Efficient purification method for nanodiamonds

Through the salt-assisted air oxidation method, the problem of difficult removal of amorphous carbon nanoparticles on the surface of nanodiamond is solved, and efficient purification and circularization of nanodiamond is achieved, improving its optical and biomedical properties, reducing production costs and environment risk.

CN116457308BActive Publication Date: 2024-11-29VERSITECH LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202180074571.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-21
Publication Date
2024-11-29
Estimated Expiration
2041-10-21

AI Technical Summary

Technical Problem

The prior art is difficult to effectively remove amorphous carbon nanoparticles on the surface of nanodiamonds, resulting in poor performance of nanodiamonds in optical and biomedical applications, and common methods such as air oxidation and liquid phase treatment pose waste and environmental risks.

Method used

Using a salt-assisted air oxidation method, nanodiamonds are mixed with salt and heated at high temperatures, and separated by low-speed centrifugation to achieve one-step treatment to remove amorphous carbon nanoparticles and obtain clean and round nanodiamond particles.

Benefits of technology

The efficient purification of nanodiamond is achieved, removing amorphous carbon nanoparticles, improving the optical properties and biological interactions of nanodiamonds, reducing production costs and environmental risks, and no additional centrifugation steps are required, avoiding agglomeration problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116457308B_ABST
    Figure CN116457308B_ABST
Patent Text Reader

Abstract

Disclosed are methods for purifying nanodiamonds and methods for preparing substantially pure nanodiamonds, each method involving mixing nanodiamonds with at least one salt to form a mixture; heating the mixture at a temperature of 200°C to 1000°C for a time of 10 minutes to 10 hours; and combining a liquid with the heated mixture and centrifuging at a speed of 30 relative centrifugal force to 25,000 relative centrifugal force for a time of 10 seconds to 60 minutes to provide purified nanodiamonds. Pure nanodiamonds can be produced by a one-step treatment after air oxidation without any further centrifugation action. In addition, the developed salt-assisted air oxidation method is capable of easily manufacturing clean nanodiamonds on a large scale, the clean nanodiamonds having a rounded shape transformed from an original fragment-like shape, which is impossible to achieve using any existing purification method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for preparing and purifying nanodiamonds. Background Art

[0002] Nanoscale diamond particles (less than 1 μm in size), commonly referred to as nanodiamonds (NDs), have several outstanding material qualities that offer a wide range of potential for fundamental science and industrial applications. In particular, many optically addressable impurity defects, such as nitrogen-vacancy (NV) color centers present in the diamond lattice, have been exploited for next-generation quantum technologies due to their unique spin properties.

[0003] Currently, there are two main approaches for large-scale fabrication of NDs: “bottom-up” detonation of NDs and “top-down” grinding of bulk high-pressure, high-temperature (HPHT) diamonds. It is well known that unprocessed ND powders (i.e., detonation or HPHT) contain considerable amounts of unwanted impurities (e.g., ultrasmall (<10 nm) sized NDs, disordered carbon, metals, and metal oxides) that are naturally introduced during synthesis and processing. However, previous reports have demonstrated that non-diamonds present on the surface of NDs are detrimental to the properties of embedded quantum color centers (e.g., NV color centers). Therefore, the removal of these impurities becomes a critical step before the final application of NDs. For example, the fluorescence lifetime and spin coherence time (T2) of NV color centers in NDs can be significantly improved by removing surface quenchers (e.g., fluorescent graphitic carbon). This has been shown to be highly beneficial for potential applications in photonics, quantum sensing, and imaging. In addition, sufficiently clean and uniform surfaces of NDs, which are desired for favorable nanobio interactions, are prerequisites for potential biomedical applications in drug delivery, biolabeling, and biosensing.

[0004] Currently, the most commonly used method for removing non-diamond carbon includes surface oxidation of unprocessed NDs at 400-600°C for several hours in the presence of air. It has been shown that the oxygen-containing functional groups obtained on the ND surface can stabilize the NV charge state, increase the colloidal stability in aqueous solution, and extend the NV spin coherence time. However, the conventional air oxidation method is to calcine the ND powder alone in a furnace, and a considerable amount of impurities are associated with such a method. The impurities are mainly amorphous carbon nanoparticles with a size range of tens of nanometers, which are difficult to remove. Due to the calcination of crystalline NDs in air, the impurities are mainly amorphous carbon nanoparticles with a size range of tens of nanometers. Those nanoparticles cannot be removed by separation methods such as low-speed centrifugation (e.g., 1000 relative centrifugal force (rcf)), but can be gradually removed by multiple rounds of high-speed centrifugation (e.g., 10000rcf). The additional centrifugation step not only leads to more waste of ND samples, but also exacerbates the serious negative problem of ND agglomeration.

[0005] Alternatively, wet chemical treatments (e.g., HNO3 / H2SO4 / HClO4) have also been employed to remove both non-diamond carbon and metallic impurities in NDs. However, the use of these liquid phase approaches is expensive, and the use of hazardous chemicals poses environmental risks. Despite considerable effort to overcome these challenges, it remains difficult to obtain NDs with well-defined surfaces, especially when examined at the individual particle level.

[0006] Based on the established liquid etching method for bulk diamond, there have been studies on intensive etching of NDs with molten potassium nitrate (KNO3), i.e., heating at 500-600°C for several minutes. The results showed that this intensive etching treatment was able to produce NDs with cleaner surfaces and more rounded morphology than NDs treated with gas oxidation methods. The rounded NDs also exhibited improved optical properties and excellent colloidal stability. However, the molten salt method involves complex procedures and requires specialized protective equipment, and these disadvantages have so far prevented its widespread adoption.

[0007] Therefore, a more convenient method is needed that can produce clean NDs on a large scale.

[0008] Disclosure of the Invention

[0009] The object of the present invention is to provide a highly efficient purification method for ND.

[0010] A simplified overview of the present invention is presented below to provide a basic understanding of some aspects of the present invention. This overview is not an extensive review of the present invention. It is neither intended to identify the key or important elements of the present invention nor to describe the scope of the present invention. On the contrary, the sole purpose of this overview is to present some concepts of the present invention in a simplified form as a preface to the more detailed description presented below.

[0011] As described herein, an efficient purification method for NDs (less than 1 μm in size) by salt-assisted air oxidation (SAAO) is explained. Using the method described herein, pure NDs (without any detectable amorphous carbon nanoparticles) can be produced by a one-step treatment (e.g., centrifugation at 1000 rcf for 5 minutes) after air oxidation without the need for any further centrifugation action. In addition, the developed SAAO method enables easy large-scale production of clean NDs having a rounded shape transformed from the original fragment-like shape, which is impossible to achieve using any existing purification method.

[0012] Disclosed herein is a method for purifying NDs, comprising mixing NDs with at least one salt to form a mixture; heating the mixture at a temperature of 200°C to 1000°C for a time of 10 minutes to 10 hours; and combining a liquid with the heated mixture and centrifuging at a speed of 30 rcf to 25000 rcf for a time of 10 seconds to 60 minutes to provide purified NDs.

[0013] Also disclosed is a method for preparing substantially pure ND, comprising mixing ND with at least one salt to form a mixture; heating the mixture at a temperature of 200° C. to 1000° C. for a time of 10 minutes to 10 hours; and combining a liquid with the heated mixture and centrifuging at a speed of 30 rcf to 25000 rcf for a time of 10 seconds to 60 minutes to provide substantially pure ND having less than 0.01% impurities by weight.

[0014] Purification of NDs is a major step in realizing most of their quantum applications. For example, surface oxidation (i.e., aerobic or anaerobic triacid oxidation) methods have been commonly used to remove surface-covered non-diamond structures (e.g., sp 2 Carbon, sp 2 Clusters). The conventional method for this is air oxidation treatment of ND at 400-600°C (calcining ND powder separately in a furnace). However, there are considerable amounts of impurities associated with such a method. Due to the calcination of crystalline ND in air, the impurities are mainly amorphous carbon nanoparticles with a size range of tens of nanometers. Those nanoparticles cannot be removed by separation methods such as low-speed centrifugation (e.g., 1000rcf), and may be gradually removed by multiple rounds of high-speed centrifugation (e.g., 10000rcf). The additional centrifugation step not only leads to more waste of ND samples, but also exacerbates the serious negative problem of ND agglomeration. As described herein, an efficient purification method for ND by SAAO is explained. With the new system and method described herein, pure ND (without any (or almost any) detectable amorphous carbon nanoparticles) can be produced by a one-step treatment (centrifugation at 1000rcf for 5 minutes) after air oxidation without any further centrifugation step.

[0015] The following description and accompanying drawings set forth certain illustrative aspects and implementations of the present invention in detail. However, these merely show some of the various ways in which the principles of the present invention may be employed. When considered in conjunction with the accompanying drawings, other objects, advantages and novel features of the present invention will become apparent from the following detailed description of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to explain the embodiments of the present invention or the technical solutions in the prior art more clearly, the drawings required for describing the embodiments of the present invention will be briefly described below. Obviously, the drawings in the following description are only some embodiments of the present invention.

[0018] Figure 1 Depicting (a) Schematic diagram of the conventional air oxidation process. (b) Scanning electron microscope (SEM) image of conventional air oxidized (500°C, 5 hours) NDs and (c) Transmission electron microscope (TEM) image of conventional air oxidized (500°C, 5 hours) NDs. In the TEM image, small-sized nanoparticles on the ND surface are indicated by black arrows. (d) Schematic diagram of the SAAO process. (e) SEM image of SAAO (500°C, 5 hours) NDs and (f) TEM image of SAAO (500°C, 5 hours) NDs. (g) Dynamic light scattering (DLS) size distribution of raw, conventional air oxidized, and SAAO NDs.

[0019] Figure 2 Depicted are (a) SEM image of unprocessed ND and (b) TEM image of unprocessed ND. (c) TEM image of impurities observed in unprocessed ND. (d) SEM image of conventionally oxidized ND after three thorough washings (11000 rcf, 10 min) and (e) TEM image of conventionally oxidized ND after three thorough washings (11000 rcf, 10 min). (f) DLS size distribution of as-prepared and finely washed air-oxidized ND. (g) SEM image of commercial ND that has been tri-acid treated before shipment and (h) TEM image of commercial ND that has been tri-acid treated before shipment. (i) TEM image of conventionally air-oxidized (500°C, 5 h) ND after incubation in deionized water for 50 days.

[0020] Figure 3 Depicted are the circularity distributions of (a) unprocessed NDs and (b) SAAO NDs. The circularity was obtained by randomly selecting 200 particles from the TEM images of each sample and then analyzed using ImageJ software. The circularity was defined as 4Aπ / (P 2 ), where A is its area, and P is its perimeter. A value of 1.0 shows a perfect circle. As the value approaches 0.0, it shows an increasingly elongated shape. The results show that SAAO ND is more round than unprocessed ND.

[0021] Figure 4 Depicted are (ad) TEM-AFM (atomic force microscopy) related characterizations of SAAO NDs and (eh) TEM-AFM (atomic force microscopy) related characterizations of unprocessed NDs.

[0022] Figure 5 Depicted are (a) X-ray powder diffraction (XRD) of raw, conventional air oxidized, and SAAO NDs, (b) Fourier transform infrared spectroscopy (FTIR) of raw, conventional air oxidized, and SAAO NDs, and (c) high resolution X-ray photoelectron spectroscopy (XPS) carbon 1s spectra of raw, conventional air oxidized, and SAAO NDs.

[0023] Figure 6 Depicting the sources of newly generated impurities observed during oxidation. (a) Schematic diagram of the impurity collection process in conventional air-oxidized NDs. (b) SEM image of the contents in the upper solution. (c) TEM image of non-diamond particles. The inset of (c) is the selected area electron diffraction (SAED) pattern of the same cluster. (d) Schematic diagram of the air oxidation study process of a single ND. Pre-cleaned NDs were first deposited onto a Si3N4 membrane-supported TEM grid, and one selected ND was observed and located by TEM (step 1). The sample was then air-oxidized at 500°C for 5 times (steps 2, 3, 4, and 5: 1 hour; step 6: 2 hours), and observed again under TEM after each time. TEM images of the selected NDs after steps 1 and 6 are shown in (e) and (f), respectively.

[0024] Figure 7 Depicted are (a) an SEM image and an energy dispersive X-ray spectroscopy (EDX) spectrum of the upper solution content of an unprocessed ND suspension, (b) an SEM image and an EDX spectrum of the upper solution content of a 2-hour conventional air-oxidized ND suspension, and (c) an SEM image and an EDX spectrum of the upper solution content of a 5-hour conventional air-oxidized ND suspension.

[0025] Figure 8 Depicting TEM images of (a) the upper solution contents of unprocessed ND suspension and (b) the upper solution contents of conventional 5-hour air-oxidized ND suspension. Small-sized impurities found in (c) the upper solution of conventional 5-hour air-oxidized ND on conventional carbon film-coated TEM grid and (d) the upper solution of conventional 5-hour air-oxidized ND on Si3N4 film-coated TEM grid.

[0026] Fig. 9Depicting the mechanism of the SAAO process: (a) SEM image of a mixture of ND and NaCl (ND+NaCl) after oxidation without any further cleaning process; (b) schematic diagram of the “salt-assisted etching atmosphere” generated during high-temperature air oxidation; (c) thermogravimetric analysis and differential scanning calorimetry (TGA-DSC) curves of ND+NaCl, (d) TGA-DSC curve of ND, and (e) TGA-DSC curve of NaCl, all of which were recorded under the same conditions, i.e., heating from room temperature (RT) to 500°C at a heating rate of 5°C / min and holding at 500°C for 5 h.

[0027] Fig.10 Schematic diagram depicting (a) NDs on Si wafer for oxidation, which simulates NDs on salt surface, (b) SEM image of NDs on Si wafer before air oxidation at 500°C for 5 hours and (c) SEM image of NDs on Si wafer after air oxidation at 500°C for 5 hours.

[0028] Fig.11 Depicting the comparison of the cleaning process of salt-assisted and conventional air oxidation methods (500°C, 2 hours). (a) Photographs showing the detailed process of salt-assisted and conventional air oxidation of NDs. (b) SEM characterization of the supernatant after centrifugation of salt-assisted air-oxidized ND aqueous solution and (c) SEM characterization of the supernatant after centrifugation of conventional air-oxidized ND aqueous solution. In (c), 200 nm NDs are indicated by circles. (d) DLS measurement of the particle size distribution of the precipitate and supernatant of the oxidized ND aqueous solution after centrifugation (1000 rcf, 5 minutes). The particle concentration of the supernatant of the SAAO ND solution was too low to be detected in the DLS measurement.

[0029] Fig.12 Depicted are SEM images of conventional air-oxidized NDs and SAAO NDs (with indicated yields) with different oxidation temperatures and times.

[0030] Fig.13 Depicting potassium chloride (KCl)-assisted air oxidation of 50 nm NDs: (a) TEM image of unprocessed NDs and (b) TEM image of NDs after 2 hours of KCl-assisted air oxidation.

[0031] Best Mode for Carrying Out the Invention

[0032] Generally, the method for purifying ND according to the present invention comprises the following steps:

[0033] mixing NDs (less than 1 μm in size) with at least one salt to form a mixture;

[0034] heating the mixture at a temperature of 200°C to 1000°C for a period of 10 minutes to 10 hours; and

[0035] The liquid is combined with the heated mixture and centrifuged at a speed of 30 rcf to 25,000 rcf for a time of 10 seconds to 60 minutes to provide purified NDs.

[0036] ND is first mixed with an appropriate amount of salt before heating. In one embodiment, ND is mixed with 0.1 to 100 times the amount of salt per unit weight. In another embodiment, ND is mixed with 0.5 to 50 times the amount of salt per unit weight. In yet another embodiment, ND is mixed with 1 to 10 times the amount of salt per unit weight.

[0037] Salt is any salt that promotes the surface oxidation of ND. Salt is an ionic compound with anions and cations. General examples of salts that can be used include alkaline earth metal halogens, alkaline earth metal sulfates, alkaline earth metal persulfates, alkaline earth metal nitrates, alkaline earth metal phosphates, etc.; alkali metal halogens, alkali metal sulfates, alkali metal persulfates, alkali metal nitrates, alkali metal phosphates, etc.; transition metal halogens, transition metal sulfates, transition metal persulfates, transition metal nitrates, transition metal phosphates, etc.; ammonium halogens, ammonium sulfates, ammonium persulfates, ammonium nitrates, ammonium phosphates, etc.; alkyl quaternary ammonium halogens, alkyl quaternary ammonium sulfates, alkyl quaternary ammonium persulfates, alkyl quaternary ammonium nitrates, alkyl quaternary ammonium phosphates, etc. One or more. Specific examples of salts that can be used include sodium chloride, magnesium chloride, potassium chloride, calcium chloride, ammonium chloride, sodium sulfate, magnesium sulfate, potassium sulfate, calcium sulfate, ammonium sulfate, etc. One or more.

[0038] The ND / salt mixture is then heated at a suitable temperature for a suitable period of time to promote surface oxidation of the NDs. In one embodiment, the ND / salt mixture is heated at a temperature of 200° C. to 1000° C. for a time of 10 minutes to 10 hours. In another embodiment, the ND / salt mixture is heated at a temperature of 300° C. to 800° C. for a time of 30 minutes to 8 hours. In yet another embodiment, the ND / salt mixture is heated at a temperature of 400° C. to 600° C. for a time of 1 hour to 5 hours.

[0039] The mixture of oxidation is then added to the liquid, and subjected to mechanical separation, such as centrifugal suitable time period at the lowest possible speed. The example of liquid includes water, deionized water or organic liquid such as alcohol. Mechanical separation separates salt from ND, realizes the collection of the ND of purification. Adopt low speed so that the damage to ND is minimized / reduced and / or the agglomeration of ND is minimized / reduced. In one embodiment, the mixture of oxidation is centrifuged for 10 seconds to 60 minutes with the speed of 30rcf to 25000rcf. In another embodiment, the mixture of oxidation is centrifuged for 30 seconds to 30 minutes with the speed of 100rcf to 10000rcf. In another embodiment, the mixture of oxidation is centrifuged for 1 minute to 15 minutes with the speed of 500rcf to 5000rcf.

[0040] Purified NDs are collected. The NDs are characterized by the presence of very little to no detectable impurities and / or a relatively narrow size distribution of the purified NDs, especially compared to a similar oxidation-centrifugation process when no salt is used. The NDs are substantially pure; meaning that the collected NDs are at least 99.9% by weight NDs, with less than 0.1% by weight impurities, such as amorphous carbon nanoparticles. In another embodiment, the collected NDs are at least 99.95% by weight NDs, with less than 0.05% by weight impurities, such as amorphous carbon nanoparticles. In yet another embodiment, the collected NDs are at least 99.99% by weight NDs, with less than 0.01% by weight impurities, such as amorphous carbon nanoparticles.

[0041] According to the method of the present invention, the purified NDs are not agglomerated.

[0042] In another aspect, the present invention provides a method for preparing substantially pure NDs, comprising the steps of:

[0043] mixing raw NDs (less than 1 μm in size) with at least one salt to form a mixture;

[0044] heating the mixture at a temperature of 200°C to 1000°C for a period of 10 minutes to 10 hours; and

[0045] The liquid is combined with the heated mixture and centrifuged at a speed of 30 rcf to 25,000 rcf for a time of 10 seconds to 60 minutes to provide substantially pure NDs having less than 0.01% impurities by weight.

[0046] In the method of preparing substantially pure ND according to the present invention, wherein the raw ND contains impurities including ultra-small (<10 nm) sized ND, amorphous carbon nanoparticles, metals and metal oxides.

[0047] ND is first mixed with an appropriate amount of salt before heating. In one embodiment, ND is mixed with 0.5 to 50 times the amount of salt per unit weight. In another embodiment, ND is mixed with 1 to 10 times the amount of salt per unit weight.

[0048] Salt is any salt that promotes the surface oxidation of ND. Salt is an ionic compound with anions and cations. General examples of salts that can be used include alkaline earth metal halogens, alkaline earth metal sulfates, alkaline earth metal persulfates, alkaline earth metal nitrates, alkaline earth metal phosphates, etc.; alkali metal halogens, alkali metal sulfates, alkali metal persulfates, alkali metal nitrates, alkali metal phosphates, etc.; transition metal halogens, transition metal sulfates, transition metal persulfates, transition metal nitrates, transition metal phosphates, etc.; ammonium halogens, ammonium sulfates, ammonium persulfates, ammonium nitrates, ammonium phosphates, etc.; alkyl quaternary ammonium halogens, alkyl quaternary ammonium sulfates, alkyl quaternary ammonium persulfates, alkyl quaternary ammonium nitrates, alkyl quaternary ammonium phosphates, etc. One or more. Specific examples of salts that can be used include sodium chloride, magnesium chloride, potassium chloride, calcium chloride, ammonium chloride, sodium sulfate, magnesium sulfate, potassium sulfate, calcium sulfate, ammonium sulfate, etc. One or more.

[0049] The ND / salt mixture is then heated at a suitable temperature for a suitable period of time to promote surface oxidation of the NDs. In one embodiment, the ND / salt mixture is heated at a temperature of 300° C. to 800° C. for a time of 30 minutes to 8 hours. In another embodiment, the ND / salt mixture is heated at a temperature of 400° C. to 600° C. for a time of 1 hour to 5 hours.

[0050] The mixture of oxidation is then added to the liquid, and subjected to mechanical separation, such as centrifugal suitable time period at the lowest possible speed. The example of liquid includes water, deionized water or organic liquid such as alcohol. Mechanical separation separates salt from ND, realizes the collection of purified ND. Adopt low speed so that the damage to ND is minimized / reduced and / or the agglomeration of ND is minimized / reduced. In one embodiment, the mixture of oxidation is centrifuged for 30 seconds to 30 minutes with a speed of 100rcf to 10000rcf. In another embodiment, the mixture of oxidation is centrifuged for 1 minute to 15 minutes with a speed of 500rcf to 5000rcf.

[0051] The liquid is selected from water, deionized water, organic liquids such as methanol, ethanol, and combinations thereof.

[0052] The resulting substantially pure NDs are collected. The NDs are characterized by the presence of very little to no detectable impurities and / or a relatively narrow size distribution of the purified NDs, especially compared to a similar oxidation-centrifugation process when no salt is used. The NDs are substantially pure, meaning that the collected NDs are at least 99.9% by weight NDs, with less than 0.1% by weight impurities, such as amorphous carbon nanoparticles. In another embodiment, the collected NDs are at least 99.95% by weight NDs, with less than 0.05% by weight impurities, such as amorphous carbon nanoparticles. In yet another embodiment, the collected NDs are at least 99.99% by weight NDs, with less than 0.01% by weight impurities, such as amorphous carbon nanoparticles.

[0053] Desirably, substantially pure NDs prepared by the methods according to the present invention are not agglomerated.

[0054] The present invention will be further described with reference to the following detailed examples. It is necessary to point out that the following examples are only for illustration and are not intended to limit the present invention. Various changes made by those skilled in the art based on the teachings of the present invention should all be within the scope of the claims of the present invention.

[0055] Example 1

[0056] Salt Assisted Air Oxidation Method (SAAO Method)

[0057] ND (HPHT, PolyQolor, China) with an average particle size of 200 nm was used as the starting material.

[0058] (1) 0.5 g of ND was mixed with 2.5 g of sodium chloride (NaCl, 99.5%, Sigma-Aldrich), and they were heated at 500° C. for 5 hours in air.

[0059] (2) 600 mg of the obtained sample was dispersed in 1 mL of deionized water and sonicated for 1 hour, and then the ND was purified by centrifugation with deionized water three times (first time: 1000 rcf, 5 minutes; second time: 3000 rcf, 5 minutes; third time: 8000 rcf, 10 minutes).

[0060] (3) The purified NDs were redispersed in deionized water and sonicated for 10 min to obtain a well-dispersed ND suspension for further characterization.

[0061] Comparative Example 1

[0062] For comparison, conventional air oxidation of ND was carried out in parallel to Example 1, ie without addition of NaCl to the starting material.

[0063] (1) 0.5 g of ND was heated at 500°C for 5 hours in air.

[0064] (2) 100 mg of the obtained sample was dispersed in 1 mL of deionized water and sonicated for 1 hour, and then the ND was purified by centrifugation 3 times with deionized water (11000 rcf, 10 minutes).

[0065] (3) The purified NDs were redispersed in 1 mL of deionized water and sonicated for 10 min to obtain a well-dispersed ND suspension for further characterization.

[0066] Characterization

[0067] Comparison of ND of Example 1 and Comparative Example 1

[0068] (I) Unremoved impurities associated with conventional air oxidation

[0069] In order to evaluate the performance of the conventional air oxidation method ( Figure 1 (a)), the raw ND powder was directly heated alone in air at 500 °C in a furnace for 5 h. The obtained sample was dispersed in deionized (DI) water for further characterization. As shown in the electron microscopy image ( Figure 1 (b), (c)), it is usually found that conventional air-oxidized NDs are covered with a large number of small-sized (<50 nm) nanoparticles ( Figure 1 In fact, the observed phenomenon is almost the same as that in the untreated sample ( Figure 2 (a), (b)). These observations confirm that it is not possible to obtain NDs with well-defined surfaces using conventional air oxidation treatment. Next, 3 rounds of washing procedures (using high-speed centrifugation, 11000 rcf, 10 minutes) were attempted to remove these unwanted impurities, but there was little improvement after the cleaning treatment ( Figure 2 Even the harsh triple-acid washing process did not help, as evidenced by the small size of nanoparticles commonly observed in association with commercial NDs known to have been triple-acid washed ( Figure 2 (g), (h)). Due to their ultra-small size and high surface energy, these small-sized nanoparticles show high binding affinity to the ND surface. This strong binding affinity may be attributed to their ionic interactions, van der Waals interactions, and hydrogen bonding, which is similar to the strong affinity reported for oxygen-terminated NDs to various proteins. Therefore, these small-sized nanoparticles (impurities) are difficult to remove using common separation methods ( Figure 2 (dh)).

[0070] Surprisingly, as shown by the significantly broadened DLS spectrum of the ND powder obtained directly dispersed in deionized water ( Figure 1 (g)), there appear to be some newly generated fractions (<50 nm) after conventional air oxidation treatment. One hypothesis for these observed impurities is the formation of ultra-small sized NDs through the milling process, which is a necessary step in the HPHT ND production. These fractions can also be attributed to the desorption of ultra-small sized NDs from “larger” NDs after oxidation, as their interactions may have been weakened by the high temperature treatment. Therefore, when the oxidized NDs are dispersed in water for DLS measurements, some of the desorbed nanoparticles may fall off, inducing a broadened DLS spectrum and a decrease in the measured average size (from ∼200 nm to ∼120 nm). Another possibility could be that these impurities are newly emerged materials rather than NDs. A detailed study of the observed newly generated impurities will be discussed in section (IV). The presence of unremoved impurities significantly limits the potential usefulness of NDs, affecting their morphology, binding capacity, and optical properties (e.g., charge state, fluorescence lifetime). In addition, the uncertainty of non-specific interactions between those impurities and NDs means that the host particles have a surface ( Figure 2 (i)), which inhibits their use in many potential applications.

[0071] (II) Clean and round NDs obtained by SAAO method

[0072] The inability to remove impurities adsorbed on the ND surface is partly due to the close packing of ND powders and partly due to defects in the oxidation process (e.g., incomplete oxidation or spontaneous oxidation). To overcome this, the so-called SAAO method was proposed, in which NDs are mixed with salt crystals (i.e., NaCl or KCl) before heat treatment. In a typical experiment, e.g. Figure 1 (d) depicts that the untreated ND powder was thoroughly mixed with NaCl crystals at a mass ratio of 1:5, and the mixture was then subjected to conventional treatment (heating in an oven at 500 °C for 5 h in air). Representative SEM images of the obtained NDs after SAAO treatment ( Figure 1 (e)) and bright field TEM ( Figure 1 (f)) The image clearly shows the uniform distribution of the resulting NDs, which contain sharp boundaries and clean surfaces, which are rarely, if ever, found in conventionally oxidized NDs ( Figure 1 (c)). DLS results ( Figure 1 (g)) also shows that the size distribution of NDs has shifted by tens of nanometers, involving a significant reduction in the average size of the resulting NDs (from ˜200 nm to ˜170 nm), and this observation is consistent with the results of the electron microscopy images. Notably, the NDs also lose their original fragment-like shape and become rounded ( Figure 3Quantitative results are shown).

[0073] To further evaluate the performance of this new method, the detailed morphological features of individual NDs were carefully characterized using TEM-AFM correlative microscopy ( Figure 4 ). Randomly selected SAAO-treated or unprocessed NDs were first observed and positioned by TEM and then measured by AFM. Figure 4 (c) shows that the randomly picked line profiles indicate the smooth surface of the selected particles processed by our SAAO method, and this is consistent with the reconstructed three-dimensional (3D) AFM image ( Figure 4 By comparison, the unprocessed ND particles show a rough surface associated with the inevitably adsorbed small-sized nanoparticles, as shown by the line profile ( Figure 4 (g)) and reconstructed 3D AFM image ( Figure 4 (h)). The significance of this breakthrough is considerable, namely, solid non-oxidizing alkali chlorides (such as NaCl and KCl) are used for ND oxidation, unlike the use of highly oxidizing molten nitrates (KNO3), but the same shape evolution (rounding effect), smoother and cleaner surface of NDs are achieved. The improved optical properties, reduced surface spin noise, improved surface roughness, reduced inter-particle friction and reduced anisotropy present in SAAO NDs enable their use in a wide range of different applications, including photonics, quantum sensing and imaging.

[0074] (III) Crystallinity and surface chemistry characterization of NDs

[0075] XRD results ( Figure 5 (a) shows the pure crystalline nature of all samples, that is, only the characteristic peaks of diamond are found in the XRD spectra. The peaks at 43.9°, 75.2° and 91.5° correspond to the (111), (220) and (311) planes of the cubic diamond lattice, respectively.

[0076] Figure 5 (b) depicts the FTIR spectra of raw, conventional air-oxidized, and SAAO NDs. -1 The strong peak observed in the range of 1310 cm-1 is attributed to CO stretching vibration. The peak at 1310 cm-1, which appears very weakly in raw ND and significantly in air-oxidized ND (both salt-assisted and conventional), appears due to air oxidation treatment. -1 The peak at 1630 cm is attributed to CO bending vibration. -1 The peak at 3500 cm is due to the -OH bending vibration, which comes from the carboxyl groups (-COOH) on the ND surface or water molecules adsorbed on the sample surface.-1 The broad peaks nearby are similar. And at ∼1770 cm -1 The peak at is attributed to the stretching mode of C=O, indicating the presence of carboxyl groups on the surface.

[0077] Figure 5 (c) High-resolution XPS carbon 1s spectrum of the sample. The main peak observed at ~285.3 eV is attributed to the diamond sp 3 Carbon. The two satellite peaks at ~286.6 eV and ~287.6 eV correspond to CO and C=O, respectively. The peak at ~284 eV is attributed to sp 2 Therefore, the surface chemistry of SAAO NDs is the same as that of conventional air-oxidized NDs.

[0078] (IV) Newly generated "impurities" during conventional oxidation

[0079] As shown in the above results ( Figure 1 (g)), a significant fraction of nanoparticles (<50 nm) was found in the NDs shortly after conventional air oxidation. In contrast, this was not the case at all in our SAAO samples. In order to determine the origin of those newly generated "impurities", they were carefully separated from the main part of the sample ("larger" NDs with a size of ∼200 nm) by leaving them in deionized water for 7 days (see Figure 6 Next, we observed a large number of small-sized nanoparticles in the supernatant, which were different from the “larger” NDs ( Figure 6 (b)) have different sizes and morphologies. In addition, as shown in the TEM diffraction pattern (see Figure 6 The inset in (c) confirms that most of these small-sized nanoparticles are amorphous materials. And the corresponding elemental analysis ( Figure 7 EDX spectra in ( ) showed that the observed small-sized nanoparticles were mainly composed of carbon. By comparison, only NDs (a few nm to ∼200 nm) were observed in the supernatant of an aqueous dispersion of unprocessed NDs after similar separation ( Figure 8 (a)), indicating that non-diamond impurities (amorphous carbon nanoparticles) should be produced during conventional air oxidation.

[0080] On the other hand, time-dependent oxidation studies of pre-cleaned single NDs (selected randomly) were performed directly on TEM grids ( Figure 6 (d)). In order to exclude the possible influence of non-diamond impurities occasionally found in the uncleaned raw ND ( Figure 2 (c)), using pre-cleaned NDs (with a high level of cleanliness) as the starting material. Figure 6(e) (TEM image of a typical ND before time-dependent oxidation study) shows that nothing was found on or near the surface of the selected particle. Gradually, after several rounds of oxidation, some ultra-small dots (~2 nm) appeared near or on the ND (by Figure 6 Several rounds of oxidation were designed to accumulate the amount of impurities produced (indicated by circles and arrows in (f)). As a result, the observed dots (judged by their morphology and TEM comparison) can be attributed to amorphous carbon nanoparticles produced during the oxidation process.

[0081] (V) Mechanism of SAAO method

[0082] To investigate the underlying mechanism of the developed SAAO method, a mixture of NDs and NaCl (after oxidation) was first examined to see whether the cleanliness of NDs on salt particles was altered directly without any further cleaning treatment (e.g., washing and centrifugation). Fig. 9 As shown in (a), it has been found that the ND adsorbed on the surface of the salt particles (with a size in the hundreds of micrometers) is clean without any obvious adsorbed small-sized nanoparticles. In addition, the morphology of the ND on the salt surface (thin "lamellar" film) is completely different from the ND morphology involved in the conventional oxidation method (highly agglomerated powder form). Therefore, considering the difference in ND morphology during oxidation, it is first assumed that the salt particles may have acted as thermal management agents in particles such as spacers, resulting in more uniform and rapid etching of ND.

[0083] To verify this, an air oxidation experiment was performed ( Fig.10 ), in which NDs were coated on a non-salt substrate (i.e., Si wafer) that simulated a salt surface. Unfortunately, nothing happened to the NDs on the Si wafer after air oxidation at 500°C for 5 h. This suggests that the formation of a "lamellar" ND film cannot be the actual mechanism of the SAAO process.

[0084] The above results indicate that NaCl may also participate in the oxidation process of NDs, rather than just acting as a spacer. Inspired by the well-known fact that chloride salts (such as NaCl and KCl) can extensively corrode metals or alloys at temperatures of 400-700°C due to the highly corrosive gases they produce, the “etching atmosphere” ( Fig. 9 (b)) will also significantly improve the etching rate of NDs (e.g. etching away adsorbed small-sized nanoparticles and making NDs round). To verify this hypothesis, TGA-DSC measurements were performed ( Fig. 9(ce)), which is used as a gold standard for examining potential chemical reactions between solid substances. The measurements were performed under the same conditions as previously employed for oxidizing ND, i.e., heating from room temperature (RT) to 500°C at a heating rate of 5°C / min and holding at 500°C in air for 5 hours. During the holding period (500°C for 5 hours), the mixture of ND and NaCl ( Fig. 9 (c)) and ND alone ( Fig. 9 The weight of ND+NaCl decreases rapidly from 100 min to 250 min (i.e., the first 150 min after the temperature reaches 500 °C), and then decreases slowly as most of the ND has been oxidized (the weight of NaCl is assumed to be constant, from Fig. 9 (e) obtained), indicating that NaCl accelerates the oxidation process of ND. At the same time, the peak at ~130 minutes (i.e., about 30 minutes after the temperature reaches 500°C) is only observed in the DSC curve of the mixture (ND+NaCl) sample, indicating that some chemical reactions do occur there. On the other hand, the oxidation of pure ND is a fairly mild process, and the weight loss gradually reaches 37.40% after 5 hours of oxidation. The above results indicate that NaCl will accelerate the oxidation process of ND with the help of the "salt-assisted etching atmosphere" generated at high temperature, resulting in the etching of both diamond and non-diamond carbon, other impurities such as metals, etc.

[0085] Example 2

[0086] Cleaning process of SAAO method

[0087] NDs with an average particle size of 200 nm were used as starting material.

[0088] (1) 0.5 g of ND was mixed with 2.5 g of NaCl (99.5%, Sigma-Aldrich), and they were heated at 500° C. for 2 hours in air.

[0089] (2) 600 mg of the obtained sample was dispersed in 1 mL of deionized water and sonicated for 1 hour, and then the ND was purified once by centrifugation (1000 rcf, 5 minutes) with deionized water.

[0090] (3) The purified NDs were redispersed in deionized water and sonicated for 10 min to obtain a well-dispersed ND suspension for further characterization.

[0091] Comparative Example 2

[0092] For comparison, conventional air oxidation of ND was carried out in parallel to Example 2, ie without addition of NaCl to the starting material.

[0093] (1) 0.5 g of ND was heated at 500°C for 2 hours in air.

[0094] (2) 100 mg of the obtained sample was dispersed in 1 mL of deionized water and sonicated for 1 hour, and then the ND was purified once with deionized water by centrifugation (1000 rcf, 10 minutes).

[0095] (3) The purified NDs were redispersed in 1 mL of deionized water and sonicated for 10 min to obtain a well-dispersed ND suspension for further characterization.

[0096] Characterization

[0097] The procedures for SAAO of ND in Example 2 and conventional (without added salt) air oxidation of ND in Comparative Example 2 are shown in Fig.11 , where (a) photographs show the detailed process of salt-assisted and conventional air oxidation of NDs. (b) SEM characterization of the supernatant after centrifugation of the salt-assisted air-oxidized ND aqueous solution and (c) SEM characterization of the supernatant after centrifugation of the conventional air-oxidized ND aqueous solution. In (c), NDs are indicated by circles. (d) DLS measurement of the particle size distribution of the precipitate and supernatant after centrifugation (1000 rcf, 5 minutes) of the oxidized ND aqueous solution. The particle concentration of the supernatant of the SAAO ND solution was too low to be detected in the DLS measurement.

[0098] from Fig.11 (a) It can be seen that SAAO NDs can be easily collected by low speed (1000 rcf) and short time (5 minutes) centrifugation, while unoxidized NDs are relatively difficult to collect (requiring higher speeds such as 11000 rcf and longer time). These required additional centrifugation steps not only lead to more waste of ND samples, but also bring serious problems of ND agglomeration.

[0099] according to Fig.11 (d) DLS measurement shows a broad particle distribution in the supernatant of the unoxidized ND solution, indicating that there are some new components other than ND in the solution. This observation is consistent with Fig.11 (c) is consistent with the SEM image, non-diamond nanoparticles can be easily observed, and the formation mechanism of these impurities has been discussed in part (IV) of Example 1. However, the supernatant of the SAAO ND solution is very clear and mainly contains Na ions or Cl ions, see Fig.11 (b), and no detectable signal in DLS. Moreover, the precipitation of SAAO ND solution is of very high purity without any comparable impurities. In fact, the salt-assisted method significantly reduces the size of the produced non-diamond nanoparticles to a few nanometers, which can be completely removed by relatively low centrifugation speeds.

[0100] The above examples demonstrate that the cleaning process of the SAAO method is much easier than that of the conventional method, i.e., pure NDs (without any detectable impurity nanoparticles) can be produced by a one-step treatment (centrifugation at 1000 rcf for 5 minutes) after air oxidation without any further centrifugation step.

[0101] Example 3

[0102] Suitable SAAO conditions for 200 nm ND

[0103] NDs with an average particle size of 200 nm were used as starting material.

[0104] (1) 0.5 g of ND was mixed with 2.5 g of NaCl (99.5%, Sigma-Aldrich), and they were heated at 400° C. for 2 hours in air.

[0105] (2) 0.5 g of ND was mixed with 2.5 g of NaCl (99.5%, Sigma-Aldrich), and they were heated at 500° C. for 1 hour in air.

[0106] (3) 0.5 g of ND was mixed with 2.5 g of NaCl (99.5%, Sigma-Aldrich), and they were heated at 500° C. for 2 hours in air.

[0107] (4) 0.5 g of ND was mixed with 2.5 g of NaCl (99.5%, Sigma-Aldrich), and they were heated at 500° C. for 10 hours in air.

[0108] (5) 0.5 g of ND was mixed with 2.5 g of NaCl (99.5%, Sigma-Aldrich), and they were heated at 500° C. for 20 hours in air.

[0109] (6) 0.5 g of ND was mixed with 2.5 g of NaCl (99.5%, Sigma-Aldrich), and they were heated at 600° C. for 2 hours in air.

[0110] (7) 600 mg of the sample obtained above was dispersed in 1 mL of deionized water and ultrasonically treated for 1 hour. Then, the ND was purified by centrifugation with deionized water for 3 times (first time: 1000 rcf, 5 minutes; second time: 3000 rcf, 5 minutes; third time: 8000 rcf, 10 minutes).

[0111] (8) The purified NDs were redispersed in deionized water and sonicated for 10 min to obtain a well-dispersed ND suspension for further characterization.

[0112] Comparative Example 3

[0113] For comparison, conventional air oxidation of ND was carried out in parallel to Example 3, ie without addition of NaCl to the starting material.

[0114] (1) 0.5 g of ND was heated at 400°C for 2 hours in air.

[0115] (2) 0.5 g of ND was heated at 500°C for 1 hour in air.

[0116] (3) 0.5 g of ND was heated at 500°C for 2 hours in air.

[0117] (4) 0.5 g of ND was heated at 500°C for 10 hours in air.

[0118] (5) 0.5 g of ND was heated at 500°C for 20 hours in air.

[0119] (6) 0.5 g of ND was heated at 600°C for 2 hours in air.

[0120] (7) 100 mg of the sample obtained above was dispersed in 1 mL of deionized water and treated with ultrasound for 1 hour. Then, ND was purified three times by centrifugation (11000 rcf, 10 minutes) with deionized water.

[0121] (8) The purified NDs were redispersed in 1 mL of deionized water and sonicated for 10 min to obtain a well-dispersed ND suspension for further characterization.

[0122] Characterization

[0123] like Fig.12As depicted, starting from 2 hours (500°C), the SAAO method will produce clean and round NDs with a yield (i.e., ND weight ratio after oxidation / before oxidation) of ~77%. On the other hand, when the oxidation time increases from 1 hour to 20 hours, the yield of conventional air-oxidized NDs gradually decreases from ~96% to ~77%, while the small-sized nanoparticles adsorbed on the ND surface remain unchanged until the oxidation time reaches 20 hours. And for the 20-hour conventional air-oxidized NDs, only a small number of small-sized nanoparticles are still adsorbed on the surface (indicated by black circles); however, the fragment-like shape remains unchanged (i.e., there is no rounding effect), which is different from the 2-hour SAAO NDs, even though they have similar yields (~77%). At the same time, 400°C (2 hours) can hardly oxidize NDs, while 600°C (2 hours) is too strong to be controlled (the yields are extremely low, ~6% for the conventional method and ~0% for the SAAO method, respectively, Fig.12 SEM images are not shown in the figure). Therefore, 500°C and 2 hours of SAAO may be an ideal condition for 200 nm ND processing, with a clean surface and relatively high yield. As for the most frequently discussed condition in Example 1 (i.e., 500°C, 5 hours), the yield of the SAAO method (~20%) is much lower than that of the conventional method (~90%), indicating that the presence of NaCl will accelerate the oxidation process of NDs.

[0124] Example 4

[0125] Versatility of the SAAO method (KCl-assisted air oxidation of 50 nm NDs)

[0126] ND (HPHT, PolyQolor, China) with an average particle size of 50 nm was used as the starting material.

[0127] (1) 0.5 g of ND was mixed with 2.5 g of potassium chloride (KCl, 99.5%, Sigma-Aldrich), and they were heated at 500° C. for 2 hours in air.

[0128] (2) 600 mg of the obtained sample was dispersed in 1 mL of deionized water and sonicated for 1 hour, and then the ND was purified by centrifugation with deionized water three times (first time: 1000 rcf, 5 minutes; second time: 3000 rcf, 5 minutes; third time: 8000 rcf, 10 minutes).

[0129] (3) The purified NDs were redispersed in deionized water and sonicated for 10 min to obtain a well-dispersed ND suspension for further characterization.

[0130] Characterization

[0131] Fig.13 The results of KCl-assisted air oxidation of 50 nm NDs are depicted, which indicates that the developed SAAO method is not limited to 200 nm NDs or NaCl, and clean and round 50 nm NDs can also be achieved by KCl-assisted air oxidation at 500 °C for 2 h.

[0132] In summary, a simple, reliable and reproducible purification method, namely salt-assisted air oxidation (SAAO) treatment, was developed, which requires only one additional prior step, namely mixing the NDs with an appropriate amount of salt crystals (e.g., sodium chloride) before conventional oxidation. The developed method enables large-scale production of clean NDs with a rounded shape transformed from the original fragment-like shape. It was found that the impurity particles adsorbed on the NDs were etched by the "etching atmosphere" introduced by NaCl at high temperatures. These findings will significantly enhance the scope of these little gems in various scientific and industrial fields, especially in demanding fields such as biomedicine and quantum sensing, which require stable and reliable surface functionality.

[0133] Unless otherwise indicated in the examples and elsewhere in the specification and claims, all parts and percentages are by weight, all temperatures are in degrees Celsius, and pressures are at or near atmospheric.

[0134] With respect to any number or numerical range for a given characteristic, a number or parameter from one range can be combined with another number or parameter from a different range for the same characteristic to produce a numerical range.

[0135] Other than in the operating examples, or where otherwise indicated, all numbers, values ​​and / or expressions referring to quantities of ingredients, reaction conditions, and so forth used in the specification and claims are to be understood as being modified in all instances by the term "about".

[0136] Although the present invention is explained with respect to certain embodiments, it should be understood that various modifications thereof will become apparent to those skilled in the art after reading this specification. Therefore, it should be understood that the invention disclosed herein is intended to cover these modifications falling within the scope of the appended claims.

Claims

1. A method for purifying nanodiamonds, comprising: mixing the nanodiamond with at least one salt to form a mixture; heating the mixture at a temperature of 400° C. to 600° C. in air for a period of 1 hour to 5 hours; as well as combining the liquid with the heated mixture and centrifuging at a speed of 30 relative centrifugal force to 25,000 relative centrifugal force for a time period of 10 seconds to 60 minutes to provide purified nanodiamonds, Wherein, the salt is selected from one or more of sodium chloride, magnesium chloride, potassium chloride, calcium chloride and ammonium chloride. 2 . The method according to claim 1 , wherein the nanodiamonds have a size below 1 μm.

3. The method according to claim 1, wherein the nanodiamond is mixed with 0.1 to 100 times by weight of salt.

4. The method according to claim 1, wherein: The nanodiamond is mixed with 0.5 to 50 times by weight of salt.

5. The method of claim 1, wherein the heated mixture is centrifuged at a speed of 100 to 10,000 relative centrifugal force for a period of 30 seconds to 30 minutes.

6. The method according to claim 5, wherein: The heated mixture is centrifuged at a speed of 500 to 5000 relative centrifugal force for a period of 1 to 15 minutes.

7. The method of claim 1, wherein the liquid is selected from the group consisting of water, deionized water, organic liquids, and combinations thereof.

8. The method according to claim 7, wherein: The organic liquid is selected from methanol and ethanol.

9. The method of claim 1, wherein the purified nanodiamond comprises at least 99.9% by weight nanodiamond and less than 0.1% by weight impurities.

10. The method of claim 1, wherein the purified nanodiamonds are not agglomerated.

11. A method for preparing pure nanodiamonds, comprising: mixing unprocessed nanodiamond with at least one salt to form a mixture; heating the mixture at a temperature of 400° C. to 600° C. in air for a period of 1 hour to 5 hours; as well as combining the liquid with the heated mixture and centrifuging at a speed of 30 relative centrifugal force to 25,000 relative centrifugal force for a time of 10 seconds to 60 minutes to provide pure nanodiamonds having less than 0.01% impurities by weight, Wherein, the salt is selected from one or more of sodium chloride, magnesium chloride, potassium chloride, calcium chloride and ammonium chloride.

12. The method of claim 11, wherein the unprocessed nanodiamond has a size below 1 μm.

13. The method of claim 11, wherein the unprocessed nanodiamond contains impurities, the impurities comprising nanodiamonds <10 nm in size, amorphous carbon nanoparticles, metals, and metal oxides.

14. The method according to claim 11, wherein the unprocessed nanodiamond is mixed with 0.1 to 100 times by weight of the salt.

15. The method according to claim 11, wherein: The raw nanodiamond is mixed with 0.5 to 50 times the weight of salt.

16. The method of claim 11, wherein the heated mixture is centrifuged at a speed of 100 relative centrifugal force to 10,000 relative centrifugal force for a time of 30 seconds to 30 minutes.

17. The method according to claim 16, wherein: The heated mixture is centrifuged at a speed of 500 to 5000 relative centrifugal force for a period of 1 to 15 minutes.

18. The method of claim 11, wherein the liquid is selected from the group consisting of water, deionized water, organic liquids, and combinations thereof.

19. The method according to claim 18, wherein: The organic liquid is selected from methanol and ethanol.

20. The method of claim 11, wherein the pure nanodiamond comprises at least 99.9% by weight nanodiamond and less than 0.1% by weight impurities.

21. The method of claim 11, wherein the pure nanodiamonds are not agglomerated.

Citation Information

Patent Citations

  • Preparation method of ultrafine-crystal grain polycrystalline diamond material

    CN103691362A

  • Method for removing impurity iron in new diamond nano-powder

    CN104276568A

  • Method for producing synthetic diamonds

    CN104884385A

  • Medicine carrier based on nano diamond, medicinal complex as well as preparation method and application thereof

    CN107929242A

  • Method for removing graphite carbon in nano-diamond ash material

    CN109305677A