] (1) The method for preparing a wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on a self-locking functional unit of the present invention adopts laser selective melting technology to prepare a NiTi honeycomb skeleton, which can accurately control the pore size and porosity of the honeycomb skeleton, thereby improving the design freedom of the nickel-titanium-based shape memory alloy based on the self-locking unit; the NiTi skeleton and the NiTiCuZr powder are combined by a single hot extrusion process to ensure a firm interface, and the dislocation strengthening during the large plastic deformation process improves the strength of the material, thereby greatly enhancing the load-bearing capacity of the nickel-titanium-based shape memory alloy. The preparation method of the present invention provides a new idea for improving the superelastic properties of nickel-titanium-based shape memory alloys.
[0033] (2) The wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on the self-locking functional element prepared by the present invention has the characteristics of wide superelastic temperature range (low phase transition temperature) and high strength of NiTiCuZr alloy, as well as significant superelastic strain and high recovery rate of NiTi alloy; and the self-locking element is formed between NiTi and NiTiCuZr phases through interface metallurgical bonding and lattice strain matching. When loaded and deformed, the nut phase self-locks the bolt phase to constrain deformation, and has strong deformation recovery ability during unloading and recovery, which overcomes the service limitations of single NiTi shape memory alloy that is prone to plastic deformation at high temperature and cannot spontaneously reverse phase transformation recovery at low temperature, so that it has excellent macroscopic superelastic properties.
[0034] (3) The superelastic temperature window of a single NiTi alloy is about 15 to 50°C, and the maximum superelastic stress is usually less than 1000 MPa. The wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on the self-locking functional element prepared by the present invention can exhibit good superelasticity in the temperature range of -100 to 100°C, and the maximum superelastic stress can reach 1600 MPa, which is conducive to promoting the application of shape memory alloys under extreme conditions such as aviation and deep sea. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a microstructure diagram of the self-locking element of the wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on the self-locking functional element in Example 1.
[0036] Figure 2 This is an enlarged view of the microstructure of the NiTiCuZr alloy in the bolt phase region and the NiTi alloy in the nut phase region in the self-locking element of the wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on the self-locking functional element in Example 1.
[0037] Figure 3 This is the Vickers hardness indentation of the NiTiCuZr alloy in the bolt phase region and the NiTi alloy in the nut phase region in the self-locking element of the wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on the self-locking functional element in Example 1.
[0038] Figure 4This is the superelastic cyclic curve of the wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on the self-locking functional element in Example 1. DETAILED DESCRIPTION
[0039] The present invention is further described in detail below in conjunction with the embodiments and drawings, but the embodiments of the present invention are not limited thereto. The technical solutions of the present invention, unless otherwise specified, are all conventional techniques in the art.
[0040] Example 1
[0041] A wide temperature range, high load-bearing 4D printing nickel-titanium-based alloy based on self-locking functional primitives, including the following features:
[0042] (1) Microstructural characteristics: The wide temperature range, high load-bearing nickel-titanium-based alloy based on the self-locking functional unit includes a regular hexagonal unit with a self-locking function. The regular hexagonal self-locking functional unit consists of a central circular bolt and a peripheral hexagonal nut (such as Figure 1 The cross-sectional diameter of the bolt phase region of the self-locking functional unit is 500 μm, and it is composed of round rod-shaped grains with a grain diameter of 0.5 to 10 μm and an aspect ratio of 5 to 15; the cross-sectional hexagon of the nut phase region is 650 μm high, and it is composed of columnar crystals with a grain diameter of 10 to 50 μm and an aspect ratio of 10 to 15 (as shown). Figure 2 shown).
[0043] (2) Composition characteristics: The bolt phase region composition of the self-locking functional unit is a NiTiCuZr alloy with 35at.% Ni, 35at.% Ti, 15at.% Cu and 15at.% Zr, and the nut phase region composition is a NiTi alloy with 50at.% Ni and 50at.% Ti.
[0044] (3) Phase characteristics: The circular bolt of the self-locking functional unit is the low-temperature phase of NiTiCuZr shape memory alloy, and the hexagonal nut is the high-temperature phase of NiTi shape memory alloy. Both are B2 austenite phase at room temperature. The phase transition temperature of the bolt phase is -120°C, and the phase transition temperature of the nut phase is 40°C.
[0045] (4) Functional characteristics: The hardness and critical stress of phase transition of the bolt phase and nut phase of the self-locking functional unit are different. The nut phase self-locks the bolt phase during loading, and the 4D printed nickel-titanium-based alloy exhibits excellent superelasticity during recovery. The Vickers hardness of the bolt phase of the self-locking functional unit is 450-500 HV, and the Vickers hardness of the nut phase is 150-200 HV. Figure 3As shown in the figure, the hardness indentation of the bolt phase is small, while the hardness indentation of the nut phase is large; the critical stress of phase transformation in the bolt phase is 1200MPa, and the critical stress of phase transformation in the nut phase is 550MPa; the superelastic response temperature range of 4D printed nickel-titanium based alloy is -100~100℃, and the bearing stress is 1400MPa.
[0046] The above-mentioned method for preparing a wide temperature range, high-load 4D printed nickel-titanium-based alloy based on a self-locking functional primitive comprises the following steps:
[0047] (1) 4D printing of honeycomb skeleton: NiTi alloy powder with a particle size of 15 to 53 μm prepared by atomization method was printed into a honeycomb shape using a 4D printing system. The laser power of 4D printing was 180 W, the scanning rate was 800 mm / s, the scanning interval was 80 μm, and the powder layer thickness was 40 μm. The residual stress was removed by post-annealing at 900 °C for 1 h. The surface was polished by silicon carbide abrasive flow for 8 h at a pressure of 100 kg to remove the surface bonding powder, thereby obtaining a NiTi honeycomb skeleton. The NiTi honeycomb skeleton is a cylindrical through hole containing hexagonal dense stacks. Any circular hole is closely surrounded by another 6 regular hexagonal circular holes. The pore diameter is about 1 mm and the porosity is about 50%.
[0048] (2) Preparation of extruded blank: The NiTi honeycomb skeleton obtained in step (1) is placed in a copper sheath, and NiTiCuZr amorphous alloy powder with a particle size of 15 to 38 μm prepared by atomization is filled into the through holes of the honeycomb skeleton. After compaction, the sheath is sealed and cold-pressed to obtain an extruded blank.
[0049] (3) Hot extrusion molding: hot extrusion is performed on the extruded billet obtained in step (2) to consolidate the NiTiCuZr amorphous alloy powder and realize the metallurgical bonding of NiTiCuZr and NiTi alloy. The extrusion temperature of hot extrusion is 980°C, the extrusion pressure is 600 MPa, the extrusion speed is 2 mm / s, and the extrusion ratio is 6:1. Then air cooling is performed to obtain a wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on a self-locking functional element.
[0050] Superelastic behavior of wide temperature range, high load-bearing nickel-titanium-based shape memory alloy with self-locking primitives: Under compression, the maximum load-bearing stress is 1400MPa, the superelastic recovery strain is 5%, and after 10 cycles, the superelastic recovery strain is 4.56%. In the temperature range of -100℃ to 100℃, it can show about 5% superelasticity, such as Figure 4 As shown in the figure, ε max is the maximum loading strain, ε irreis the irrecoverable strain, and η is the recovery rate. Compared with relevant literature reports, such as the maximum bearing stress of 850MPa and superelastic recovery rate of 4% at room temperature (Acta mater.194 (2020) 178-189), the maximum bearing stress of 600MPa and superelastic recovery rate of 5.2% at room temperature (Sci.Rep.9 (2019) 41), the maximum bearing stress of 1000MPa and superelastic recovery rate of 5% at a temperature of 50°C (J.Alloy Compd.677 (2016) 204-210), its superelasticity has a wider service temperature range and higher bearing capacity. The biomedical device spinal correction rod made of the wide temperature range and high-load nickel-titanium-based shape memory alloy with self-locking elements in this embodiment can withstand a large pre-deformation before implantation and will not fail during the correction period.
[0051] Example 2
[0052] A wide temperature range, high load-bearing 4D printing nickel-titanium-based alloy based on self-locking functional primitives, including the following features:
[0053] (1) Microstructure characteristics: The wide temperature range, high load-bearing nickel-titanium-based alloy based on the self-locking functional unit includes a regular hexagonal unit with a self-locking function. The regular hexagonal self-locking functional unit consists of a circular bolt in the center and a hexagonal nut on the periphery. The cross-sectional diameter of the bolt phase area of the self-locking functional unit is 750μm, composed of round rod-shaped grains with a grain diameter of 10 to 30μm and an aspect ratio of 10 to 20; the cross-sectional hexagon of the nut phase area is 950μm high, composed of columnar crystals with a grain diameter of 30 to 100μm and an aspect ratio of 15 to 30.
[0054] (2) Composition characteristics: The bolt phase region composition of the self-locking functional unit is a NiTiCuZr alloy with 40at.% Ni, 40at.% Ti, 10at.% Cu and 10at.% Zr, and the nut phase region composition is a NiTi alloy with 52at.% Ni and 48at.% Ti.
[0055] (3) Phase characteristics: The circular bolt of the self-locking functional unit is the low-temperature phase of NiTiCuZr shape memory alloy, and the hexagonal nut is the high-temperature phase of NiTi shape memory alloy. Both are B2 austenite phase at room temperature. The phase transition temperature of the bolt phase is -160°C, and the phase transition temperature of the nut phase is 10°C.
[0056] (4) Functional characteristics: The hardness and critical stress of phase transformation of the bolt phase and nut phase of the self-locking functional unit are different. The nut phase self-locks the bolt phase during loading, and the 4D printed nickel-titanium alloy exhibits excellent superelasticity during recovery. The Vickers hardness of the bolt phase region of the self-locking functional unit is 500-650HV, and the Vickers hardness of the nut phase region is 200-300HV; the critical stress of phase transformation in the bolt phase region is 1150MPa, and the critical stress of phase transformation in the nut phase region is 550MPa; the superelastic response temperature range of the 4D printed nickel-titanium alloy is -100-100℃, and the bearing stress is 1600MPa.
[0057] The above-mentioned method for preparing a wide temperature range, high-load 4D printed nickel-titanium-based alloy based on a self-locking functional primitive comprises the following steps:
[0058] (1) 4D printing of honeycomb skeleton: NiTi alloy powder with a particle size of 15 to 53 μm prepared by atomization method was printed into a honeycomb shape using a 4D printing system. The laser power of 4D printing was 250 W, the scanning rate was 1400 mm / s, the scanning interval was 120 μm, and the powder layer thickness was 30 μm. The residual stress was removed by post-annealing at 1050°C for 1 h. The surface was polished by silicon carbide abrasive flow for 6 h at a pressure of 100 kg to remove the surface bonding powder, thereby obtaining a NiTi honeycomb skeleton. The NiTi honeycomb skeleton is a cylindrical through hole containing hexagonal dense stacks. Any circular hole is closely surrounded by another 6 regular hexagonal circular holes. The pore diameter is about 2 mm and the porosity is about 75%.
[0059] (2) Preparation of extruded blank: The NiTi honeycomb skeleton obtained in step (1) is placed in a copper sheath, and NiTiCuZr amorphous alloy powder with a particle size of 15 to 38 μm prepared by atomization is filled into the through holes of the honeycomb skeleton. After compaction, the sheath is sealed and cold-pressed to obtain an extruded blank.
[0060] (3) Hot extrusion molding: hot extrusion is performed on the extruded billet obtained in step (2) to consolidate the NiTiCuZr amorphous alloy powder and realize the metallurgical bonding of NiTiCuZr and NiTi alloy. The extrusion temperature of hot extrusion is 980°C, the extrusion pressure is 1200MPa, the extrusion speed is 6mm / s, and the extrusion ratio is 8:1. Then air cooling is performed to obtain a wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on a self-locking functional element.
[0061] Superelastic behavior of wide temperature range, high load-bearing nickel-titanium-based shape memory alloy with self-locking primitives: Under compression, the maximum bearing stress is 1400MPa, the superelastic recovery strain is 4.87%, and after 10 cycles, the superelastic recovery strain is 4%. In the temperature range of -100℃ to 100℃, it can show superelasticity of about 4.5%. Compared with relevant literature reports, such as the maximum bearing stress of 850MPa and superelastic recovery rate of 4% at room temperature (Acta mater.194(2020)178-189), the maximum bearing stress of 600MPa and superelastic recovery rate of 5.2% at room temperature (Sci.Rep.9(2019)41), the maximum bearing stress of 1000MPa and superelastic recovery rate of 5% at 50℃ (J.Alloy Compd.677(2016)204-210), its superelasticity has a wider service temperature range and higher load-bearing capacity. The shock absorber in the construction and civil engineering field made of the wide temperature range, high load-bearing nickel-titanium-based shape memory alloy with self-locking elements in this embodiment can withstand large impacts without being damaged, and can be used as a shock absorber for low-temperature deep-sea equipment.
[0062] Example 3
[0063] A wide temperature range, high load-bearing 4D printing nickel-titanium-based alloy based on self-locking functional primitives, including the following features:
[0064] (1) Microstructure characteristics: The wide temperature range, high load-bearing nickel-titanium-based alloy based on the self-locking functional unit includes a regular hexagonal unit with a self-locking function. The regular hexagonal self-locking functional unit consists of a circular bolt in the center and a hexagonal nut on the periphery. The cross-sectional diameter of the bolt phase area of the self-locking functional unit is 200μm, composed of round rod-shaped grains with a grain diameter of 10-15μm and an aspect ratio of 5-15; the cross-sectional hexagon of the nut phase area is 400μm high, composed of columnar crystals with a grain diameter of 50-100μm and an aspect ratio of 15-30.
[0065] (2) Composition characteristics: The bolt phase region composition of the self-locking functional unit is a NiTiCuZr alloy with 35at.%Ni, 35at.%Ti, 15at.%Cu and 15at.%Zr, and the nut phase region composition is a NiTi alloy with 51at.%Ni and 49at.%Ti.
[0066] (3) Phase characteristics: The circular bolt of the self-locking functional unit is the low-temperature phase of NiTiCuZr shape memory alloy, and the hexagonal nut is the high-temperature phase of NiTi shape memory alloy. Both are B2 austenite phase at room temperature. The phase transition temperature of the bolt phase is -150°C, and the phase transition temperature of the nut phase is 20°C.
[0067] (4) Functional characteristics: The hardness and critical stress of phase transformation of the bolt phase and nut phase of the self-locking functional element are different. The nut phase self-locks the bolt phase during loading, and the 4D printed nickel-titanium alloy exhibits excellent superelasticity during recovery. The Vickers hardness of the bolt phase region of the self-locking functional element is 450-500HV, and the Vickers hardness of the nut phase region is 150-200HV; the critical stress of phase transformation in the bolt phase region is 1000MPa, and the critical stress of phase transformation in the nut phase region is 450MPa; the superelastic response temperature range of the 4D printed nickel-titanium alloy is -100-100℃, and the bearing stress is 1500MPa.
[0068] The above-mentioned method for preparing a wide temperature range, high-load 4D printed nickel-titanium-based alloy based on a self-locking functional primitive comprises the following steps:
[0069] (1) 4D printing of honeycomb skeleton: NiTi alloy powder with a particle size of 15 to 53 μm prepared by atomization method was printed into a honeycomb shape using a 4D printing system. The laser power of 4D printing was 250 W, the scanning rate was 1250 mm / s, the scanning interval was 100 μm, and the powder layer thickness was 30 μm. The residual stress was removed by annealing post-treatment at 900 °C for 1.5 h. The surface was polished by silicon carbide abrasive flow for 6 h at a pressure of 100 kg to remove the surface bonding powder, thereby obtaining a NiTi honeycomb skeleton. The NiTi honeycomb skeleton is a cylindrical through hole containing hexagonal dense stacks. Any circular hole is closely surrounded by another 6 regular hexagonal circular holes. The pore diameter is about 0.5 mm and the porosity is about 25%.
[0070] (2) Preparation of extruded blank: The NiTi honeycomb skeleton obtained in step (1) is placed in a copper sheath, and NiTiCuZr amorphous alloy powder with a particle size of 15 to 38 μm prepared by atomization is filled into the through holes of the honeycomb skeleton. After compaction, the sheath is sealed and cold-pressed to obtain an extruded blank.
[0071] (3) Hot extrusion molding: hot extrusion is performed on the extruded billet obtained in step (2) to consolidate the NiTiCuZr amorphous alloy powder and realize the metallurgical bonding of NiTiCuZr and NiTi alloy. The extrusion temperature of hot extrusion is 850°C, the extrusion pressure is 1200MPa, the extrusion speed is 6mm / s, and the extrusion ratio is 4:1. Then air cooling is performed to obtain a wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on a self-locking functional element.
[0072] Superelastic behavior of wide temperature range, high load-bearing nickel-titanium-based shape memory alloy with self-locking primitives: Under compression, the maximum bearing stress is 1400MPa, the superelastic recovery strain is 5.8%, and after 10 cycles, the superelastic recovery strain is 4.7%. In the temperature range of -100℃ to 100℃, it can show about 5% superelasticity. Compared with relevant literature reports, such as the maximum bearing stress of 850MPa and superelastic recovery rate of 4% at room temperature (Acta mater.194(2020)178-189), the maximum bearing stress of 600MPa and superelastic recovery rate of 5.2% at room temperature (Sci.Rep.9(2019)41), the maximum bearing stress of 1000MPa and superelastic recovery rate of 5% at 50℃ (J.Alloy Compd.677(2016)204-210), its superelasticity has a wider service temperature range and higher load-bearing capacity. The radial reinforcement of aerospace tires made of the wide temperature range, high load-bearing nickel-titanium-based shape memory alloy with self-locking elements in this embodiment can increase the tire load-bearing capacity and avoid permanent damage to the tire when it is subjected to large deformation.
[0073] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a wide temperature range and high load-bearing 4D printed nickel-titanium-based alloy based on a self-locking functional unit, characterized in that: The following steps are involved: (1) Honeycomb skeleton 4D printing: NiTi alloy powder is printed into a honeycomb shape using a 4D printing system. The residual stress is removed by annealing post-treatment, and the surface bonding powder is removed by abrasive flow polishing to obtain a NiTi honeycomb skeleton. (2) Preparation of extruded blank: placing the NiTi honeycomb skeleton obtained in step (1) in a copper sheath, filling the through holes of the honeycomb skeleton with NiTiCuZr amorphous alloy powder, sealing the sheath after compaction, and cold pressing to obtain an extruded blank; (3) hot extrusion molding: hot extruding the extruded billet obtained in step (2) to consolidate the NiTiCuZr amorphous alloy powder to achieve metallurgical bonding of NiTiCuZr and NiTi alloy, followed by air cooling to obtain a wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on a self-locking functional element; The process parameters of the 4D printing in step (1) are: laser power 180-250 W, scanning rate 800-1400 mm / s, scanning spacing 80-120 μm, powder layer thickness 30-40 μm; the annealing temperature of the annealing post-treatment is 900-1050°C, and the annealing time is 1-1.5 h; the abrasive of the abrasive flow polishing treatment is silicon carbide, the pressure is 80-100 kg, and the treatment time is 6-8 h; the NiTi honeycomb skeleton is a cylindrical through hole containing hexagonal close-packed holes, any circular hole is closely surrounded by another 6 regular hexagonal circular holes, the pore diameter is 0.5-2 mm, and the porosity is 25-75%; The wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on the self-locking functional primitive includes the following features: (1) Microstructure characteristics: The wide temperature range, high load-bearing nickel-titanium-based alloy based on the self-locking functional unit includes a regular hexagonal unit with a self-locking function. The regular hexagonal self-locking functional unit consists of a circular bolt in the center and a hexagonal nut on the periphery; (2) Composition characteristics: The bolt phase region composition of the self-locking functional unit is a NiTiCuZr alloy with 35-40 at.% Ni, 35-40 at.% Ti, 10-15 at.% Cu and 10-15 at.% Zr, and the nut phase region composition is a NiTi alloy with 50-52 at.% Ni and 48-50 at.% Ti; (3) Phase characteristics: The circular bolt of the self-locking functional unit is the low-temperature phase of NiTiCuZr shape memory alloy, and the hexagonal nut is the high-temperature phase of NiTi shape memory alloy. Both are B2 austenite phase at room temperature; (4) Functional characteristics: The hardness and critical stress of phase transition of the bolt phase and nut phase of the self-locking functional element are different. During the loading process, the nut phase self-locks the bolt phase.
2. The method for preparing a wide temperature range and high load-bearing 4D printed nickel-titanium-based alloy based on a self-locking functional element according to claim 1, characterized in that: The cross-sectional diameter of the bolt phase region of the self-locking functional unit in the feature (1) is 200~750 μm, and it is composed of round rod-shaped grains with a grain diameter of 0.5~30 μm and an aspect ratio of 5~20; the cross-sectional hexagon height of the nut phase region is 400~950 μm, and it is composed of columnar crystals with a grain diameter of 10~100 μm and an aspect ratio of 10~30.
3. The method for preparing a wide temperature range and high load-bearing 4D printed nickel-titanium-based alloy based on a self-locking functional element according to claim 1, characterized in that: The phase transition temperature of the bolt phase region of the self-locking functional unit in the feature (3) is -160~-120°C, and the phase transition temperature of the nut phase region is 10~40°C.
4. The method for preparing a wide temperature range and high load-bearing 4D printed nickel-titanium-based alloy based on a self-locking functional element according to claim 1, characterized in that: The Vickers hardness of the self-locking functional element in the characteristic (4) is 450~650 HV in the bolt phase region, and 150~300 HV in the nut phase region; the critical stress of phase transformation in the bolt phase region is 1000~1200 MPa, and the critical stress of phase transformation in the nut phase region is 450~550 MPa; the superelastic response temperature range of the nickel-titanium based alloy is -100~100℃, and the bearing stress is 1400~1600 MPa.
5. The method for preparing a wide temperature range and high load-bearing 4D printed nickel-titanium-based alloy based on a self-locking functional element according to claim 1, characterized in that: The NiTi alloy powder is prepared by an atomization method, and has a particle size of 15 to 53 μm; the NiTiCuZr amorphous alloy powder is prepared by an atomization method, and has a particle size of 15 to 38 μm.
6. The method for preparing a wide temperature range and high load-bearing 4D printed nickel-titanium-based alloy based on a self-locking functional element according to claim 1, characterized in that: The extrusion temperature of the hot extrusion in step (3) is 850-980°C, the extrusion pressure is 600-1200 MPa, the extrusion speed is 2-6 mm / s, and the extrusion ratio is (4-8):
1.
7. Application of the wide temperature range, high load-bearing 4D printed nickel-titanium-based alloy based on self-locking functional elements prepared by the method according to any one of claims 1 to 4 in the fields of medical devices, automobile industry, construction and civil engineering, and aerospace.
8. The use of the wide temperature range, high load-bearing 4D printing nickel-titanium-based alloy based on the self-locking functional element according to claim 7, characterized in that: The medical device products include cardiovascular stents, intestinal stents, spinal orthotic rods, pressurized saddle staples, and orthopedic spring environmentally friendly internal fixators; the automotive industry products include radiator mask valves, brake energy storage devices, and fan clutches; the construction and civil engineering products include elastic heat coolers, temperature control springs, elastic dampers, and shock absorbers; the aerospace products include tire radial reinforcements, space truss assembly structures, self-deployed satellite antennas, exhaust automatic adjustment nozzles, flexible wings, and pipe joints.
Citation Information
Patent Citations
4D printing method of nickel-titanium-based ternary shape memory alloy
CN111842888A
Ultrahigh-superelasticity titanium-nickel shape memory alloy with functional element sequence structure and 4D printing preparation method and application of ultrahigh-elasticity titanium-nickel shape memory alloy
CN113199036A
Ultrahigh-superelasticity titanium-nickel shape memory alloy with sequentially structured functional unit, and 4d printing preparation method and application thereof
JP2022169459A
Erosion and wear resistant protective structures for turbine engine components
US20050207896A1
A method for the production of structured layers of titanium and nickel
WO2008000467A1