A kind of synthetic method of lithium tetrafluoroborate

In the synthesis process of lithium tetrafluoroborate, the reaction of boron oxide with hydrofluoric acid and high-purity lithium carbonate, combined with low-temperature evaporation and fractionation technology, solved the problem of incomplete crystallinity and crystal form of domestic lithium tetrafluoroborate electrolyte materials. Problem, high-performance lithium tetrafluoroborate preparation was achieved, which improved the electrochemical performance of lithium batteries and reduced the problem of gas expansion.

CN116462205BActive Publication Date: 2024-10-11YICHUN GUOXUAN BATTERY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310322296.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-11
Estimated Expiration
2043-03-29

AI Technical Summary

Technical Problem

Domestic lithium tetrafluoroborate electrolyte materials have poor lithium battery performance due to incomplete crystallinity and crystal form, which can easily lead to battery bulging, easy electrolyte decomposition, poor cycle performance and low voltage platform.

Method used

The reaction between boron oxide and hydrofluoric acid is used to generate a tetrafluoroboric acid solution, which is combined with high-purity lithium carbonate for hydrogenation reaction to form a lithium tetrafluoroborate solution. Through low-temperature evaporation and low-temperature fractionation technology, the concentration is gradually increased and crystal nuclei are grown to obtain crystals. It uses low-boiling organic solvents to dissolve and calcium hydride to remove trace moisture to achieve the integrity and purity of the crystal form.

Benefits of technology

It improves the rate performance and cycle life of lithium batteries and reduces the inflation problem of lithium batteries. The prepared lithium tetrafluoroborate has high crystallinity and complete crystal form, which significantly improves the electrochemical performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a synthesis method of lithium tetrafluoroborate, comprising: S1, slowly adding boron oxide to a hydrofluoric acid solution under stirring, fully reacting, standing for a period of time after the reaction is completed, and obtaining a tetrafluoroboric acid solution; S2, evenly mixing lithium carbonate micropowder and water in a hydrogenation device, introducing CO2 gas, performing a hydrogenation reaction under stirring, standing for a period of time after the reaction is completed, and obtaining a lithium bicarbonate solution; S3, slowly adding the tetrafluoroboric acid solution to a lithium bicarbonate solution under stirring, fully reacting, standing for a period of time after the reaction is completed, and obtaining a lithium tetrafluoroborate solution; S4, low-temperature evaporation of the lithium tetrafluoroborate solution, collecting crystals, dissolving in a low-boiling point organic solvent, adding an appropriate amount of calcium hydride to remove trace water, and then performing low-temperature fractionation, collecting crystals, and obtaining. The lithium tetrafluoroborate prepared by the invention has the characteristics of high crystallinity, complete crystal form, and excellent electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion battery electrolytes, and in particular to a method for synthesizing lithium tetrafluoroborate. Background Art

[0002] The production and consumption of lithium-ion batteries has become a mainstream product of new energy consumption. At present, the production and sales volume of lithium-ion batteries produced in my country has reached 232,624,205,000 units. With the introduction of the "dual carbon" concept, the production and sales of lithium-ion batteries have shown a more rapid growth trend.

[0003] As lithium-ion battery manufacturing technology gradually matures and stabilizes, traditional technologies have encountered bottlenecks in improving the performance of lithium-ion batteries, especially in the field of power battery manufacturing, which requires improving the battery's specific energy, specific power, cycle life, and lower internal resistance. It is far from enough to improve these performances only from the perspective of battery cell structure and ratio. It is necessary for all fields in the industry to conduct research on all aspects of batteries in order to achieve the goal of improving battery performance overall.

[0004] my country is currently the world's major manufacturer of lithium batteries, and its manufacture and use of electrolytes have made comprehensive progress. Since 2021, with the explosion of the lithium battery application market and the lithium battery manufacturing market, the demand for electrolytes has exploded. Due to different crystallinity and incomplete crystal forms, domestic electrolytes prepared with domestic electrolyte materials cause problems such as battery swelling, easy decomposition and gas production of electrolytes, poor cycle performance, and low voltage platform. Therefore, how to prepare lithium tetrafluoroborate with higher crystallinity and more complete crystal form, thereby improving the electrochemical performance of lithium batteries and reducing the problem of gas swelling of lithium batteries, has become a problem that needs to be solved urgently. Summary of the invention

[0005] Based on the technical problems existing in the background technology, the present invention proposes a synthesis method of lithium tetrafluoroborate.

[0006] A method for synthesizing lithium tetrafluoroborate proposed by the present invention comprises the following steps:

[0007] S1. Slowly add boron oxide to the hydrofluoric acid solution under stirring to fully react. After the reaction is completed, let it stand for 3-6.5 hours to obtain a tetrafluoroboric acid solution;

[0008] S2, in a hydrogenation device, lithium carbonate powder and water are mixed evenly, CO2 gas is introduced, and a hydrogenation reaction is carried out under stirring. After the reaction is completed, the mixture is allowed to stand for 25-30 minutes to obtain a lithium bicarbonate solution;

[0009] S3, slowly adding the tetrafluoroboric acid solution to the lithium bicarbonate solution under stirring to fully react, and after the reaction is completed, standing at 15-33° C. for 14-16 hours to obtain a lithium tetrafluoroborate solution;

[0010] S4, subjecting the lithium tetrafluoroborate solution to low-temperature evaporation, collecting crystals after evaporation is complete, dissolving the crystals in a low-boiling point organic solvent, adding an appropriate amount of calcium hydride to remove trace moisture, and then subjecting the solution to low-temperature fractionation, collecting the crystals after fractionation is complete, to obtain.

[0011] Preferably, the molar ratio of boron oxide to hydrofluoric acid is 1:(8-8.15).

[0012] Preferably, the purity of the boron oxide is ≥99.9%; and the concentration of the hydrofluoric acid solution is 22.5 mol / L.

[0013] Preferably, in S1, the reaction conditions are: stirring the reaction at a temperature of 23-28° C. for 30-45 min; preferably, in S1, the rotation speed of the stirring reaction is 10-15 r / min.

[0014] Preferably, the purity of the lithium carbonate powder is ≥99.9% and the particle size is 5-25 μm.

[0015] Preferably, in S2, the temperature of the hydrogenation reaction is 25-28°C and the time is 30-45 min; preferably, in S2, the stirring speed of the hydrogenation reaction is 35-65 r / min.

[0016] Preferably, in S2, the flow rate of CO2 gas is 0.15-0.2 L / min.

[0017] Preferably, in S2, the weight ratio of lithium carbonate powder to water is (335-370):5000.

[0018] Preferably, in S3, the molar ratio of tetrafluoroboric acid to lithium bicarbonate is (1.03-1.05):1.

[0019] Preferably, in S3, the reaction conditions are: stirring the reaction at 23-28° C. for 2.5-3 h; preferably, in S3, the rotation speed of the stirring reaction is 5-8 r / min.

[0020] Preferably, in S4, the temperature of the low-temperature evaporation is 15-33°C.

[0021] Preferably, in S4, the temperature of the low-temperature distillation is 35-63° C.; and the low-boiling point organic solvent is at least one of anhydrous ethanol and anhydrous ether.

[0022] In S4, the low boiling point organic solvent can be recovered by freezing and condensing.

[0023] The beneficial effects of the present invention are as follows:

[0024] The present invention first uses boron oxide and hydrofluoric acid to react to obtain a tetrafluoroboric acid solution, uses high-purity lithium carbonate to perform a hydrogenation reaction to obtain a lithium bicarbonate solution, then reacts the tetrafluoroboric acid solution with the lithium bicarbonate solution to obtain a lithium tetrafluoroborate solution, and allows the solution to stand for a long time to fully react; then the lithium tetrafluoroborate solution is evaporated at low temperature, as the concentration gradually increases during the evaporation process and a crystal nucleus is formed, the crystal nucleus gradually grows to obtain a crystal of lithium tetrafluoroborate, and then a low-boiling point organic solvent is used as a solvent to dissolve the crystal, calcium hydride is added to remove trace water, and then fractionated at low temperature, as the solvent continues to volatilize, the concentration of lithium tetrafluoroborate continues to increase, and its crystal nucleus continues to grow along the crystal, thereby achieving crystal reformation, and obtaining lithium tetrafluoroborate with a more complete crystal form. The lithium tetrafluoroborate prepared by the present invention has the characteristics of high crystallinity and complete crystal form, can effectively improve the electrochemical properties such as rate performance and cycle life of lithium batteries, and effectively reduce the problem of gas expansion of lithium batteries. DETAILED DESCRIPTION

[0025] The technical solution of the present invention is described in detail below through specific embodiments.

[0026] Example 1

[0027] A method for synthesizing lithium tetrafluoroborate comprises the following steps:

[0028] S1. Boron oxide (B2O3) with a purity of 99.9% was slowly added to a hydrofluoric acid solution with a concentration of 22.5 mol / L under stirring, and the mixture was stirred for reaction for 30 min at a temperature of 23° C. and a rotation speed of 10 r / min. After the reaction was completed, the mixture was allowed to stand for 3 h to obtain a tetrafluoroboric acid solution, wherein the molar ratio of boron oxide to hydrofluoric acid was 1:8;

[0029] S2, add 5000mL deionized water to the hydrogenation tank, slowly pass CO2 gas (flow rate is 0.15L / min) at the bottom of the hydrogenation tank, pass CO2 gas for 20min, add 370g lithium carbonate powder with a purity of 99.9% and a particle size of 5-25μm to the hydrogenation tank under stirring, stir and react for 30min at a temperature of 25°C and a rotation speed of 35r / min, and stand for 25min after completion of the reaction to obtain a lithium bicarbonate solution;

[0030] S3, slowly adding the tetrafluoroboric acid solution to the lithium bicarbonate solution under stirring, stirring and reacting for 2.5 hours at a temperature of 23° C. and a rotation speed of 5 r / min. After the reaction is completed, standing at 15° C. for 14 hours to obtain a lithium tetrafluoroborate solution, wherein the molar ratio of tetrafluoroboric acid to lithium bicarbonate is 1.01:1;

[0031] S4. The lithium tetrafluoroborate solution is evaporated at 15°C, and the crystals are collected after evaporation. 70 g of the crystals are dissolved in 600 mL of anhydrous ethanol, and 25 g of calcium hydride is added to remove trace moisture. The solution is then fractionated at 35°C, and the crystals are collected after fractionation.

[0032] After testing, the purity of the product obtained above was 99.99%.

[0033] Example 2

[0034] A method for synthesizing lithium tetrafluoroborate comprises the following steps:

[0035] S1. Boron oxide (B2O3) with a purity of 99.9% was slowly added to a hydrofluoric acid solution with a concentration of 22.5 mol / L under stirring, and the mixture was stirred for reaction for 40 min at a temperature of 25° C. and a rotation speed of 12 r / min. After the reaction was completed, the mixture was allowed to stand for 5 h to obtain a tetrafluoroboric acid solution, wherein the molar ratio of boron oxide to hydrofluoric acid was 1:8.05;

[0036] S2, add 5000mL deionized water to the hydrogenation tank, slowly pass CO2 gas at the bottom of the hydrogenation tank (flow rate is 0.18L / min), pass CO2 gas for 20min, add 370g lithium carbonate powder with a purity of 99.9% and a particle size of 5-25μm to the hydrogenation tank under stirring, stir and react for 35min at a temperature of 26°C and a rotation speed of 50r / min, and let stand for 28min after completion of the reaction to obtain a lithium bicarbonate solution;

[0037] S3, the tetrafluoroboric acid solution was slowly added to the lithium bicarbonate solution under stirring, and the reaction was stirred for 2.8 hours at a temperature of 25 ° C and a rotation speed of 7 r / min. After the reaction was completed, the solution was allowed to stand at 25 ° C for 15 hours to obtain a lithium tetrafluoroborate solution, wherein the molar ratio of tetrafluoroboric acid to lithium bicarbonate was 1.03:1;

[0038] S4. The lithium tetrafluoroborate solution is evaporated at 25°C, and the crystals are collected after evaporation. 70 g of the crystals are dissolved in 600 mL of anhydrous ethanol, and 25 g of calcium hydride is added to remove trace moisture. The solution is then fractionated at 50°C, and the crystals are collected after fractionation.

[0039] After testing, the purity of the product obtained above was 99.99%.

[0040] Example 3

[0041] A method for synthesizing lithium tetrafluoroborate comprises the following steps:

[0042] S1. Boron oxide (B2O3) with a purity of 99.9% was slowly added to a hydrofluoric acid solution with a concentration of 22.5 mol / L under stirring, and the mixture was stirred for reaction for 45 min at a temperature of 28° C. and a rotation speed of 15 r / min. After the reaction was completed, the mixture was allowed to stand for 6.5 h to obtain a tetrafluoroboric acid solution, wherein the molar ratio of boron oxide to hydrofluoric acid was 1:8.15;

[0043] S2, add 5000mL deionized water to the hydrogenation tank, slowly pass CO2 gas (flow rate is 0.2L / min) at the bottom of the hydrogenation tank, pass CO2 gas for 20min, add 370g lithium carbonate powder with a purity of 99.9% and a particle size of 5-25μm to the hydrogenation tank under stirring, stir and react for 45min at a temperature of 28°C and a rotation speed of 65r / min, and let stand for 30min after completion of the reaction to obtain a lithium bicarbonate solution;

[0044] S3, slowly adding the tetrafluoroboric acid solution to the lithium bicarbonate solution under stirring, stirring and reacting for 3 hours at a temperature of 28° C. and a rotation speed of 8 r / min. After the reaction is completed, standing at 33° C. for 16 hours to obtain a lithium tetrafluoroborate solution, wherein the molar ratio of tetrafluoroboric acid to lithium bicarbonate is 1.05:1;

[0045] S4. The lithium tetrafluoroborate solution is evaporated at 33°C, and the crystals are collected after evaporation. 70 g of the crystals are dissolved in 600 mL of anhydrous ethanol, and 25 g of calcium hydride is added to remove trace moisture. The solution is then fractionated at 63°C, and the crystals are collected after fractionation.

[0046] After testing, the purity of the product obtained above was 99.99%.

[0047] Comparative Example 1

[0048] A method for synthesizing lithium tetrafluoroborate comprises the following steps:

[0049] S1. Boron oxide (B2O3) with a purity of 99.9% was slowly added to a hydrofluoric acid solution with a concentration of 22.5 mol / L under stirring, and the mixture was stirred for reaction for 30 min at a temperature of 23° C. and a rotation speed of 10 r / min. After the reaction was completed, the mixture was allowed to stand for 3 h to obtain a tetrafluoroboric acid solution, wherein the molar ratio of boron oxide to hydrofluoric acid was 1:8;

[0050] S2. Slowly add lithium carbonate powder with a purity of 99.9% and a particle size of 5-25 μm into the tetrafluoroboric acid solution under stirring, and stir the mixture for 2.5 hours at a temperature of 23° C. and a rotation speed of 5 r / min. After the reaction is completed, the mixture is allowed to stand at 15° C. for 14 hours to obtain a lithium tetrafluoroborate solution, wherein the molar ratio of tetrafluoroboric acid to lithium carbonate is 1.01:0.5;

[0051] S4. The lithium tetrafluoroborate solution is evaporated at 15°C, and the crystals are collected after evaporation. 70 g of the crystals are dissolved in 600 mL of anhydrous ethanol, and 25 g of calcium hydride is added to remove trace moisture. The solution is then fractionated at 35°C, and the crystals are collected after fractionation.

[0052] After testing, the purity of the product obtained above was 99.8%.

[0053] Comparative Example 2

[0054] A method for synthesizing lithium tetrafluoroborate comprises the following steps:

[0055] S1. Boron oxide (B2O3) with a purity of 99.9% was slowly added to a hydrofluoric acid solution with a concentration of 22.5 mol / L under stirring, and the mixture was stirred for reaction for 30 min at a temperature of 23° C. and a rotation speed of 10 r / min. After the reaction was completed, the mixture was allowed to stand for 3 h to obtain a tetrafluoroboric acid solution, wherein the molar ratio of boron oxide to hydrofluoric acid was 1:8;

[0056] S2, add 5000mL deionized water to the hydrogenation tank, slowly pass CO2 gas (flow rate is 0.15L / min) at the bottom of the hydrogenation tank, pass CO2 gas for 20min, add 370g lithium carbonate powder with a purity of 99.9% and a particle size of 5-25μm to the hydrogenation tank under stirring, stir and react for 30min at a temperature of 25°C and a rotation speed of 35r / min, and stand for 25min after completion of the reaction to obtain a lithium bicarbonate solution;

[0057] S3, slowly adding the tetrafluoroboric acid solution to the lithium bicarbonate solution under stirring, stirring and reacting for 2.5 hours at a temperature of 23° C. and a rotation speed of 5 r / min. After the reaction is completed, standing at 15° C. for 14 hours to obtain a lithium tetrafluoroborate solution, wherein the molar ratio of tetrafluoroboric acid to lithium bicarbonate is 1.01:1;

[0058] S4. Heat the lithium tetrafluoroborate solution at 45°C to evaporate, collect the crystals after evaporation, dissolve 70 g of the crystals in 600 mL of anhydrous ethanol, add 25 g of calcium hydride to remove trace moisture, and then perform low-temperature fractionation at 35°C. Collect the crystals after fractionation to obtain S4.

[0059] After testing, the purity of the product obtained above was 99.3%.

[0060] Comparative Example 3

[0061] A method for synthesizing lithium tetrafluoroborate comprises the following steps:

[0062] S1. Boron oxide (B2O3) with a purity of 99.9% was slowly added to a hydrofluoric acid solution with a concentration of 22.5 mol / L under stirring, and the mixture was stirred for reaction for 30 min at a temperature of 23° C. and a rotation speed of 10 r / min. After the reaction was completed, the mixture was allowed to stand for 3 h to obtain a tetrafluoroboric acid solution, wherein the molar ratio of boron oxide to hydrofluoric acid was 1:8;

[0063] S2, add 5000mL deionized water to the hydrogenation tank, slowly pass CO2 gas (flow rate is 0.15L / min) at the bottom of the hydrogenation tank, pass CO2 gas for 20min, add 370g lithium carbonate powder with a purity of 99.9% and a particle size of 5-25μm to the hydrogenation tank under stirring, stir and react for 30min at a temperature of 25°C and a rotation speed of 35r / min, and stand for 25min after completion of the reaction to obtain a lithium bicarbonate solution;

[0064] S3, slowly adding the tetrafluoroboric acid solution to the lithium bicarbonate solution under stirring, stirring and reacting for 2.5 hours at a temperature of 23° C. and a rotation speed of 5 r / min. After the reaction is completed, standing at 15° C. for 14 hours to obtain a lithium tetrafluoroborate solution, wherein the molar ratio of tetrafluoroboric acid to lithium bicarbonate is 1.01:1;

[0065] S4. The lithium tetrafluoroborate solution is evaporated at 15°C, and the crystals are collected after evaporation. 70 g of the crystals are dissolved in 600 mL of anhydrous ethanol, and low-temperature distilled at 35°C. After the distillation is completed, the crystals are collected to obtain.

[0066] After testing, the purity of the product obtained above was 99.7%.

[0067] In Comparative Example 1, lithium carbonate reacts directly with lithium tetrafluoroborate, and impurities in solid lithium carbonate are directly introduced into the lithium tetrafluoroborate product, which is an interfering phase for crystal growth in the subsequent crystallization process, resulting in low product purity, relatively low crystal purity, and relatively poor electrical properties.

[0068] In Comparative Example 2, the temperature during the evaporation and crystallization of lithium tetrafluoroborate solution was too high, the water volatilized quickly, the crystal nuclei were generated and grew rapidly, and a large number of impurity ions could not be discharged into the solution and removed smoothly, but grew together with the crystals, resulting in a high impurity content in the final product lithium tetrafluoroborate crystals and relatively poor electrical properties.

[0069] In Comparative Example 3, calcium hydride was not added to the anhydrous ethanol to remove water, resulting in the inability to remove trace amounts of water molecules in the anhydrous ethanol. During the crystallization process of lithium tetrafluoroborate, these water molecules would be mixed into the lithium tetrafluoroborate crystals, affecting the purity of the crystals and resulting in relatively poor electrochemical performance.

[0070] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for synthesizing lithium tetrafluoroborate, characterized in that: The following steps are involved: S1. Slowly add boron oxide to the hydrofluoric acid solution under stirring to fully react. After the reaction is completed, let it stand for 3-6.5 hours to obtain a tetrafluoroboric acid solution; S2. Evenly mix lithium carbonate powder and deionized water in a hydrogenation device, introduce CO2 gas, carry out hydrogenation reaction under stirring, and stand for 25-30 minutes after the reaction is completed to obtain a lithium bicarbonate solution; S3, slowly adding the tetrafluoroboric acid solution to the lithium bicarbonate solution under stirring to fully react, and after the reaction is completed, standing at 15-33° C. for 14-16 hours to obtain a lithium tetrafluoroborate solution; S4, subjecting the lithium tetrafluoroborate solution to low-temperature evaporation at 15-33°C, collecting crystals after evaporation, dissolving the crystals in a low-boiling point organic solvent, adding an appropriate amount of calcium hydride to remove trace moisture, and then subjecting the solution to low-temperature fractionation at 35-63°C, collecting crystals after fractionation, to obtain; the low-boiling point organic solvent is at least one of anhydrous ethanol and anhydrous ether.

2. The method for synthesizing lithium tetrafluoroborate according to claim 1, characterized in that: The molar ratio of boric oxide to hydrofluoric acid is 1:(8-8.15).

3. The method for synthesizing lithium tetrafluoroborate according to claim 1, characterized in that: The purity of the boron oxide is ≥99.9%; the concentration of the hydrofluoric acid solution is 22.5 mol / L.

4. The method for synthesizing lithium tetrafluoroborate according to claim 1, characterized in that: In S1, the reaction conditions are: stirring the reaction at 23-28°C for 30-45 minutes; in S1, the standing temperature is 23-28°C.

5. The method for synthesizing lithium tetrafluoroborate according to claim 1, characterized in that: The purity of the lithium carbonate micropowder is ≥99.9% and the particle size is 5-25 μm.

6. The method for synthesizing lithium tetrafluoroborate according to claim 1, characterized in that: In S2, the temperature of the hydrogenation reaction is 25-28°C and the time is 30-45 minutes.

7. The method for synthesizing lithium tetrafluoroborate according to claim 1, characterized in that: In S3, the molar ratio of tetrafluoroboric acid to lithium bicarbonate is 1.01-1.05:

1.

8. The method for synthesizing lithium tetrafluoroborate according to claim 1, characterized in that: In S3, the reaction conditions are: stirring the reaction at 23-28°C for 2.5-3h.

Citation Information

Patent Citations

  • Preparation method for lithium tetrafluoroborate

    CN103236562A

  • Method for preparing anhydrous lithium tetrafluoroborate

    CN103466650A

  • Preparation method of low moisture lithium tetrafluoroborate

    CN104528752A

  • Method for synthesizing lithium tetrafluoroborate by rheological phase method

    CN107585776A

  • Synthesis method of lithium tetrafluoroborate

    CN115196646A