High temperature oxidation resistant dual phase high entropy alloy and preparation method thereof
Through a biphasic high-entropy alloy composed of Al, Cr, Co, Fe and Ni elements, combined with vacuum induction smelting and multiple temperature-changing smelting technology, a BCC and FCC biphasic structure is formed, solving the shortcomings of high-strength and oxidation resistance in the high-temperature field. , realizes the stable performance and antioxidant effect of high entropy alloys at high temperatures.
Patent Information
- Application Number
- CN202310434336.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-04-21
AI Technical Summary
There are few researches on the application of existing high-entropy alloys in the field of high temperatures, and their mechanical properties are limited, making it difficult to have high strength and high-temperature oxidation resistance.
The two-phase high-entropy alloy composed of Al, Cr, Co, Fe and Ni elements is formed through vacuum induction smelting process and multiple temperature-changing smelting processes to form an alloy with BCC and FCC biphasic structures, and the Al2O3 protective film generated by Al is improved. High temperature antioxidant capacity.
It achieves high strength and hardness that are stable at high temperatures. A dense oxide film is formed on the surface of the alloy, and the microhardness exceeds 500HV, which significantly improves the high-temperature oxidation resistance.
Smart Images

Figure CN116463537B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alloy materials and preparation thereof, and particularly relates to a high-entropy alloy resistant to high-temperature oxidation and a preparation method thereof. Background Art
[0002] With the rapid development of aerospace, nuclear energy, petrochemical and other fields, the performance requirements for high-temperature resistant metal materials are getting higher and higher, which has prompted the continuous progress of the new high-temperature resistant alloy industry in recent years. The emergence of the concept of high-entropy alloys has provided a very broad idea for the design of metal materials. The design concept of high-entropy alloys is very different from that of traditional alloys. It is defined as being composed of 5 or more elements as the main elements, and the atomic percentage of each element is usually between 5% and 35%. The structure is simple and stable, mostly FCC phase and BCC phase. High-entropy alloys have excellent properties that traditional metal materials cannot match. High-entropy alloys have high entropy effects and hysteresis diffusion effects, etc. It is easy to obtain solid solution phases and nanostructures with high thermal stability, making them stable at high temperatures and have high high-temperature resistance potential.
[0003] So far, a large number of literatures on high entropy alloys have been published, mainly focusing on how to improve the physical and mechanical properties of metals. Early high entropy alloys mainly focused on single-phase microstructures, with limited mechanical properties, poor casting properties, and few application studies in high-temperature fields. Therefore, how to provide a dual-phase high entropy alloy with both high strength and high-temperature oxidation resistance has become a technical problem that technicians in this field need to solve urgently. Summary of the invention
[0004] In response to the urgent need for new materials in the high-temperature field, the present invention provides a high-temperature oxidation-resistant dual-phase high-entropy alloy and a preparation method thereof.
[0005] The high-temperature oxidation-resistant dual-phase high-entropy alloy of the present invention consists of Al, Cr, Co, Fe and Ni elements, wherein the atomic molar ratio of Al, Cr, Co, Fe and Ni is 1:1:1:1:2.1, and the dual-phase high-entropy alloy has a BCC and FCC dual-phase structure.
[0006] The preparation method of the high temperature oxidation resistant dual-phase high entropy alloy of the present invention is achieved by the following steps:
[0007] 1. Weigh 12% to 18% Al, 12% to 18% Cr, 12% to 18% Co, 12% to 18% Fe and 30% to 36% Ni (single substance) metal particles as raw materials according to atomic percentage;
[0008] 2. The raw materials in step 1 are evenly stacked from bottom to top in the crucible according to the melting point from low to high, and then the crucible is sent into the outer crucible of the melting furnace and fixed, the water cooler is turned on, the cooling circulation system is turned on, the furnace cover of the melting furnace is closed and locked, the vacuum pump pre-vacuum valve is opened, and the pressure in the furnace is evacuated to less than 10MPa, the vacuum valve is closed, the valve of the argon gas bottle is opened, and the argon gas is filled into the melting furnace until the vacuum degree is 0.05-0.08MPa;
[0009] 3. Repeat step 2 to evacuate and fill with argon 2-3 times, then close the argon filling valve and the mechanical pump to complete the furnace cleaning;
[0010] 4. Turn on the high-frequency heating power supply of the melting furnace to start heating. The electrode is heated by the coil wrapped around the crucible. By adjusting the current control knob, the current is gradually increased to 40-45A for melting. When the temperature reaches 1600℃-1680℃, keep it warm for 20-30 minutes to obtain molten metal.
[0011] 5. After the insulation is completed, gradually reduce the current and lower the temperature in the furnace to 1200℃~1280℃. When the current drops to 30~35A, increase the current to 40~45A for variable temperature smelting;
[0012] 6. Repeat the temperature-variable melting process of step 5 3 to 6 times;
[0013] 7. After the smelting is completed, turn off the current, turn off the heating power supply, keep the water cooler powered on, discharge the heat in the furnace, allow the metal in the crucible to cool naturally, open the vent valve, open the smelting furnace cover to take out the high-entropy alloy ingot, and complete the preparation of high-temperature oxidation-resistant duplex high-entropy alloy.
[0014] Furthermore, in step 4, the electrode and the crucible can be manually rotated outside the furnace body, and the pouring and pouring of the liquid can be completed in the cavity.
[0015] Furthermore, in step 4 and step 5, the interval between each current adjustment is not less than 5 minutes, and the current is adjusted to 1A each time.
[0016] The present invention adopts a vacuum induction melting process and adds an element (Al) that can stabilize the BCC phase. Through multiple temperature-variable melting processes, the diffusion and fusion between the elements are accelerated, and the formation of a dual phase in the alloy is promoted. At the same time, the alloy containing Al is prone to generate an Al2O3 protective film during high-temperature oxidation, which is beneficial to improving the high-temperature oxidation resistance of the alloy.
[0017] Compared with the existing technology, the high temperature oxidation resistant dual-phase high entropy alloy and the preparation method thereof of the present invention include the following beneficial technical effects:
[0018] 1. AlCrCoFeNi of the present invention 2.1The dual-phase high-entropy alloy is composed of FCC phase and BCC phase matrix, and has both high strength and high hardness. The microhardness of this alloy can reach more than 500HV, and its application value is expected in the future.
[0019] 2. AlCrCoFeNi of the present invention 2.1 High entropy alloys have good high-temperature oxidation resistance. Tests have shown that they are stable at high temperatures of 820°C. An oxide film will form on the surface of the alloy, slowing down the oxidation process of the alloy, and the oxide film is not easy to fall off. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The microhardness bar graph of the high entropy alloy of Example 1;
[0021] Figure 2 The AlCrCoFeNi of Example 1 2.1 X-ray diffraction (XRD) spectrum of high entropy alloy;
[0022] Figure 3 This is a microstructure morphology of the high temperature oxidation resistant dual-phase high entropy alloy prepared in Example 1;
[0023] Figure 4 AlCrCoFeNi of Example 2 2.1 Weight gain curve of high entropy alloy oxidized at 820℃, where ▲ represents AlCrCoFeNi 2.1 High entropy alloy, ● represents 304 stainless steel. DETAILED DESCRIPTION
[0024] Specific implementation method one: In this implementation method, the high-temperature oxidation-resistant dual-phase high-entropy alloy is composed of Al, Cr, Co, Fe and Ni elements, and the atomic molar ratio of Al, Cr, Co, Fe and Ni is 1:1:1:1:2.1. The dual-phase high-entropy alloy has a BCC and FCC dual-phase structure.
[0025] The structural formula of the high temperature oxidation resistant dual phase high entropy alloy in this embodiment is AlCrCoFeNi 2.1 .
[0026] Specific implementation method 2: The preparation method of the high temperature oxidation resistant dual-phase high entropy alloy in this implementation method is implemented according to the following steps:
[0027] 1. Weigh 12% to 18% Al, 12% to 18% Cr, 12% to 18% Co, 12% to 18% Fe and 30% to 36% Ni (single substance) metal particles as raw materials according to atomic percentage;
[0028] 2. The raw materials in step 1 are evenly stacked from bottom to top in the crucible according to the melting point from low to high, and then the crucible is sent into the outer crucible of the melting furnace and fixed, the water cooler is turned on, the cooling circulation system is turned on, the furnace cover of the melting furnace is closed and locked, the vacuum pump pre-vacuum valve is opened, and the pressure in the furnace is evacuated to less than 10MPa, the vacuum valve is closed, the valve of the argon gas bottle is opened, and the argon gas is filled into the melting furnace until the vacuum degree is 0.05-0.08MPa;
[0029] 3. Repeat step 2 to evacuate and fill with argon 2-3 times, then close the argon filling valve and the mechanical pump to complete the furnace cleaning;
[0030] 4. Turn on the high-frequency heating power supply of the melting furnace to start heating. The electrode is heated by the coil wrapped around the crucible. By adjusting the current control knob, the current is gradually increased to 40-45A for melting. When the temperature reaches 1600℃-1680℃, keep it warm for 20-30 minutes to obtain molten metal.
[0031] 5. After the insulation is completed, gradually reduce the current and lower the temperature in the furnace to 1200℃~1280℃. When the current drops to 30~35A, increase the current to 40~45A for variable temperature smelting;
[0032] 6. Repeat the temperature-variable melting process of step 5 3 to 6 times;
[0033] 7. After the smelting is completed, turn off the current, turn off the heating power supply, keep the water cooler powered on, discharge the heat in the furnace, allow the metal in the crucible to cool naturally, open the vent valve, open the smelting furnace cover to take out the high-entropy alloy ingot, and complete the preparation of high-temperature oxidation-resistant duplex high-entropy alloy.
[0034] Specific implementation method three: This implementation method is different from specific implementation method two in that the purity of each metal particle in step one is higher than 99.9%.
[0035] Specific implementation method 4: This implementation method is different from specific implementation methods 2 or 3 in that the melting furnace described in step 2 is a vacuum induction melting furnace.
[0036] Specific implementation mode 5: This implementation mode is different from any one of specific implementation modes 2 to 4 in that the crucible in step 2 is a zirconia crucible, a graphite crucible or a cast iron crucible.
[0037] Specific implementation method 6: The difference between this implementation method and any one of specific implementation methods 2 to 5 is that in step 4, the current is gradually increased to 42A for smelting, and when the temperature is raised to 1600°C, it is kept warm for 30 minutes.
[0038] Specific implementation method 7: The difference between this implementation method and any one of specific implementation methods 2 to 6 is that in the process of gradually increasing the current in step 4, the current is adjusted by 1A each time, and the interval time is not less than 5 minutes.
[0039] Specific implementation eight: This implementation differs from any one of specific implementations two to seven in that in step five, when the current drops to 33-35 A, the current is increased again to 40-44 A.
[0040] Specific implementation method 9: The difference between this implementation method and any one of specific implementation methods 2 to 8 is that in step 5, the current is adjusted by 1A each time during the process of gradually reducing the current, and the interval time is 5 to 6 minutes; the current is adjusted by 1A each time during the process of increasing the current, and the interval time is 5 to 6 minutes.
[0041] Specific implementation method ten: This implementation method is different from any one of specific implementation methods two to nine in that in step six, the temperature-variable melting process of step five is repeated 3 to 6 times.
[0042] Embodiment 1: The preparation method of the high temperature oxidation resistant dual-phase high entropy alloy of this embodiment is implemented according to the following steps:
[0043] 1. Weigh 16% Al, 14% Cr, 16% Co, 18% Fe and 36% Ni (single substance) metal particles as raw materials according to atomic percentage;
[0044] 2. The raw materials in step 1 are evenly stacked from bottom to top in the crucible according to the melting point from low to high, and then the crucible is sent into the outer crucible of the VIF type vacuum induction melting furnace for fixing, the water cooler is turned on, the cooling circulation system is turned on, the furnace cover of the melting furnace is closed and locked, the vacuum pump pre-evacuation valve is opened, and the vacuum is evacuated until the pressure in the furnace is lower than 10MPa, the vacuum valve is closed, the valve of the argon gas bottle is opened, and the argon gas is filled into the melting furnace until the pressure reaches 0.75 atmospheres;
[0045] 3. Repeat step 2 to evacuate and fill with argon gas 3 times, then close the argon filling valve and the mechanical pump to complete the furnace cleaning;
[0046] 4. Turn on the high-frequency heating power supply of the melting furnace to start heating. The rotating electrode is heated by the coil wrapped around the crucible. By adjusting the current control knob, the initial current is 12A, and the current is gradually increased to 42A for melting. The current is adjusted by 1A each time, and the interval of each current adjustment is 5 minutes. When the temperature rises to 1600℃, keep it at this temperature for 30 minutes to obtain molten metal;
[0047] 5. After the insulation is completed, gradually reduce the current and lower the temperature in the furnace to 1200℃. When the current drops to 34A, increase the current to 42A for variable temperature melting. Adjust the current by 1A each time, and the interval time is 5min.
[0048] 6. Repeat the temperature-variable melting process of step 5 6 times;
[0049] 7. After the smelting is completed, turn off the current, turn off the heating power supply, keep the water cooler powered on, discharge the heat in the furnace, allow the metal in the crucible to cool naturally, open the vent valve, open the smelting furnace cover to take out the high-entropy alloy ingot, and complete the preparation of high-temperature oxidation-resistant duplex high-entropy alloy.
[0050] After the smelting is completed, the cylindrical alloy ingot can be cooled and the oxide layer on the surface can be removed by a wire cutting machine, and then the ingot can be cut into AlCrCoFeNi alloys with a radius of about 40 mm and a thickness of about 25 mm. 2.1 High entropy alloy block.
[0051] The AlCrCoFeNi prepared in this example 2.1 High entropy alloy, its microhardness curve is as follows Figure 1 As shown, it can be seen that AlCrCoFeNi 2.1 The hardness of high entropy alloys can exceed 500 HV.
[0052] The high entropy alloy sample was subjected to XRD phase analysis, and its XRD spectrum was as follows: Figure 2 As shown, it can be seen that the high entropy alloy consists of FCC phase and BCC phase, which is a two-phase structure, in which the FCC phase is the main phase.
[0053] Embodiment 2: The preparation method of the high temperature oxidation resistant dual-phase high entropy alloy of this embodiment is implemented according to the following steps:
[0054] 1. Weigh 18% Al, 16% Cr, 15% Co, 16% Fe and 35% Ni (single substance) metal particles as raw materials according to atomic percentage;
[0055] 2. The raw materials in step 1 are evenly stacked from bottom to top in the crucible according to the melting point from low to high, and then the crucible is sent into the outer crucible of the melting furnace and fixed, the water cooler is turned on, the cooling circulation system is turned on, the furnace cover of the melting furnace is closed and locked, the vacuum pump pre-evacuation valve is opened, and the vacuum is evacuated until the pressure in the furnace is lower than 10MPa, the vacuum valve is closed, the valve of the argon gas bottle is opened, and the argon gas is filled into the melting furnace until the pressure reaches 0.75 atmospheres;
[0056] 3. Repeat step 2 to evacuate and fill with argon gas 3 times, then close the argon filling valve and the mechanical pump to complete the furnace cleaning;
[0057] 4. Turn on the high-frequency heating power supply of the melting furnace to start heating. The rotating electrode is heated by the coil wrapped around the crucible. By adjusting the current control knob, the initial current is 12A, and the current is gradually increased to 42A for melting. When the temperature reaches 1600℃, keep it at this temperature for 30 minutes to obtain molten metal;
[0058] 5. After the insulation is completed, gradually reduce the current and lower the temperature in the furnace to 1200℃. When the current drops to 34A, increase the current to 42A for variable temperature melting. Adjust the current by 1A each time, and the interval time is 5min.
[0059] 6. Repeat the temperature-variable melting process of step 5 4 times;
[0060] 7. After the smelting is completed, turn off the current, turn off the heating power supply, keep the water cooler powered on, discharge the heat in the furnace, allow the metal in the crucible to cool naturally, open the vent valve, open the smelting furnace cover to take out the high-entropy alloy ingot, and complete the preparation of high-temperature oxidation-resistant duplex high-entropy alloy.
[0061] In this example, the oxidation weight gain curve of the prepared dual-phase high entropy alloy at 820°C is analyzed. Figure 4 It can be seen that after oxidation at 820℃ for 50h, the weight gains of the duplex high entropy alloy and 304 stainless steel in this embodiment are 0.95mg / cm 2 and 2.1 mg / cm 2 The weight gain of the high entropy alloy in this embodiment is compared with the weight gain of 304 stainless steel, which gradually tends to be stable over time. From the perspective of oxidation kinetics, the high entropy alloy in this embodiment has excellent high-temperature oxidation resistance.
[0062] Further analysis of the oxide film attached to the surface of the alloy after high-temperature oxidation shows that after the high-entropy alloy of the present invention is oxidized at a high temperature of 820°C for 10 hours, the oxide film formed on the surface of the alloy is stable at high temperatures and has good density, which can protect the alloy matrix from further oxidation.
Claims
1. A method for preparing a high temperature oxidation resistant dual phase high entropy alloy, characterized in that The preparation method is achieved by the following steps:
1. Weigh 12% to 18% Al, 12% to 18% Cr, 12% to 18% Co, 12% to 18% Fe and 30% to 36% Ni metal particles as raw materials according to atomic percentage; 2. The raw materials in step 1 are evenly stacked from bottom to top in the crucible according to the melting point from low to high, and then the crucible is sent into the outer crucible of the melting furnace and fixed, the water cooler is turned on, the cooling circulation system is turned on, the furnace cover of the melting furnace is closed and locked, the vacuum pump pre-vacuum valve is opened, and the pressure in the furnace is evacuated to less than 10MPa, the vacuum valve is closed, the valve of the argon gas bottle is opened, and the argon gas is filled into the melting furnace until the vacuum degree is 0.05-0.08MPa; 3. Repeat step 2 to evacuate and fill with argon 2-3 times, then close the argon filling valve and the mechanical pump to complete the furnace cleaning; 4. Turn on the high-frequency heating power supply of the melting furnace to start heating. The electrode is heated by the coil wrapped around the crucible. By adjusting the current control knob, the current is gradually increased to 40-45A for melting. When the temperature reaches 1600℃-1680℃, keep it warm for 20-30 minutes to obtain molten metal.
5. After the insulation is completed, gradually reduce the current and lower the temperature in the furnace to 1200℃~1280℃. When the current drops to 30~35A, increase the current to 40~45A for variable temperature smelting; 6. Repeat the temperature-variable melting process of step 5 3 to 6 times; 7. After the smelting is completed, turn off the current, turn off the heating power supply, keep the water cooler powered on, discharge the heat in the furnace, let the metal in the crucible cool naturally, open the vent valve, open the smelting furnace cover to take out the high entropy alloy ingot, and complete the preparation of high temperature oxidation resistant dual-phase high entropy alloy; In the process of gradually reducing the current in step 5, the current is adjusted by 1A each time, and the interval time is 5 to 6 minutes; in the process of increasing the current, the current is adjusted by 1A each time, and the interval time is 5 to 6 minutes.
2. The method for preparing a high temperature oxidation resistant dual phase high entropy alloy according to claim 1, characterized in that The purity of each metal particle in step 1 is higher than 99.9%.
3. The method for preparing a high temperature oxidation resistant dual phase high entropy alloy according to claim 1, characterized in that The smelting furnace described in step 2 is a vacuum induction smelting furnace.
4. The method for preparing a high temperature oxidation resistant dual phase high entropy alloy according to claim 1, characterized in that In step 2, the crucible is a zirconia crucible, a graphite crucible or a cast iron crucible.
5. The method for preparing a high temperature oxidation resistant dual phase high entropy alloy according to claim 1, characterized in that In step 4, the current is gradually increased to 42A for smelting, and the temperature is raised to 1600°C and kept at this temperature for 30 minutes.
6. The method for preparing a high temperature oxidation resistant dual phase high entropy alloy according to claim 1, characterized in that In the process of gradually increasing the current in step 4, adjust the current by 1A each time, with an interval of no less than 5 minutes.
7. The method for preparing a high temperature oxidation resistant dual phase high entropy alloy according to claim 1, characterized in that In step 5, when the current drops to 33-35A, the current is increased again to 40-44A.
8. The method for preparing a high temperature oxidation resistant dual phase high entropy alloy according to claim 1, characterized in that In step six, the temperature-variable melting process of step five is repeated 5 to 6 times.
Citation Information
Patent Citations
AlCoCuFeNix high-entropy alloy having both high strength and soft magnetic property and preparation method thereof
CN108517452A
Eutectic high-entropy alloy with low notch sensitivity and preparation method thereof
CN111321336A
Corrosion-resistant aluminum-transition metal system double-phase high-entropy alloy and preparation method thereof
CN112458352A
Superhard as-cast NiAlCoFeNb double-phase high-entropy alloy and preparation method thereof
CN115404367A
Alloy structure
JP2016023351A