A gas separation membrane, preparation method and application in carbon dioxide capture
By preparing polyols, hydroxylated ionic liquids, and modified polyionic liquids, and combining them with ultraporous MOF materials and composite additives, a gas separation membrane with high porosity is formed, solving the trade-off between selectivity and permeability in existing technologies and achieving efficient carbon dioxide capture.
Patent Information
- Application Number
- CN202411304601.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-19
AI Technical Summary
Existing organic membrane materials involve a trade-off between selectivity and permeability in gas separation processes, making it difficult to simultaneously improve both the selectivity and permeability of gas separation membranes.
Intermediate product A was prepared by reacting allyl glycidyl ether with bis(2-mercaptoethyl) ether, and then reacted with allyl borate pinacol ester and 2,6-diaminopyridine to form a polyol. Subsequently, a hydroxylated ionic liquid was formed with 3-chloro-1,2-propanediol and N-methylimidazole. Finally, a gas separation membrane was prepared with the modified polyionic liquid and composite additives. The porous composite structure and silver ions enhanced the affinity and permeability of carbon dioxide.
It improves the permeability and selectivity of the gas separation membrane for carbon dioxide, enhances its resistance to organic fouling, and extends the membrane's lifespan and separation efficiency.
Smart Images

Figure CN118807485B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of membrane separation technology, and in particular to a gas separation membrane, a preparation method and application in carbon dioxide capture. Background Art
[0002] With the acceleration of the world's industrialization process, the emission of greenhouse gases such as carbon dioxide continues to rise. The emission of carbon dioxide has caused serious environmental and ecological problems. As one of the ways to reduce carbon emissions, the capture of carbon dioxide has attracted widespread attention from countries around the world in recent years. At present, the methods used for carbon dioxide capture and separation mainly include absorption, cryogenic separation, adsorption and membrane separation. As an emerging carbon dioxide separation and enrichment technology, membrane separation has the advantages of low operating cost, no use of solvents, and small footprint. It has become one of the future development directions of carbon dioxide capture technology. Membrane materials are the basis of membrane separation technology, and their performance directly affects the application prospects of membrane separation technology. Gas separation membranes can be divided into inorganic membranes and organic membranes. Commonly used organic membrane materials include cellulose, polyamide, polysulfone, polyether, etc. However, commercial organic membranes are severely limited by the trade-off between selectivity and permeability. How to improve selectivity while ensuring the permeability of gas separation membranes is an important topic in gas separation membrane research. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a method for preparing a gas separation membrane, comprising the following steps:
[0004] Step (1), reacting allyl glycidyl ether with bis(2-mercaptoethyl) ether to obtain an intermediate product A; reacting the intermediate product A with allyl boronic acid pinacol ester to obtain an intermediate product B;
[0005] Step (2), reacting the intermediate product B with 2,6-diaminopyridine to obtain an intermediate product C; reacting the intermediate product C and D-glucosamine with terephthalaldehyde as a crosslinking agent to obtain a polyol;
[0006] Step (3), using 3-chloro-1,2-propanediol and N-methylimidazole as raw materials, reacting to obtain a hydroxylated ionic liquid;
[0007] Polyol, hydroxylated ionic liquid, isophorone diisocyanate and dimethylol propionic acid are used as raw materials to obtain a polyionic liquid dispersion through reaction;
[0008] Step (4), after the polyionic liquid dispersion is diluted, silver tetrafluoroborate and aluminum nitrate are added to obtain a modified polyionic liquid dispersion; a composite additive is added to the modified polyionic liquid dispersion to obtain a membrane raw material mixed solution, the membrane raw material mixed solution is coated on a glass plate, and evaporated to obtain a gas separation membrane;
[0009] Wherein, the preparation method of the composite additive comprises the following steps:
[0010] Step S1, using 1,4-diazabicyclo[2.2.2]octane, 2-aminoterephthalic acid, and zinc nitrate hexahydrate as raw materials to prepare an ultra-microporous MOF material;
[0011] Step S2, after the reaction of (R)-piperazine-2-carboxylic acid and cyanuric chloride, the ultra-microporous MOF material is grafted to obtain a porous composite material;
[0012] Step S3, modifying the porous composite material with thionyl chloride to obtain a modified porous composite material; reacting the modified porous composite material with pentaethylenehexamine to obtain a composite additive.
[0013] Preferably, in step (1), the method for preparing the intermediate product B comprises the following steps:
[0014] Mix allyl glycidyl ether and bis(2-mercaptoethyl) ether, stir at room temperature at a speed of 200-400 r / min for 3-5 hours, and purify to obtain intermediate product A; wherein the mass ratio of allyl glycidyl ether to bis(2-mercaptoethyl) ether is (3-6):(11.2-22.4);
[0015] The intermediate product A is added to tetrahydrofuran, stirred for 10-20 minutes, heated to 50-60°C, and then allyl boric acid pinacol ester and azobisisobutyronitrile are added, the temperature is kept constant, and the reaction is stirred at a speed of 200-400r / min for 1-3h. After the reaction is completed, the intermediate product B is obtained by vacuum distillation; wherein the mass ratio of the intermediate product A, tetrahydrofuran, allyl boric acid pinacol ester and azobisisobutyronitrile is (2.5-5):(20-50):(1.6-3.2):(0.02-0.05);
[0016] In the above process, the carbon-carbon double bond of allyl glycidyl ether undergoes a thiol-ene click reaction with the thiol group at one end of bis(2-mercaptoethyl) ether to obtain an intermediate product A containing an epoxy group and a thiol group; the thiol group of the intermediate product A is also combined with the carbon-carbon double bond of allyl boronic acid pinacol ester through a thiol-ene click reaction to obtain an intermediate product B containing an epoxy group and a boronic acid pinacol ester group.
[0017] Preferably, in step (2), the method for preparing the polyol comprises the following steps:
[0018] The intermediate product B is added to methanol, ultrasonically treated for 20-40 minutes, and then 2,6-diaminopyridine is added. The mixture is stirred at 70-90°C and 200-400 r / min for 20-30 hours. After the reaction is completed, the mixture is cooled to room temperature and evaporated to obtain an intermediate product C; wherein the mass ratio of the intermediate product B, methanol, and 2,6-diaminopyridine is (2.8-5.6):(50-90):(0.7-1.4);
[0019] The intermediate products C and D-glucosamine are added to ethanol at a temperature of 40-50°C, and ultrasonic treatment is performed for 10-30 minutes to obtain a mixed solution; terephthalaldehyde is dissolved in ethanol, and then added to the mixed solution, and stirred at 60-70°C for 2-4 hours. After the reaction is completed, the polyol is obtained by distillation under reduced pressure; wherein the mass ratio of the intermediate product C, D-glucosamine, and terephthalaldehyde is (2.5-5):(0.9-1.8):(0.6-1.2);
[0020] In the above process, the epoxy group of the intermediate product B reacts with the amino group of 2,6-diaminopyridine to obtain an intermediate product C containing a hydroxyl group, a pyridine group, an amino group and a pinacol borate group; further, terephthalaldehyde is used as a cross-linking agent, and its two aldehyde groups react with D-glucosamine and the amino group of the intermediate product C respectively to form a polyol with a long-chain structure, in which there are multiple hydroxyl groups, pyridine groups and pinacol borate groups.
[0021] Preferably, in step (3), the method for preparing the hydroxylated ionic liquid comprises the following steps:
[0022] In a glycerol bath at a temperature of 65-75°C, maintaining a stirring speed of 200-400 r / min, adding 3-chloro-1,2-propylene glycol to N-methylimidazole within 40-80 minutes, maintaining the temperature unchanged, stirring and reacting for 70-80 hours, after the reaction is completed, removing the reaction mixture from the glycerol bath, washing with ethyl acetate 5-9 times, and vacuum drying to obtain a hydroxylated ionic liquid; wherein the mass ratio of 3-chloro-1,2-propylene glycol to N-methylimidazole is (13.2-26.4):(12-24);
[0023] Preferably, in step (3), the method for preparing the polyionic liquid dispersion comprises the following steps:
[0024] Under constant stirring conditions at a speed of 200-400 r / min, add polyol to methyl ethyl ketone, stir for 10-20 min, add hydroxylated ionic liquid, stir for 20-40 min, then add dibutyltin dilaurate and isophorone diisocyanate, react at 65-75° C. for 2-3 h, then add dimethylolpropionic acid, react at 65-75° C. for 2-3 h, and obtain a polyionic liquid dispersion; wherein the mass ratio of polyol, methyl ethyl ketone, hydroxylated ionic liquid, dibutyltin dilaurate, isophorone diisocyanate, and dimethylolpropionic acid is (3.1-6.2):(50-80):(0.7-1.4):(0.03-0.05):(2.2-4.4):(0.2-0.5);
[0025] In the above process, under the catalytic action of dibutyltin dilaurate, polyol, methyl ethyl ketone and hydroxylated ionic liquid are polymerized to form a prepolymer, and then dimethylol propionic acid is used as a hydrophilic chain extender to extend the chain to obtain a polyionic liquid containing a polyurethane chain.
[0026] Preferably, in the step (4), the preparation method of the modified polyionic liquid dispersion is as follows: at a temperature of 40-50° C. and a stirring speed of 150-250 r / min, the polyionic liquid dispersion is diluted with methyl ethyl ketone to obtain a 2-5 wt% polyionic liquid dilution; silver tetrafluoroborate is first added to the polyionic liquid dilution, and stirred at a speed of 100-200 r / min for 10-20 min, and then aluminum nitrate is added, and stirring is continued for 10-20 min to obtain a modified polyionic liquid dispersion, wherein the mass ratio of the polyionic liquid, silver tetrafluoroborate, and aluminum nitrate is 1:(0.08-0.15):(0.01-0.03);
[0027] In the above process, the hydroxyl groups in the polyurethane chain of the polyionic liquid combine with the silver ions in silver tetrafluoroborate to introduce the silver ions into the polyionic liquid. Further, aluminum nitrate is added and the aluminum salt wraps up the silver ions.
[0028] Preferably, in step (4), the thickness of the gas separation membrane is 150-250 µm; the content of the composite additive in the raw material mixture is 5-20 wt %; and the evaporation conditions are: evaporation at room temperature for 4-6 days.
[0029] Furthermore, in step (4), the preparation method of the composite additive comprises the following steps:
[0030] Step S1, adding 1,4-diazabicyclo[2.2.2]octane, 2-aminoterephthalic acid, and zinc nitrate hexahydrate to dimethyl sulfoxide, ultrasonically dispersing for 20-40 minutes, adding N,N-dimethylformamide, stirring, and then adding deionized water, sealing, reacting at 100-110° C. for 70-80 hours to form crystals, cooling, placing the crystals in methanol and standing for 5-7 hours, taking them out, washing them with methanol 2-3 times, and then soaking them in methanol for 10-30 hours, filtering, and obtaining an ultra-microporous MOF material; wherein the mass ratio of 1,4-diazabicyclo[2.2.2]octane, 2-aminoterephthalic acid, and zinc nitrate hexahydrate is (0.1-0.2):(2.7-5.4):(1-2);
[0031] In the above process, using 1,4-diazabicyclo[2.2.2]octane, 2-aminoterephthalic acid, and zinc nitrate hexahydrate as raw materials, an ultra-microporous MOF material can be obtained, the pore size of which can accommodate carbon dioxide, but will block nitrogen or methane gas, and show high selectivity for carbon dioxide through size exclusion behavior;
[0032] Step S2, at 3-7°C, add N,N-diisopropylethylamine and (R)-piperazine-2-carboxylic acid to 1,4-dioxane to obtain a reaction solution; in a nitrogen atmosphere, at 3-7°C, while stirring, drip cyanuric chloride into 1,4-dioxane at a rate of 0.5-0.8 mL / min, then add the above reaction solution, first stir the reaction at 12-18°C for 1.5-2.5 h, then stir the reaction at 22-28°C 1.5-2.5h, then add the ultra-microporous MOF material, stir and react at 80-90°C for 20-30h, after the reaction is completed, precipitate the product with ethanol, collect and dry the precipitate to obtain a porous composite material; wherein the mass ratio of N,N-diisopropylethylamine, (R)-piperazine-2-carboxylic acid, cyanuric chloride and ultra-microporous MOF material is (7-14):(1.9-3.8):(2.5-5):(1.9-3.8);
[0033] In the above process, the acyl chloride of cyanuric chloride first reacts with the NH of (R)-piperazine-2-carboxylic acid and polymerizes, and then reacts with the amino group of the ultra-microporous MOF material to form a porous covalent organic skeleton on the surface of the ultra-microporous MOF material, thereby forming a porous composite structure with higher porosity.
[0034] Step S3, dispersing the porous composite material in thionyl chloride, then adding N,N-dimethylformamide, heating to 50-70°C and maintaining for 20-30 hours, and heating to 85-95°C after the reaction is completed to obtain a modified porous composite material; wherein the mass ratio of the porous composite material, thionyl chloride, and N,N-dimethylformamide is (1-3):(300-500):(4.8-9.6);
[0035] Add pentaethylenehexamine to N,N-dimethylformamide, then add the modified porous composite material, heat to 80-100°C and stir to react for 20-30h. After the reaction is completed, collect the precipitate, wash it, and dry it to obtain a composite additive; wherein the mass ratio of pentaethylenehexamine, N,N-dimethylformamide, and the modified porous composite material is (5-10):(20-40):(1-3);
[0036] In the above process, the carboxyl group in the porous composite material reacts with the acyl chloride of thionyl chloride to introduce the acyl chloride into the porous composite material, and then reacts with the amino group of pentaethylenehexamine to graft the pentaethylenehexamine onto the porous composite material to form a composite additive.
[0037] The invention also discloses a gas separation membrane prepared by adopting the gas separation membrane preparation method.
[0038] A gas separation membrane as described above is applied to carbon dioxide capture.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] 1. The present invention uses polyol, methyl ethyl ketone and hydroxylated ionic liquid to polymerize to form a prepolymer, and then uses dimethylol propionic acid as a hydrophilic chain extender to extend the chain to obtain a polyionic liquid; wherein, the long chain structure of the polyol contains multiple hydroxyl groups, pyridine groups (hydrophilic groups) and pinacol ester groups, and the pyridine groups with Lewis basicity can interact with Lewis acidic carbon dioxide to promote the combination of the two; the boric acid pinacol ester group has a strong affinity for carbon dioxide, and due to the large volume of the boric acid pinacol ester group, pores are formed in the membrane during the film formation process; the hydroxylated ionic liquid also has an affinity for carbon dioxide, which can promote the diffusion and solvent of carbon dioxide, so that the gas separation membrane prepared with the polyionic liquid of the present invention as a membrane matrix has good permeability and selectivity to carbon dioxide, and due to the presence of hydrophilic groups in its polyurethane chain, the gas separation membrane has a certain resistance to organic pollution; dimethylol propionic acid is used as a hydrophilic chain extender, which can make the gas separation membrane have better resistance to organic pollution, improve the separation efficiency of the membrane, and extend the life of the membrane;
[0041] Furthermore, silver ions are introduced into the polyionic liquid through silver tetrafluoroborate. The empty s orbital of the silver ion enhances its interaction with carbon dioxide, thereby improving the solubility and selectivity of carbon dioxide. Aluminum nitrate is then added, and the aluminum salt wraps up the silver ions, stabilizing them and maximizing the interaction between the empty s orbital and carbon dioxide, allowing the silver ions to exist stably for a long time, thereby further improving the membrane permeability and selectivity.
[0042] 2. The present invention grafts a porous covalent organic skeleton on the surface of an ultra-microporous MOF material to form a porous composite structure with a higher porosity, then grafts pentaethylenehexamine on the porous composite material to form a composite additive, and then adds the composite additive to a modified polyionic liquid dispersion to obtain a membrane raw material mixed solution. The porous structure of the composite additive helps to improve the permeability of the gas separation membrane. The multiple amino groups in pentaethylenehexamine have an affinity for carbon dioxide, which cooperates with the size exclusion effect of the ultra-microporous MOF material to improve the performance of the gas separation membrane; and the introduction of the amino group of pentaethylenehexamine improves the hydrophilicity of the composite additive, thereby improving the anti-organic pollution performance of the gas separation membrane; further, compared with the ultra-microporous MOF material, the covalent organic skeleton has better interfacial compatibility with the modified polyionic liquid, and the introduction of a large number of amino groups in pentaethylenehexamine allows the composite additive to form hydrogen bonds with groups such as hydroxyl and carboxyl groups (introduced by dimethylol propionic acid) in the modified polyionic liquid, and the electrostatic interaction between the carboxyl group and the amino group improves the dispersibility of the composite additive in the gas separation membrane, thereby improving the performance of the gas separation membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 is a process flow chart of a method for preparing a gas separation membrane of the present invention;
[0044] Figure 2 It is a schematic diagram of the synthesis of the intermediate product C of the present invention;
[0045] Figure 3 is a schematic structural diagram of the hydroxylated ionic liquid of the present invention;
[0046] Figure 4 is a schematic diagram of the synthesis of the porous composite material of the present invention;
[0047] Figure 5 It is a comparison chart of CO2 permeability test of gas separation membranes of Example 2-4 of the present invention and Comparative Example 2-8;
[0048] Figure 6 It is a comparison chart of CO2 / N2 selectivity test of the gas separation membranes of Examples 2-4 of the present invention and Comparative Examples 2-8. DETAILED DESCRIPTION
[0049] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0050] Embodiment 1: This embodiment discloses a method for preparing a composite additive, comprising the following steps:
[0051] Step S1, adding 0.15g 1,4-diazabicyclo[2.2.2]octane, 4g 2-aminoterephthalic acid, and 1.5g zinc nitrate hexahydrate to 150g dimethyl sulfoxide, ultrasonically dispersing for 30min, adding 16.5g N,N-dimethylformamide, stirring, and then adding 42g deionized water, sealing, reacting at 105°C for 75h to form crystals, cooling, placing the crystals in 120g methanol and standing for 6h, taking them out, washing them with methanol 3 times, and then soaking them in 240g methanol for 20h, filtering, and obtaining ultra-microporous MOF materials;
[0052] Step S2, at 5°C, add 10.5g N,N-diisopropylethylamine and 2.7g (R)-piperazine-2-carboxylic acid to 115g 1,4-dioxane to obtain a reaction solution; in a nitrogen atmosphere, at 5°C, while stirring, dropwise add 3.8g cyanuric chloride to 38g 1,4-dioxane at a rate of 0.7mL / min, then add the above reaction solution, stir and react at 15°C for 2h, then stir and react at 25°C for 2h, then add 2.9g ultra-microporous MOF material, stir and react at 85°C for 25h, after the reaction is completed, precipitate the product with ethanol, collect the precipitate and vacuum dry it at 75°C to obtain a porous composite material;
[0053] Step S3, dispersing 2 g of the porous composite material in 400 g of thionyl chloride, then adding 7.1 g of N,N-dimethylformamide, heating to 60° C. and maintaining for 25 h, and after the reaction is completed, heating to 90° C. to remove excess thionyl chloride, to obtain a modified porous composite material;
[0054] 7.5 g of pentaethylenehexamine was added to 30 g of N,N-dimethylformamide, and then 2 g of the modified porous composite material was added, heated to 90°C and stirred for reaction for 25 hours. After the reaction was completed, the precipitate was collected, washed with deionized water 4 times, and dried at 60°C for 8 hours to obtain a composite additive.
[0055] Example 2: This example discloses a method for preparing a gas separation membrane, comprising the following steps:
[0056] Step (1), 3 g of allyl glycidyl ether and 11.2 g of bis(2-mercaptoethyl) ether were mixed, stirred at room temperature at a speed of 200 r / min for 5 h, and then purified by silica gel flash column chromatography (eluent was obtained by mixing ethyl acetate / heptane in a volume ratio of 1:2), i.e., intermediate product A;
[0057] 2.5 g of intermediate product A was added to 20 g, stirred for 10 min, heated to 50°C, and then 1.6 g of allyl boric acid pinacol ester and 0.02 g of azobisisobutyronitrile were added. The temperature was kept constant and stirred at a speed of 200 r / min for 3 h. After the reaction was completed, the solvent was removed by reduced pressure distillation at 40°C to obtain intermediate product B;
[0058] Step (2), adding 2.8 g of intermediate product B to 50 g of methanol, ultrasonically treating for 20 min, then adding 0.7 g of 2,6-diaminopyridine, stirring at 70° C. and 200 r / min for 30 h, after the reaction is completed, cooling to room temperature, and evaporating the solvent at 40° C. to obtain intermediate product C;
[0059] 2.5 g of intermediate product C and 0.9 g of D-glucosamine were added to 40 g of ethanol at 40°C, and ultrasonically treated for 10 min to obtain a mixed solution; 0.6 g of terephthalaldehyde was dissolved in 20-30 g of ethanol, and then added to the mixed solution, stirred and reacted at 60°C for 4 h. After the reaction was completed, the solvent was removed by reduced pressure distillation at 60°C to obtain a polyol;
[0060] Step (3), in a glycerol bath at a temperature of 65°C, maintaining a stirring speed of 200 r / min, adding 13.2 g of 3-chloro-1,2-propanediol to 12 g of N-methylimidazole within 40 minutes, maintaining the temperature unchanged, stirring and reacting for 70 hours. After the reaction is completed, the reaction mixture is removed from the glycerol bath, washed with ethyl acetate 5 times, and then vacuum dried at 65°C for 20 hours to obtain a hydroxylated ionic liquid;
[0061] Under constant stirring conditions at a speed of 200 r / min, 3.1 g of polyol was added to 50 g of methyl ethyl ketone, stirred for 10 min, 0.7 g of hydroxylated ionic liquid was added, stirred for 20 min, 0.03 g of dibutyltin dilaurate and 2.2 g of isophorone diisocyanate were added, and the mixture was reacted at 65° C. for 3 h, and then 0.2 g of dihydroxymethylpropionic acid was added, and the mixture was reacted at 65° C. for 3 h to obtain a polyionic liquid dispersion;
[0062] Step (4), diluting the polyionic liquid dispersion with methyl ethyl ketone to obtain a 2 wt% polyionic liquid dilution at a temperature of 40° C. and a stirring speed of 150 r / min; first adding silver tetrafluoroborate to the polyionic liquid dilution, stirring at a speed of 100 r / min for 10 min, then adding aluminum nitrate, and continuing to stir for 10 min to obtain a modified polyionic liquid dispersion, wherein the mass ratio of polyionic liquid, silver tetrafluoroborate, and aluminum nitrate is 1:0.08:0.01;
[0063] A composite additive is added to the modified polyionic liquid dispersion to obtain a membrane raw material mixed solution, the membrane raw material mixed solution is coated on a glass plate, and the solvent is evaporated at room temperature for 4 days to obtain a gas separation membrane with a thickness of 200µm; wherein the content of the composite additive in the membrane raw material mixed solution is 5wt%.
[0064] Example 3: This example discloses a method for preparing a gas separation membrane, comprising the following steps:
[0065] Step (1), 6 g of allyl glycidyl ether and 22.4 g of bis(2-mercaptoethyl) ether were mixed, stirred at room temperature at a speed of 400 r / min for 3 h, and then purified by silica gel flash column chromatography (eluent was obtained by mixing ethyl acetate / heptane in a volume ratio of 1:2), i.e., intermediate product A;
[0066] 5 g of intermediate product A was added to 50 g of tetrahydrofuran, stirred for 10 min, heated to 60°C, and then 3.2 g of allylboronic acid pinacol ester and 0.05 g of azobisisobutyronitrile were added. The temperature was kept constant and stirred at a speed of 400 r / min for 1 h. After the reaction was completed, the solvent was removed by distillation under reduced pressure at 50°C to obtain intermediate product B;
[0067] Step (2), adding 5.6 g of intermediate product B to 90 g of methanol, ultrasonically treating for 40 min, then adding 1.4 g of 2,6-diaminopyridine, stirring at 90° C. and 400 r / min for 20 h, after the reaction is completed, cooling to room temperature, and evaporating the solvent at 60° C. to obtain intermediate product C;
[0068] 5 g of intermediate product C and 1.8 g of D-glucosamine were added to 60 g of ethanol at 50°C, and ultrasonically treated for 30 min to obtain a mixed solution; 1.2 g of terephthalaldehyde was dissolved in 30 g of ethanol, and then added to the mixed solution, stirred and reacted at 70°C for 2 h. After the reaction was completed, the solvent was removed by reduced pressure distillation at 80°C to obtain a polyol;
[0069] Step (3), in a glycerol bath at a temperature of 75°C, maintaining a stirring speed of 400 r / min, adding 26.4 g of 3-chloro-1,2-propanediol to 24 g of N-methylimidazole within 80 minutes, maintaining the temperature unchanged, stirring and reacting for 80 hours. After the reaction is completed, the reaction mixture is removed from the glycerol bath, washed with ethyl acetate for 9 times, and then vacuum dried at 75°C for 20 hours to obtain a hydroxylated ionic liquid;
[0070] Under constant stirring conditions at a speed of 400 r / min, 6.2 g of polyol was added to 80 g of methyl ethyl ketone, stirred for 20 min, 1.4 g of hydroxylated ionic liquid was added, stirred for 40 min, 0.05 g of dibutyltin dilaurate and 4.4 g of isophorone diisocyanate were added, reacted at 75° C. for 2 h, and then 0.5 g of dihydroxymethylpropionic acid was added, reacted at 75° C. for 2 h to obtain a polyionic liquid dispersion;
[0071] Step (4), diluting the polyionic liquid dispersion with methyl ethyl ketone to obtain a 5 wt% polyionic liquid dilution at a temperature of 50° C. and a stirring speed of 250 r / min; first adding silver tetrafluoroborate to the polyionic liquid dilution, stirring at a speed of 200 r / min for 10 min, then adding aluminum nitrate, and continuing to stir for 20 min to obtain a modified polyionic liquid dispersion, wherein the mass ratio of polyionic liquid, silver tetrafluoroborate, and aluminum nitrate is 1:0.15:0.03;
[0072] A composite additive is added to the modified polyionic liquid dispersion to obtain a membrane raw material mixed solution, the membrane raw material mixed solution is coated on a glass plate, and the solvent is evaporated at room temperature for 6 days to obtain a gas separation membrane with a thickness of 200µm; wherein the content of the composite additive in the membrane raw material mixed solution is 20wt%.
[0073] Example 4: This example discloses a method for preparing a gas separation membrane, comprising the following steps:
[0074] Step (1), 4.5 g of allyl glycidyl ether and 16.8 g of bis(2-mercaptoethyl) ether were mixed, stirred at room temperature at a speed of 300 r / min for 4 h, and then purified by silica gel flash column chromatography (eluent was obtained by mixing ethyl acetate / heptane in a volume ratio of 1:2), i.e., intermediate A;
[0075] 3.8 g of intermediate product A was added to 35 g of tetrahydrofuran, stirred for 15 min, heated to 55° C., and then 2.4 g of allylboronic acid pinacol ester and 0.03 g of azobisisobutyronitrile were added. The temperature was kept constant and stirred at a speed of 300 r / min for 2 h. After the reaction was completed, the solvent was removed by reduced pressure distillation at 45° C. to obtain intermediate product B;
[0076] Step (2), adding 4.2 g of intermediate product B to 70 g of methanol, ultrasonically treating for 30 min, then adding 1.1 g of 2,6-diaminopyridine, stirring at 80° C. and 300 r / min for 25 h, after the reaction is completed, cooling to room temperature, and evaporating the solvent at 40-60° C. to obtain intermediate product C;
[0077] 3.8 g of intermediate product C and 1.4 g of D-glucosamine were added to 50 g of ethanol at 45°C, and ultrasonically treated for 20 min to obtain a mixed solution; 0.9 g of terephthalaldehyde was dissolved in 25 g of ethanol, and then added to the mixed solution, and stirred at 65°C for 3 h. After the reaction was completed, the solvent was removed by reduced pressure distillation at 70°C to obtain a polyol;
[0078] Step (3), in a glycerol bath at a temperature of 70°C, maintaining a stirring speed of 300 r / min, adding 19.8 g of 3-chloro-1,2-propanediol to 18 g of N-methylimidazole within 60 minutes, maintaining the temperature unchanged, stirring and reacting for 75 hours. After the reaction is completed, the reaction mixture is removed from the glycerol bath, washed with ethyl acetate 7 times, and then vacuum dried at 70°C for 25 hours to obtain a hydroxylated ionic liquid;
[0079] Under constant stirring conditions of a rotation speed of 300 r / min, 4.7 g of polyol was added to 65 g of methyl ethyl ketone, stirred for 15 min, 1.1 g of hydroxylated ionic liquid was added, stirred for 30 min, 0.04 g of dibutyltin dilaurate and 3.3 g of isophorone diisocyanate were added, and the mixture was reacted at 70° C. for 2.5 h, and then 0.4 g of dihydroxymethylpropionic acid was added, and the mixture was reacted at 70° C. for 2.5 h to obtain a polyionic liquid dispersion;
[0080] Step (4), diluting the polyionic liquid dispersion with methyl ethyl ketone to obtain a 3.5 wt% polyionic liquid dilution at a temperature of 45° C. and a stirring speed of 200 r / min; first adding silver tetrafluoroborate to the polyionic liquid dilution, stirring at a speed of 150 r / min for 15 minutes, then adding aluminum nitrate, and continuing to stir for 15 minutes to obtain a modified polyionic liquid dispersion, wherein the mass ratio of polyionic liquid, silver tetrafluoroborate, and aluminum nitrate is 1:0.12:0.02;
[0081] A composite additive was added to the modified polyionic liquid dispersion to obtain a membrane raw material mixed solution, the membrane raw material mixed solution was coated on a glass plate, and the solvent was evaporated at room temperature for 5 days to obtain a gas separation membrane with a thickness of 200µm; wherein the content of the composite additive in the membrane raw material mixed solution was 12.5wt%.
[0082] The composite additives in the above Examples 2-4 are the composite additives prepared in Example 1.
[0083] Comparative Example 1
[0084] Comparative Example 1 Compared with Example 1, in Comparative Example 1, during the preparation of the porous composite material, no ultra-microporous MOF material was added, and other conditions remained unchanged.
[0085] Comparative Example 2
[0086] Comparative Example 2 Compared with Example 4, Comparative Example 2 uses the composite additive prepared in Comparative Example 1, and other conditions remain unchanged.
[0087] Comparative Example 3
[0088] Comparative Example 3 Compared with Example 4, in the process of preparing the gas separation membrane in Comparative Example 3, the porous composite material is used instead of the composite additive, and other conditions remain unchanged.
[0089] Comparative Example 4
[0090] Comparative Example 4 Compared with Example 4, in the process of preparing the gas separation membrane in Comparative Example 4, the ultra-microporous MOF material is used instead of the composite additive, and other conditions remain unchanged.
[0091] Comparative Example 5
[0092] Compared with Example 4, in Comparative Example 5, in the process of preparing intermediate product C, intermediate product A is used instead of intermediate product B, and other conditions remain unchanged.
[0093] Comparative Example 6
[0094] Comparative Example 6 Compared with Example 4, in the process of preparing the polyionic liquid dispersion, no hydroxylated ionic liquid was added in Comparative Example 6, and other conditions remained unchanged.
[0095] Comparative Example 7
[0096] Comparative Example 7 Compared with Example 4, in the process of preparing the modified polyionic liquid dispersion in Comparative Example 7, no silver tetrafluoroborate was added, and other conditions remained unchanged.
[0097] Comparative Example 8
[0098] Comparative Example 8 Compared with Example 4, in the process of preparing the modified polyionic liquid dispersion in Comparative Example 8, no aluminum nitrate was added, and other conditions remained unchanged.
[0099] Experimental Example: The performance of the gas separation membranes of Examples 2-4 and Comparative Examples 2-8 was tested.
[0100] The mixed gas separation performance was tested by a constant pressure variable volume (CPVV) device. A CO2 / N2 (20 / 80 vol%) mixed gas was used to simulate the composition of flue gas or natural gas. A pure N2 flow was used as an upstream sweep gas (20 SCCM) to eliminate the concentration polarization effect, and the feed pressure for all tests was maintained at 2 bar. The downstream permeate composition was analyzed by a gas chromatograph (Shimadzu GC-2030). In order to accurately evaluate the separation performance, each test took at least 1 hour to reach a steady state, and all membrane tests were repeated three times.
[0101] The permeability is calculated by the following formula:
[0102] Among them, P i is the gas permeability (1Barrer=10 -10 cm 3 (STP)cm / cm -2 s -1 cmHg), Q i is the volume flow rate (cm 3 s -1 , STP), L is the membrane thickness (cm), A is the membrane effective area (cm 2 ), Δp i is the pressure difference between upstream and downstream of the membrane (cmHg).
[0103] The formula for calculating the selectivity of mixed gas is:
[0104] where x i / x j and i / y j are the volume fractions of feed gas and permeate gas, respectively. For the permeation tests at different pressures, all other conditions were kept constant except the upstream pressure (ranging from 2 to 50 bar).
[0105] The test results are shown in Table 1:
[0106] Table 1
[0107] <![CDATA[CO2 Permeability / barrer]]> <![CDATA[CO2 / N2 selectivity]]> Example 2 9840.22 65.26 Example 3 9968.41 67.39 Example 4 9889.83 66.54 Comparative Example 2 9587.27 63.27 Comparative Example 3 9807.29 64.32 Comparative Example 4 9597.76 61.38 Comparative Example 5 9626.14 62.11 Comparative Example 6 9573.59 60.61 Comparative Example 7 9764.32 63.88 Comparative Example 8 9827.54 65.07
[0108] It can be seen from the test results in Table 1 that the gas separation membranes prepared in Examples 2-4 of the present invention have excellent permeability and selectivity for carbon dioxide. From the comparison between Comparative Example 2 and Example 4, it can be seen that the ultra-microporous MOF material improves the permeability and selectivity of the gas separation membrane through its own porous structure and size exclusion effect; from the comparison between Comparative Example 3 and Example 4, it can be seen that the multiple amino groups in pentaethylenehexamine have affinity for carbon dioxide, thereby improving the performance of the gas separation membrane; from the comparison between Comparative Example 4 and Example 4, it can be seen that the grafting of covalent organic skeletons and pentaethylenehexamine on the ultra-microporous MOF material improves the permeability and selectivity of the gas separation membrane by increasing the porosity, increasing the amino groups and improving the dispersibility of the composite additives in the gas separation membrane; from the comparison between Comparative Example 5 and Example 4, it can be seen that the boric acid pinacol ester group has a strong affinity for carbon dioxide, and Due to the large volume of the pinacol borate ester group, pores are formed in the membrane during the film formation process, which has a positive effect on the performance improvement of the gas separation membrane; from the comparison between Comparative Example 6 and Example 4, it can be seen that the hydroxylated ionic liquid also has an affinity for carbon dioxide, can promote the diffusion and solvent of carbon dioxide, and thus can improve the performance of the gas separation membrane; from the comparison between Comparative Examples 7-8 and Example 4, it can be seen that the empty s orbital of the silver ion enhances its interaction with carbon dioxide, improves the solubility and selectivity of carbon dioxide, and then adds aluminum nitrate, the aluminum salt wraps the silver ions, stabilizes the silver ions, maximizes the interaction between the empty s orbital and carbon dioxide, and enables the silver ions to exist stably for a long time, thereby further improving the membrane permeability and selectivity.
[0109] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a gas separation membrane, It is characterized in that The following steps are involved: Step (1), reacting allyl glycidyl ether with bis(2-mercaptoethyl) ether to obtain an intermediate product A; reacting the intermediate product A with allyl boronic acid pinacol ester to obtain an intermediate product B; Step (2), reacting the intermediate product B with 2,6-diaminopyridine to obtain an intermediate product C; reacting the intermediate product C and D-glucosamine with terephthalaldehyde as a crosslinking agent to obtain a polyol; Step (3), using 3-chloro-1,2-propanediol and N-methylimidazole as raw materials, reacting to obtain a hydroxylated ionic liquid; Polyol, hydroxylated ionic liquid, isophorone diisocyanate and dimethylol propionic acid are used as raw materials to obtain a polyionic liquid dispersion through reaction; Step (4), after the polyionic liquid dispersion is diluted, silver tetrafluoroborate and aluminum nitrate are added to obtain a modified polyionic liquid dispersion; Adding a composite additive to a modified polyionic liquid dispersion to obtain a membrane raw material mixed solution, coating the membrane raw material mixed solution on a glass plate, and evaporating the mixed solution to obtain a gas separation membrane; Wherein, the preparation method of the composite additive comprises the following steps: Step S1, using 1,4-diazabicyclo[2.2.2]octane, 2-aminoterephthalic acid, and zinc nitrate hexahydrate as raw materials to prepare an ultra-microporous MOF material; Step S2, after the reaction of (R)-piperazine-2-carboxylic acid and cyanuric chloride, the ultra-microporous MOF material is grafted to obtain a porous composite material; Step S3, modifying the porous composite material with thionyl chloride to obtain a modified porous composite material; reacting the modified porous composite material with pentaethylenehexamine to obtain a composite additive.
2. The method for preparing a gas separation membrane according to claim 1, It is characterized in that In the step (1), the preparation method of the intermediate product B comprises the following steps: Mix allyl glycidyl ether and bis(2-mercaptoethyl) ether, stir at room temperature at a speed of 200-400 r / min for 3-5 hours, and purify to obtain intermediate product A; wherein the mass ratio of allyl glycidyl ether to bis(2-mercaptoethyl) ether is (3-6):(11.2-22.4); The intermediate product A is added to tetrahydrofuran, stirred for 10-20 minutes, heated to 50-60°C, and then allyl boric acid pinacol ester and azobisisobutyronitrile are added. The temperature is kept constant and the reaction is stirred at a speed of 200-400 r / min for 1-3 hours. After the reaction is completed, the intermediate product B is obtained by distillation under reduced pressure; wherein the mass ratio of the intermediate product A, tetrahydrofuran, allyl boric acid pinacol ester and azobisisobutyronitrile is (2.5-5):(20-50):(1.6-3.2):(0.02-0.05).
3. The method for preparing a gas separation membrane according to claim 1, It is characterized in that In the step (2), the method for preparing the polyol comprises the following steps: The intermediate product B is added to methanol, ultrasonically treated for 20-40 minutes, and then 2,6-diaminopyridine is added. The mixture is stirred at 70-90°C and 200-400 r / min for 20-30 hours. After the reaction is completed, the mixture is cooled to room temperature and evaporated to obtain an intermediate product C; wherein the mass ratio of the intermediate product B, methanol, and 2,6-diaminopyridine is (2.8-5.6):(50-90):(0.7-1.4); The intermediate products C and D-glucosamine are added to ethanol at a temperature of 40-50°C, and ultrasonic treatment is performed for 10-30 minutes to obtain a mixed solution; terephthalaldehyde is dissolved in ethanol, and then added to the mixed solution, and stirred for reaction at 60-70°C for 2-4 hours. After the reaction is completed, reduced pressure distillation is performed to obtain a polyol; wherein the mass ratio of the intermediate product C, D-glucosamine, and terephthalaldehyde is (2.5-5):(0.9-1.8):(0.6-1.2).
4. The method for preparing a gas separation membrane according to claim 1, It is characterized in that In the step (3), the method for preparing the hydroxylated ionic liquid comprises the following steps: In a glycerol bath at a temperature of 65-75°C, maintain a stirring speed of 200-400 r / min, add 3-chloro-1,2-propanediol to N-methylimidazole within 40-80 minutes, maintain the temperature unchanged, and stir the reaction for 70-80 hours. After the reaction is completed, remove the reaction mixture from the glycerol bath, wash it with ethyl acetate 5-9 times, and vacuum dry it to obtain a hydroxylated ionic liquid; wherein the mass ratio of 3-chloro-1,2-propanediol to N-methylimidazole is (13.2-26.4):(12-24).
5. The method for preparing a gas separation membrane according to claim 1, It is characterized in that In the step (3), the method for preparing the polyionic liquid dispersion comprises the following steps: Under constant stirring conditions at a rotation speed of 200-400 r / min, a polyol is added to methyl ethyl ketone, stirred for 10-20 min, a hydroxylated ionic liquid is added, stirred for 20-40 min, dibutyltin dilaurate and isophorone diisocyanate are added, reacted at 65-75° C. for 2-3 h, and then dimethylolpropionic acid is added, reacted at 65-75° C. for 2-3 h to obtain a polyionic liquid dispersion; wherein the mass ratio of the polyol, methyl ethyl ketone, hydroxylated ionic liquid, dibutyltin dilaurate, isophorone diisocyanate and dimethylolpropionic acid is (3.1-6.2):(50-80):(0.7-1.4):(0.03-0.05):(2.2-4.4):(0.2-0.5).
6. The method for preparing a gas separation membrane according to claim 1, It is characterized in that In the step (4), the preparation method of the modified polyionic liquid dispersion is: Under the conditions of a temperature of 40-50° C. and a stirring speed of 150-250 r / min, a polyionic liquid dispersion is diluted with methyl ethyl ketone to obtain a 2-5wt% polyionic liquid dilution; silver tetrafluoroborate is first added to the polyionic liquid dilution, and stirred at a speed of 100-200 r / min for 10-20 min, and then aluminum nitrate is added, and stirring is continued for 10-20 min to obtain a modified polyionic liquid dispersion, wherein the mass ratio of the polyionic liquid, silver tetrafluoroborate, and aluminum nitrate is 1:(0.08-0.15):(0.01-0.03).
7. The method for preparing a gas separation membrane according to claim 1, It is characterized in that In the step (4), the thickness of the gas separation membrane is 150-250 μm; the content of the composite additive in the raw material mixture is 5-20 wt %; and the evaporation conditions are: evaporation at room temperature for 4-6 days.
8. The method for preparing a gas separation membrane according to claim 1, It is characterized in that In step (4), the preparation method of the composite additive comprises the following steps: Step S1, adding 1,4-diazabicyclo[2.2.2]octane, 2-aminoterephthalic acid, and zinc nitrate hexahydrate to dimethyl sulfoxide, ultrasonically dispersing for 20-40 minutes, adding N,N-dimethylformamide, stirring, and then adding deionized water, sealing, reacting at 100-110° C. for 70-80 hours to form crystals, cooling, placing the crystals in methanol and standing for 5-7 hours, taking them out, washing them with methanol 2-3 times, and then soaking them in methanol for 10-30 hours, filtering, and obtaining an ultra-microporous MOF material; wherein the mass ratio of 1,4-diazabicyclo[2.2.2]octane, 2-aminoterephthalic acid, and zinc nitrate hexahydrate is (0.1-0.2):(2.7-5.4):(1-2); Step S2, at 3-7°C, add N,N-diisopropylethylamine and (R)-piperazine-2-carboxylic acid to 1,4-dioxane to obtain a reaction solution; in a nitrogen atmosphere, at 3-7°C, while stirring, drip cyanuric chloride into 1,4-dioxane at a rate of 0.5-0.8 mL / min, then add the above reaction solution, first stir the reaction at 12-18°C for 1.5-2.5 h, then stir the reaction at 22-28°C 1.5-2.5h, then add the ultra-microporous MOF material, stir and react at 80-90°C for 20-30h, after the reaction is completed, precipitate the product with ethanol, collect and dry the precipitate to obtain a porous composite material; wherein the mass ratio of N,N-diisopropylethylamine, (R)-piperazine-2-carboxylic acid, cyanuric chloride and ultra-microporous MOF material is (7-14):(1.9-3.8):(2.5-5):(1.9-3.8); Step S3, dispersing the porous composite material in thionyl chloride, then adding N,N-dimethylformamide, heating to 50-70°C and maintaining for 20-30 hours, and heating to 85-95°C after the reaction is completed to obtain a modified porous composite material; wherein the mass ratio of the porous composite material, thionyl chloride, and N,N-dimethylformamide is (1-3):(300-500):(4.8-9.6); Pentaethylenehexamine is added to N,N-dimethylformamide, and then a modified porous composite material is added, heated to 80-100°C and stirred for reaction for 20-30 hours. After the reaction is completed, the precipitate is collected, washed, and dried to obtain a composite additive; wherein the mass ratio of pentaethylenehexamine, N,N-dimethylformamide, and the modified porous composite material is (5-10):(20-40):(1-3).
9. A gas separation membrane prepared by the method for preparing a gas separation membrane according to any one of claims 1 to 8.
10. Use of the gas separation membrane according to claim 9 in carbon dioxide capture.