A Pd / Ni / SSZ-13 catalyst with high hydrothermal stability and its preparation method and application

By doping Ni in the Pd/SSZ-13 catalyst and preparing the Pd/Ni/SSZ-13 catalyst by equal volume impregnation method, the problem of insufficient hydrothermal stability in the water vapor environment is solved, and the cold start-up process is realized Highly efficient NOx adsorption and emission control.

CN116459867BActive Publication Date: 2024-11-22HUAQIAO UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310384034.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-11-22
Estimated Expiration
2043-04-12

AI Technical Summary

Technical Problem

The existing Pd/SSZ-13 catalysts are insufficient in water vapor environments, resulting in poor NOx emission control effect during the cold start of the diesel engine.

Method used

The Pd/Ni/SSZ-13 catalyst was prepared by two-step equal volume impregnation method. The hydrothermal stability of the catalyst was improved by doping the transition metal Ni in the NH4/SSZ-13 molecular sieve and loading the metal Pd at a lower temperature.

Benefits of technology

It significantly improves the hydrothermal stability of the catalyst, maintains almost the same NO adsorption capacity, and avoids a significant decrease in NO adsorption amount after hydrothermal aging. It is suitable for low-temperature cold-start NOx emission control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116459867B_ABST
    Figure CN116459867B_ABST
Patent Text Reader

Abstract

The present invention discloses a high hydrothermal stability Pd / Ni / SSZ‑13 catalyst and its preparation method and application. Using an isovolumetric impregnation method, Ni is loaded onto NH4‑SSZ‑13 to prepare Ni / SSZ‑13; then using an isovolumetric impregnation method, Pd is loaded onto Ni / SSZ‑13 to obtain Pd / Ni / SSZ‑13. The doping amount of transition metal Ni is 0.02‑0.15 mmol / g, and Ni mainly exists in ionic form; the loading amount of Pd is 1 wt.%, and it mainly exists in ionic form. The catalyst is used to adsorb and store NO during the cold start process of an automobile, and while having a high NO adsorption amount, it also improves the hydrothermal stability of the original Pd / SSZ‑13 catalyst. The catalyst is environmentally friendly, has a simple catalyst preparation process, and is easy to operate and scale up.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and specifically relates to a Pd / Ni / SSZ-13 catalyst with high hydrothermal stability and a preparation method and application thereof, and is especially used for adsorbing NO during the cold start (temperature < 200°C) process of an automobile. Background Art

[0002] At present, with the increase in the number of motor vehicles, the problem of air pollution caused by motor vehicle exhaust has also attracted widespread attention. Among them, nitrogen oxides are one of the main pollutants causing air pollution. 95% of the thermal nitrogen oxides produced by high-temperature combustion of motor vehicle internal combustion engines are NO. NO is easily oxidized into other nitrogen oxides in the air, further polluting the atmosphere.

[0003] Currently NO x Emission control is mainly through the reaction of NH3 to NO x Ammonia selective catalytic reduction (NH3-SCR) or NO x Storage reduction (NSR) removes NO in a wide temperature range (200-500°C). However, in vehicles equipped with SCR or NSR systems, 80% of NOx is emitted during the cold start process (2-5 minutes), when the denitrification catalyst has not yet reached the operating temperature. In the future, reducing cold start NOx X Emissions are to control diesel engine exhaust NO x Emissions are key.

[0004] Passive NO x Adsorption (PNA) is the process of converting NO x Adsorb and store, desorb NO at temperatures above 200°C x At this time, the SCR / NSR catalyst reaches the optimal catalytic temperature and can desorb NO x Eliminate. Pd / SSZ-13 is the most promising PNA catalyst for commercial applications. However, due to the fact that the catalyst will be exposed to a harsh water vapor environment during the regeneration of diesel particulate filters, insufficient hydrothermal stability has always been the main challenge for Pd / SSZ-13 in practical vehicle applications. Therefore, it is necessary to improve the hydrothermal stability of Pd / SSZ-13. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies of the prior art, provide a Pd / Ni / SSZ-13 catalyst with high hydrothermal stability and a preparation method and application thereof, and solve the problems in the above-mentioned background technology.

[0006] One of the technical solutions adopted by the present invention to solve the technical problem is: a method for preparing a Pd / Ni / SSZ-13 catalyst with high hydrothermal stability is provided, comprising the following steps:

[0007] 1) dissolving the nitrate of transition metal Ni in water to form a nitrate aqueous solution; adding the nitrate aqueous solution to a NH4 + NH4 / SSZ-13 molecular sieve, stirred until completely wetted and then allowed to stand in an air atmosphere at 20-25°C to allow transition metal Ni to reach the doping amount. After drying, Ni / SSZ-13 catalyst was obtained;

[0008] 2) adding the Ni / SSZ-13 catalyst prepared in step 1) to a 1 wt.% aqueous palladium nitrate solution by an equal volume impregnation method, stirring until completely wetted, and then standing in an air atmosphere at 20-25° C. to allow Pd to reach the loading amount. After drying, calcining in an air atmosphere at 500-550° C. for 4-6 hours to obtain a Pd / Ni / SSZ-13 catalyst.

[0009] In a preferred embodiment of the present invention, in step 1), the concentration of the nitrate aqueous solution is 0.02-0.15 mmol / L.

[0010] In a preferred embodiment of the present invention, in step 1), the NH4 / SSZ-13 molecular sieve is composed of Si, Al and O connected to each other and has a chabazite structure.

[0011] In a preferred embodiment of the present invention, in step 1), the doping amount of transition metal Ni is 0.02-0.15 mmol / g.

[0012] In a preferred embodiment of the present invention, the standing time in step 1) and step 2) is at least 10 hours, preferably 12-24 hours.

[0013] In a preferred embodiment of the present invention, in step 2), calcination is carried out in an air atmosphere with a programmed heating rate of 2°C / min.

[0014] In a preferred embodiment of the present invention, in step 1), the equal volume impregnation method is to add nitrate aqueous solution (total amount 1 mL) dropwise to 1g NH4 / SSZ-13 molecular sieve carrier, and the stirring process needs to make the solution evenly dispersed in the carrier. The impregnation and stirring process in step 2) is similar.

[0015] The second technical solution adopted by the present invention to solve its technical problem is: providing a high hydrothermal stability Pd / Ni / SSZ-13 catalyst prepared by the above method, including a SSZ-13 carrier, doped metal Ni and loaded metal Pd.

[0016] In a preferred embodiment of the present invention, the transition metal Ni exists in the form of ions, and the doping amount is 0.02 mmol / g, 0.05 mmol / g and 0.15 mmol / g, preferably 0.05 mmol / g.

[0017] In a preferred embodiment of the present invention, the loaded metal Pd exists in the form of ions, and the loading amount is 1 wt.%.

[0018] The third technical solution adopted by the present invention to solve its technical problem is: providing the application of the above-mentioned catalyst in low-temperature adsorption of NO, which is used for emission control of exhaust nitrogen oxides during the cold start process of motor vehicle exhaust gas, wherein the exhaust gas temperature during the cold start process is lower than 200°C.

[0019] Compared with the background technology, this technical solution has the following advantages:

[0020] The present invention adopts a two-step equal volume impregnation method to prepare NH4 / SSZ-13 into Pd / Ni / SSZ-13. Compared with the original Pd / SSZ-13, in the technical scheme of the present invention, Pd / Ni / SSZ-13 has almost the same NO adsorption capacity, but its hydrothermal stability is significantly improved. When the transition metal Ni doping amount is 0.05mmol / g, the NO adsorption amount of the catalyst after high-temperature hydrothermal aging treatment is equivalent to the NO adsorption amount of fresh Pd / SSZ-13. However, after hydrothermal aging under the same conditions, the NO adsorption amount of the Pd / SSZ-13 catalyst control sample decreased by 80%. It shows that the introduction of Ni has a significant improvement effect on the hydrothermal stability of Pd / SSZ-13. The raw materials of the catalyst are cheap and environmentally friendly. The catalyst preparation process is simple and easy to operate and scale up. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is the XRD spectra of fresh Pd / Ni / SSZ-13 catalyst and ordinary Pd / SSZ-13 catalyst.

[0022] Figure 2 It is the XRD spectra of the hydrothermal aging (HTA) Pd / Ni / SSZ-13 catalyst and the ordinary Pd / SSZ-13 catalyst.

[0023] Figure 3 In the figure, (a) is a graph showing the low-temperature NO adsorption and desorption performance of different fresh catalysts, (b) is a graph showing the low-temperature NO adsorption and desorption performance of different catalysts after hydrothermal treatment at 850°C, where the horizontal axis is time, the left vertical axis is the concentration of NO, and the right vertical axis is temperature; (c) is a bar graph comparing different catalysts before and after hydrothermal treatment. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is further illustrated and described below through specific implementation modes in combination with the accompanying drawings.

[0025] Embodiment 1:

[0026] The 0.02Pd / Ni / SSZ-13 catalyst was prepared by the following specific steps:

[0027] (1) Take 0.02mmol of Ni(NO3)2 solid and 1000mL of deionized water and mix them evenly; first, place 1g of NH4 / SSZ-13 in an agate mortar, take 1mL of the prepared Ni(NO3)2 solution, and add the Ni(NO3)2 solution drop by drop into the NH4 / SSZ-13, stirring and grinding continuously during the addition process to make the Ni(NO3)2 solution evenly dispersed in the SSZ-13 carrier, and let the wet catalyst after the addition stand in an air atmosphere at room temperature of 20-25℃ for 10 hours to obtain 0.02Ni / SSZ-13 catalyst.

[0028] (2) 1 g of 0.02 Ni / SSZ-13 was placed in an agate mortar, and 1 mL of 1 wt.% Pd(NO3)2 solution was added dropwise onto the 0.02 Ni / SSZ-13. The mixture was continuously stirred and ground during the addition process. The wet catalyst was allowed to stand in an air atmosphere at room temperature of 20-25°C for 10 hours. After standing, the catalyst was heated to 600°C in a muffle furnace at a heating rate of 2°C / min and calcined for 5 hours to obtain a fresh 0.02 Pd / Ni / SSZ-13 catalyst.

[0029] (3) 1 g of 0.02Pd / Ni / SSZ-13 was placed in a tubular furnace for hydrothermal aging treatment (HTA). HTA was carried out at 850°C for 16 hours in air containing 10% H2O at a total flow rate of 100 mL / min. After the treatment, an aged 0.02Pd / Ni / SSZ-13 catalyst was prepared.

[0030] Embodiment 2:

[0031] The 0.1Pd / Ni / SSZ-13 catalyst was prepared by the following specific steps:

[0032] (1) 0.1 mmol of Ni(NO3)2 solid and 1000 mL of deionized water are mixed and stirred evenly; first, 1 g of NH4 / SSZ-13 is placed in an agate mortar, 1 mL of the prepared Ni(NO3)2 solution is taken, and the Ni(NO3)2 solution is added dropwise to the NH4 / SSZ-13. During the addition, the Ni(NO3)2 solution is continuously stirred and ground to make the Ni(NO3)2 solution evenly dispersed in the Ni / SSZ-13. The wet catalyst after the addition is allowed to stand in an air atmosphere at room temperature of 20-25°C for 10 hours to obtain 0.1 Ni / SSZ-13.

[0033] (2) 1 g of 0.1 Ni / SSZ-13 was placed in an agate mortar, and 1 mL of 1 wt.% Pd(NO3)2 solution was added dropwise onto the 0.1 Ni / SSZ-13. The mixture was continuously stirred and ground during the addition process. The wet catalyst was allowed to stand in an air atmosphere at room temperature of 20-25°C for 10 hours. After standing, the catalyst was heated to 600°C in a muffle furnace at a heating rate of 2°C / min and calcined for 5 hours to obtain 0.1 Pd / Ni / SSZ-13.

[0034] (3) 1 g of 0.1 Pd / Ni / SSZ-13 was placed in a tubular furnace for hydrothermal aging treatment (HTA). HTA was carried out at 850°C for 16 hours in air containing 10% H2O with a total flow rate of 100 mL / min. After the treatment, aged 0.1 Pd / Ni / SSZ-13 was obtained.

[0035] Example 3

[0036] The 0.15Pd / Ni / SSZ-13 catalyst was prepared by the following specific steps:

[0037] (1) 0.15mmol Ni(NO3)2 solid and 25mL deionized water are mixed and stirred evenly; first, 1g NH4 / SSZ-13 is placed in an agate mortar, 1mL of the prepared Ni(NO3)2 solution is taken, and the Ni(NO3)2 solution is added dropwise to the NH4 / SSZ-13, and the Ni(NO3)2 solution is continuously stirred and ground during the addition process to make the Ni(NO3)2 solution evenly dispersed in the Ni / SSZ-13. The wet catalyst after the addition is allowed to stand in an air atmosphere at room temperature of 20-25°C for 10 hours to obtain 0.15Ni / SSZ-13.

[0038] (2) 1 g of Ni / SSZ-13 was placed in an agate mortar, and 1 mL of 1 wt.% Pd(NO3)2 solution was dripped onto the Ni / SSZ-13 dropwise, with continuous stirring and grinding during the dripping process. The wet catalyst was allowed to stand in an air atmosphere at room temperature of 20-25°C for 10 hours. After standing, the catalyst was heated to 600°C in a muffle furnace at a heating rate of 2°C / min and calcined for 5 hours to prepare 0.15Pd / Ni / SSZ-13.

[0039] Low temperature NO adsorption performance test:

[0040] 40 mg of each of the catalysts prepared in Examples 1 to 3 and a common Pd / SSZ-13 catalyst were taken for low-temperature NO adsorption performance testing. NO adsorption and subsequent desorption experiments were carried out in a fixed-bed quartz tube reactor (inner diameter 4 mm) under simulated automobile exhaust conditions. The total flow rate was adjusted to 200 mL / min by a mass flowmeter controller. The reaction gas contained 200 ppm of NO, 5% H2O, 5% O2 and N2 in balance. 40 mg of the catalyst (40-60 mesh) was diluted with 260 mg of quartz sand of the same size, equivalent to 360,000 mL·h -1 ·g -1 The bed temperature at the top and bottom of the quartz tube was monitored by thermocouples. The gas tube was heated to 140 °C by heating tape to avoid condensation of water vapor.

[0041] Before NO absorption and desorption, the sample was pretreated with 10% O2 / N2 at 600°C for 30 minutes and then cooled to 100°C. The feed gas was first stabilized in the bypass line for 10 minutes and then directed to the catalyst at 100°C and maintained for 10 minutes to ensure catalyst adsorption equilibrium. The temperature was then raised to 600°C at a heating rate of 10°C / min for NO absorption and desorption. x Desorption.

[0042] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a Pd / Ni / SSZ-13 catalyst with high hydrothermal stability, characterized in that: The steps include: 1) Dissolve the nitrate of transition metal Ni in water to form a nitrate aqueous solution; add the nitrate aqueous solution into a solution containing NH4 + NH4 / SSZ-13 molecular sieves, stirred until completely wetted, and then allowed to stand in an air atmosphere at 20-25°C to allow the transition metal Ni to reach the doping amount. After drying, the Ni / SSZ-13 catalyst was obtained; 2) Adding the Ni / SSZ-13 catalyst prepared in step 1) to a 1 wt.% aqueous palladium nitrate solution by an equal volume impregnation method, stirring until completely wetted, and standing in an air atmosphere at 20-25 °C to allow Pd to reach the loading amount, and after drying, calcining in an air atmosphere at 500-550 °C for 4-6 hours to obtain a Pd / Ni / SSZ-13 catalyst, wherein the transition metal Ni exists in the form of ions with a doping amount of 0.05 mmol / g; and the loaded metal Pd exists in the form of ions with a loading amount of 1 wt%.

2. The method for preparing a Pd / Ni / SSZ-13 catalyst with high hydrothermal stability according to claim 1, characterized in that: In step 1), the concentration of the nitrate aqueous solution is 0.02-0.15 mmol / L.

3. The method for preparing a Pd / Ni / SSZ-13 catalyst with high hydrothermal stability according to claim 1, characterized in that: In step 1), the NH4 / SSZ-13 molecular sieve is composed of Si, Al and O connected to each other and has a chabazite structure.

4. The method for preparing a Pd / Ni / SSZ-13 catalyst with high hydrothermal stability according to claim 1, characterized in that: The standing time in step 1) and step 2) is 10-24 hours.

5. The method for preparing a Pd / Ni / SSZ-13 catalyst with high hydrothermal stability according to claim 1, characterized in that: In step 2), calcination is carried out in an air atmosphere with a programmed heating rate of 2 °C / min.

6. A Pd / Ni / SSZ-13 catalyst with high hydrothermal stability prepared by the method according to any one of claims 1 to 5, characterized in that: The invention comprises a SSZ-13 carrier, doped metal Ni and loaded metal Pd.

7. Use of the catalyst as claimed in claim 6 in low temperature adsorption of NO, characterized in that: Used for controlling the emission of nitrogen oxides from exhaust gas during the cold start process of motor vehicle exhaust gas, wherein the exhaust gas temperature during the cold start process is lower than 200°C.