Method for producing catalyst for producing ethyl acetate
By impregnating an aqueous solution of heteropoly acid or its salt into the support and processing it under specific drying conditions, the problem of catalyst load control is solved, and an efficient and excellent selective industrial manufacturing of ethyl acetate catalyst is achieved.
Patent Information
- Application Number
- CN202180063469.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-09-29
- Filing Date
- 2021-08-23
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-08-23
AI Technical Summary
In the prior art, when producing a catalyst for ethyl acetate, it is difficult to control the loading of active ingredients between the catalyst particles, and industrial manufacturing is not suitable, and the catalyst performance and selectivity are insufficient.
The aqueous solution of heteropoly acid or salt is used to infiltrate at 80 to 105% of the saturated water absorption capacity of the carrier, and the drying rate is set at 5 to 300 g H2O/kg supcapat·min, and the temperature of the drying medium is 80 to 130°C. Drying under the relative humidity of 0 to 60% RH is prepared to produce a highly efficient catalyst.
The production of ethyl acetate with high catalyst activity and excellent selectivity is achieved, and is used for high productivity catalysts and is suitable for industrial manufacturing.
Smart Images

Figure CN116472113B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a catalyst for producing ethyl acetate and a method for producing ethyl acetate using the catalyst. Background Art
[0002] It is well known that corresponding esters can be produced from lower aliphatic carboxylic acids and lower olefins by gas phase contact reaction. It is also well known that supported catalysts in which a heteropolyacid and / or a salt thereof is supported on a carrier are useful (Patent Documents 1 to 3).
[0003] In a gas phase contact reaction using a supported catalyst, a method of improving catalyst performance by supporting an active component near the surface of a support to increase the contact efficiency between the active component and the reactant is known (Patent Documents 4 and 5).
[0004] For example, Patent Document 4 describes a catalyst in which an active ingredient is supported near the surface of a carrier by impregnating a carrier with a solution obtained by dissolving an active ingredient in an acetic acid solvent having a water absorption capacity of 10 to 40% by volume of the carrier. Patent Document 5 describes a catalyst in which an active ingredient is supported near the surface of a carrier by impregnating a carrier with a solution obtained by dissolving an active ingredient in water having a water absorption capacity of 10 to 70% by volume of the carrier, and drying the obtained impregnated body under reduced pressure at a predetermined speed.
[0005] However, in Patent Document 4, acetic acid used as a solvent is harmful, and in Patent Document 5, the impregnation body is dried under reduced pressure, so neither of these production methods is suitable for industrial production of catalysts. In addition, in these production methods, since the amount of solution impregnated into the carrier needs to be a relatively small amount of 10 to 40 volume % or 10 to 70 volume % of the water absorption of the carrier, there is a fear that catalyst particles with a large amount of active components and catalyst particles with a small amount or almost no active components may be produced.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 09-118647
[0009] Patent Document 2: Japanese Patent Application Publication No. 2000-342980
[0010] Patent Document 3: Japanese Patent Application No. 2008-513534
[0011] Patent Document 4: Japanese Patent Application Publication No. 2004-209469
[0012] Patent Document 5: Japanese Patent Application Publication No. 2019-162604 Summary of the invention
[0013] In order to efficiently produce esters from lower aliphatic carboxylic acids and lower olefins by gas phase contact reaction, it is necessary to produce a catalyst having a heteropoly acid and / or a salt thereof supported near the surface of a carrier. However, in a production method in which the amount of impregnation solution used is suppressed to a low level, it is difficult to control the fluctuation of the amount of active components supported between catalyst particles. Therefore, a method for simply producing a catalyst having excellent activity and selectivity in industry is desired.
[0014] Under such circumstances, an object of the present invention is to provide a method for producing a catalyst for producing ethyl acetate having high productivity and excellent catalyst performance, wherein a heteropolyacid and / or a salt thereof is supported near the surface of a carrier.
[0015] The present inventors have repeatedly conducted in-depth studies on a method for producing a catalyst for ethyl acetate production using a heteropolyacid and / or its salt as an active ingredient, and have found that even when an aqueous solution of a heteropolyacid and / or its salt having a volume close to 100% of the saturated water absorption capacity of the carrier (also referred to as "heteropolyacid aqueous solution" in the present disclosure) is used as an impregnation solution and the impregnation solution is uniformly infiltrated into the interior of the carrier, by setting the constant rate drying speed in a particularly large specific range in the drying process of the impregnated body, more active ingredients can be loaded on the surface of the carrier, and a catalyst for ethyl acetate production having high catalytic activity and excellent selectivity can be efficiently produced, thereby completing the present invention.
[0016] That is, the present invention relates to the following [1] to [7]. [1]
[0018] A method for producing a catalyst for producing ethyl acetate comprises the following steps in sequence:
[0019] (1) an impregnation step of impregnating a silica support with an aqueous solution of a heteropolyacid or a salt thereof at 80 to 105% by volume of the saturated water absorption capacity of the support to form an impregnated body; and
[0020] (2) 5 to 300 g H2O / kg supcat A drying step of drying the impregnated body at a constant drying rate of minutes. [2]
[0022] According to the method for producing a catalyst for producing ethyl acetate described in [1], the constant rate drying speed in the drying step is 10 to 150 g H2O / kg supcat ·minute. [3]
[0024] The method for producing a catalyst for producing ethyl acetate according to [1] or [2], wherein the constant rate drying rate in the drying step is 15 to 50 g H2O / kg supcat ·minute. [4]
[0026] The method for producing a catalyst for producing ethyl acetate according to any one of [1] to [3], wherein the temperature of the drying medium used in the drying step is 80 to 130°C. [5]
[0028] According to the method for producing a catalyst for producing ethyl acetate described in any one of [1] to [4], the drying medium in the drying step is air having a relative humidity of 0 to 60% RH, and the air is brought into contact with the impregnated body as a circulating airflow to dry the impregnated body. [6]
[0030] The method for producing a catalyst for producing ethyl acetate according to any one of [1] to [5], wherein the pressure in the drying step is normal pressure. [7]
[0032] A method for producing ethyl acetate, comprising reacting ethylene and acetic acid as raw materials in the presence of a catalyst for producing ethyl acetate produced by the method described in any one of [1] to [6].
[0033] According to the present invention, a catalyst for producing ethyl acetate, in which an active component is present near the surface of a carrier and which exhibits high catalytic performance, can be provided with high productivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is an illustration of the fixed rate drying period.
[0035] Figure 2 This is an EPMA image of the catalyst of Example 1 in which a heteropoly acid is supported on a silica support.
[0036] Figure 3 This is an EPMA image of the catalyst of Comparative Example 1 in which a heteropoly acid is supported on a silica support.
[0037] Figure 4 This is a graph showing the selectivity of butene as a by-product in Examples 1 to 5 and Comparative Examples 1 to 3. DETAILED DESCRIPTION
[0038] Hereinafter, preferred embodiments of the present invention will be described, but the present invention is not limited to these embodiments, and it should be understood that various applications are possible within the spirit and scope of the present invention.
[0039] [Manufacture of catalyst for ethyl acetate production]
[0040] In one embodiment, ethyl acetate is produced by reacting ethylene and acetic acid in a gas phase using a solid acid catalyst. The solid acid catalyst used to produce ethyl acetate is a heteropolyacid or a salt thereof (also referred to as a "heteropolyacid salt" in this disclosure), which is supported by a silica carrier and used.
[0041] [Heteropolyacids and their salts]
[0042] Heteropolyacids are composed of a central element and peripheral elements bonded to oxygen. The central element is usually silicon or phosphorus, but can be composed of any of a variety of elements selected from Groups 1 to 17 of the periodic table. Specifically, for example, divalent copper ions; divalent ions of beryllium, zinc, cobalt or nickel; trivalent ions of boron, aluminum, gallium, iron, cerium, arsenic, antimony, phosphorus, bismuth, chromium or rhodium; tetravalent ions of silicon, germanium, tin, titanium, zirconium, vanadium, sulfur, tellurium, manganese, nickel, platinum, thorium, hafnium, cerium and other rare earth ions; pentavalent ions of phosphorus, arsenic, vanadium, antimony; hexavalent tellurium ions; and heptavalent iodine ions, etc., but are not limited to these. In addition, as specific examples of peripheral elements, tungsten, molybdenum, vanadium, niobium, tantalum, etc. can be cited, but are not limited to these.
[0043] Such heteropolyacids are also known as "polyoxyanions", "polyoxymetallic salts" or "metal oxide clusters". Some structures of well-known anion classes are named after researchers in the field, for example, Keggin-type structures, Wells-Dawson-type structures and Anderson-Evans-Perloff-type structures are known. Details are described in "Chemistry of Polyacids" (edited by the Chemical Society of Japan, Quarterly Chemical Review No. 20, 1993). Heteropolyacids generally have high molecular weights, for example, molecular weights in the range of 700 to 8500, including not only monomers thereof but also dimer complexes thereof.
[0044] As for the heteropoly acid salt, any metal salt or There are no particular limitations on the salt. Specifically, for example, metal salts of lithium, sodium, potassium, cesium, magnesium, barium, copper, gold, and gallium, and salts of ammonia, etc. Salt, but not limited to this.
[0045] Particularly preferred examples of heteropolyacids that can be used as catalysts include:
[0046] Silicotungstic Acid H 4 [SiW 12 O 40 ]·xH 2 O
[0047] Phosphotungstic acid H3 [PW 12 O 40 ]·xH 2 O
[0048] Phosphomolybdic acid H 3 [PMo 12 O 40 ]·xH 2 O
[0049] Silicomolybdic acid H 4 [SiMo 12 O 40 ]·xH 2 O
[0050] Silicon Vanadium Tungstate H 4+n [SiV n W 12-n O 40 ]·xH 2 O
[0051] Phosphovanadotungstate H 3+n [PV n W 12-n O 40 ]·xH 2 O
[0052] Phosphovanadomolybdic acid H 3+n [PV n Mo 12-n O 40 ]·xH 2 O
[0053] Silicovanadomolybdic acid H 4+n [SiV n Mo 12-n O 40 ]·xH 2 O
[0054] Silicomolybdic acid H 4 [SiMo n W 12-n O 40 ]·xH 2 O
[0055] Phosphomolybdic acid H 3 [PMo n W 12-n O 40 ]·xH 2 O
[0056] (wherein n is an integer of 1 to 11, and x is an integer greater than or equal to 1)
[0057] And so on, but not limited to this.
[0058] The heteropoly acid is preferably silicotungstic acid, phosphotungstic acid, phosphomolybdic acid, silicomolybdic acid, silicovanadotungstic acid or phosphovanadotungstic acid, more preferably silicotungstic acid or phosphotungstic acid.
[0059] There is no particular limitation on the method for synthesizing such heteropolyacids, and various methods can be used. For example, heteropolyacids can be obtained by heating an acidic aqueous solution (about pH 1 to pH 2) containing a salt of molybdic acid or tungstic acid and a simple oxygen-containing acid or its salt containing a heteroatom. For example, heteropolyacid compounds can be isolated by crystallization separation in the form of a metal salt from the generated heteropolyacid aqueous solution. Specific examples of the manufacture of heteropolyacids are recorded in "New Experimental Chemistry Lecture 8 Synthesis of Inorganic Compounds (III)" (edited by the Chemical Society of Japan, published by Maruzen Co., Ltd., August 20, 1945, 3rd edition), page 1413, but are not limited to this. In addition to chemical analysis, the structural confirmation of the synthesized heteropolyacid can also be carried out by X-ray diffraction, UV or IR measurement.
[0060] Preferred examples of the heteropolyacid salts include lithium salts, sodium salts, potassium salts, cesium salts, magnesium salts, barium salts, copper salts, gold salts, gallium salts and ammonium salts of the above-mentioned preferred heteropolyacids.
[0061] Specific examples of heteropolyacids include lithium salts of silicotungstic acid, sodium salts of silicotungstic acid, cesium salts of silicotungstic acid, copper salts of silicotungstic acid, gold salts of silicotungstic acid, and gallium salts of silicotungstic acid; lithium salts of phosphotungstic acid, sodium salts of phosphotungstic acid, cesium salts of phosphotungstic acid, copper salts of phosphotungstic acid, gold salts of phosphotungstic acid, and gallium salts of phosphotungstic acid; lithium salts of phosphomolybdic acid, sodium salts of phosphomolybdic acid, cesium salts of phosphomolybdic acid, copper salts of phosphomolybdic acid, gold salts of phosphomolybdic acid, and gallium salts of phosphomolybdic acid; lithium salts of silicomolybdic acid, sodium salts of silicomolybdic acid, cesium salts of silicomolybdic acid, copper salts of silicomolybdic acid, gold salts of silicomolybdic acid, and gallium salts of silicomolybdic acid; silicovanadotungstic acid. Lithium salt of silicovanadotungstic acid, sodium salt of silicovanadotungstic acid, cesium salt of silicovanadotungstic acid, copper salt of silicovanadotungstic acid, gold salt of silicovanadotungstic acid, gallium salt of silicovanadotungstic acid; lithium salt of phosphovanadotungstic acid, sodium salt of phosphovanadotungstic acid, cesium salt of phosphovanadotungstic acid, copper salt of phosphovanadotungstic acid, gold salt of phosphovanadotungstic acid, gallium salt of phosphovanadotungstic acid; lithium salt of phosphovanadomolybdic acid, sodium salt of phosphovanadomolybdic acid, cesium salt of phosphovanadomolybdic acid, copper salt of phosphovanadomolybdic acid, gold salt of phosphovanadomolybdic acid, gallium salt of phosphovanadomolybdic acid; lithium salt of silicovanadomolybdic acid, sodium salt of silicovanadomolybdic acid, cesium salt of silicovanadomolybdic acid, copper salt of silicovanadomolybdic acid, gold salt of silicovanadomolybdic acid, gallium salt of silicovanadomolybdic acid, etc.
[0062] The heteropolyacid salt is preferably a lithium salt of silicotungstic acid, a sodium salt of silicotungstic acid, a cesium salt of silicotungstic acid, a copper salt of silicotungstic acid, a gold salt of silicotungstic acid, a gallium salt of silicotungstic acid; a lithium salt of phosphotungstic acid, a sodium salt of phosphotungstic acid, a cesium salt of phosphotungstic acid, a copper salt of phosphotungstic acid, a gold salt of phosphotungstic acid, a gallium salt of phosphotungstic acid; a lithium salt of phosphomolybdic acid, a sodium salt of phosphomolybdic acid, a cesium salt of phosphomolybdic acid, a copper salt of phosphomolybdic acid, a gold salt of phosphomolybdic acid, a gallium salt of phosphomolybdic acid; a silicon molybdenum salt The invention relates to a lithium salt of silicomolybdic acid, a sodium salt of silicomolybdic acid, a cesium salt of silicomolybdic acid, a copper salt of silicomolybdic acid, a gold salt of silicomolybdic acid, and a gallium salt of silicomolybdic acid; a lithium salt of silicovanadotungstic acid, a sodium salt of silicomolybdic acid, a cesium salt of silicomolybdic acid, a copper salt of silicomolybdic acid, a gold salt of silicomolybdic acid, and a gallium salt of silicomolybdic acid; a lithium salt of silicovanadotungstic acid, a sodium salt of silicovanadotungstic acid, a cesium salt of silicovanadotungstic acid, a copper salt of silicovanadotungstic acid, a gold salt of silicovanadotungstic acid, and a gallium salt of silicovanadotungstic acid; a lithium salt of phosphovanadotungstic acid, a sodium salt of phosphovanadotungstic acid, a cesium salt of phosphovanadotungstic acid, a copper salt of phosphovanadotungstic acid, a gold salt of phosphovanadotungstic acid, or a gallium salt of phosphovanadotungstic acid.
[0063] As the heteropolyacid salt, a lithium salt of silicotungstic acid or a cesium salt of phosphotungstic acid is particularly preferably used.
[0064] [Silica carrier]
[0065] The silica carrier may be in any shape, and is not particularly limited thereto, but is preferably spherical or granular. The particle size of the silica carrier varies depending on the reaction form, and when used in a fixed bed, is preferably 2 mm to 10 mm, and more preferably 3 mm to 7 mm.
[0066] In one embodiment, the loading of the heteropolyacid or its salt on the silica carrier sequentially comprises: a step (impregnation step) of causing the silica carrier to absorb (impregnate) an aqueous solution of the heteropolyacid or its salt (heteropolyacid aqueous solution) at a specific impregnation rate; and a step (drying step) of drying the carrier impregnated with the heteropolyacid aqueous solution under specific drying conditions. Other steps (such as an air drying step, a transfer step from an impregnation device to a drying device, etc.) may also be included between the impregnation step and the drying step, but it is preferred that these two steps are performed continuously.
[0067] [Impermeation process]
[0068] In the impregnation step, for example, a spherical or granular silica carrier absorbs a heteropolyacid aqueous solution as an impregnation liquid to form an impregnated body. The carrier is preferably stirred during the impregnation operation. The concentration of the heteropolyacid or its salt in the heteropolyacid aqueous solution is determined by the volume of the heteropolyacid aqueous solution calculated from the impregnation rate and the amount of the catalyst to be supported on the carrier. The concentration of the heteropolyacid or its salt in the heteropolyacid aqueous solution can generally be 0.8 to 1.2 kg / L.
[0069] The volume of the heteropolyacid aqueous solution impregnated in the carrier is in the range of 80 to 105 volume % of the saturated water absorption capacity of the carrier, preferably in the range of 90 to 100 volume %, and more preferably in the range of 95 to 100 volume %. When the volume of the heteropolyacid aqueous solution is less than 80 volume %, catalyst particles that are not supported by the heteropolyacid or its salt may be mixed. When the volume of the heteropolyacid aqueous solution is greater than 105 volume %, the heteropolyacid or its salt that is not absorbed by the carrier exists in a free state, and it is afraid that the necessary amount of catalyst cannot be uniformly supported on the carrier.
[0070] "Saturated water absorption capacity of the carrier" refers to the volume (L) of water that can be absorbed by a carrier with an apparent volume of 1 L. The details of the determination method are described later. "Impermeation rate" is shown in the following formula, which is the ratio (volume %) of the volume of the heteropolyacid aqueous solution absorbed by the carrier to the saturated water absorption capacity of the carrier. The saturated water absorption capacity (L) and the volume (L) of the heteropolyacid aqueous solution are values at room temperature (23°C).
[0071] Impregnation rate (%)
[0072] = 100 × volume of heteropolyacid aqueous solution absorbed by the carrier of apparent volume 1L / saturated water absorption capacity of the carrier
[0073] [Drying process]
[0074] In the drying process, the impregnated body is dried under specific drying conditions. Specifically, the drying speed during the fixed-rate drying period (fixed-rate drying speed) at the initial stage of drying of the impregnated body is controlled within a specific range. The drying speed after the fixed-rate drying period may be different.
[0075] When the wet material is dried, the amount of reduction in moisture content per unit time (reduction rate) is constant in the initial stage of drying (represented by a straight line in the coordinate diagram of drying time relative to moisture content), and gradually decreases in the later stage of drying. At this time, in the coordinate diagram of drying time relative to moisture content, the interval in which the moisture content changes linearly is called the "constant rate drying period", and the drying rate during this period is called the "constant rate drying rate". The constant rate drying period depends on the structure of the drying device, the amount of drying object, the air volume, temperature, humidity of the drying medium, etc. The constant rate drying period is preferably defined as a period of 20 minutes after the start of drying, and more preferably defined as a period of 15 minutes after the start of drying. It is most preferred to conduct a preliminary drying experiment based on actual equipment and conditions in advance, and make a sample such as Figure 1 The coordinate diagram shown determines the constant rate drying period. Figure 1 This is a graph showing the moisture content at different drying times when a silica carrier was impregnated with water (impregnation rate 95%) and air-dried at a temperature of 100°C and a wind speed of 13 m / min. Figure 1The period from the start of drying to about 20 minutes can be said to be the constant rate drying period. The constant rate drying rate is defined as the value obtained by dividing the difference (variation) between the amount of water contained in the impregnated body before drying and the amount of water contained in the impregnated body dried until a specified time within the constant rate drying period (15 minutes from the start of drying in Example 1) by the drying time and the mass of the supported catalyst. The mass of the supported catalyst is the total value of the mass of the support and the dehydrate of the heteropolyacid or its salt (a substance obtained by removing hydration water from the heteropolyacid or its salt).
[0076] For example, in the case where the heteropolyacid or its salt is silicotungstic acid, a specific method for calculating the constant rate drying speed is as follows.
[0077] Let the water content of the impregnated body be:
[0078] Mass of supported catalyst (mass of silica carrier + mass of silicotungstic anhydride): C
[0079] Water content (hydration water of silicotungstic acid + water used to prepare heteropolyacid aqueous solution): x
[0080] Assuming that the silicotungstic acid after heating and drying is anhydride (dehydrate), it can be expressed as
[0081] y = (mass before heating and drying - mass after heating and drying) / mass before heating and drying
[0082] =[(C+x)-C] / (C+x)=x / (C+x).
[0083] Drying speed (g H2O / kg supcat ·min) is defined as the moisture content before hot air drying x 0 The moisture content x after drying for a specified time t 1 The difference (g) is divided by the mass C (kg) of the supported catalyst and the drying time t (minutes).
[0084] Drying speed (g H2O / kg supcat ·minute)
[0085] =(x 0 -x 1 ) / (C×t)
[0086] At this time, according to y=x / (C+x), it can be transformed into x=(C×y) / (1-y). Therefore, it becomes
[0087] Drying speed (g H2O / kg supcat ·minute)
[0088] =(x 0 -x 1 ) / (C×t)
[0089] =[(C×y 0 ) / (1-y 0 )-(C×y 1 ) / (1-y 1 )] / (C×t)
[0090] =[y 0 / (1-y 0 )-y 1 / (1-y 1 )] / t.
[0091] Furthermore, in the process of deriving the formula, the mass C of the supported catalyst is offset in the denominator and numerator, and therefore is not included in the formula for the drying rate.
[0092] The constant drying rate in the drying process is 5 to 300 g H2O / kg supcat · minutes, preferably 10 to 150 g H2O / kg supcat · Minutes, more preferably 15 to 50 g H2O / kg supcat In another embodiment, the constant rate drying speed in the drying step is preferably 10 to 270 g / min. H2O / kg supcat · Minutes, more preferably 15 to 240 g H2O / kg supcat ·Minutes. At a constant drying rate of less than 5g H2O / kg supcat When the drying speed exceeds 300 g / min, the heteropolyacid or its salt may not be supported on the support surface. H2O / kg supcat If the reaction time is less than 1 minute, the heteropolyacid or its salt may aggregate, and sufficient catalyst performance may not be obtained.
[0093] As a drying method, common methods such as normal pressure drying and reduced pressure drying using hot air can be adopted. From the viewpoint of cost and the number of operation steps, the pressure in the drying process is preferably normal pressure (atmospheric pressure). The drying medium used in the drying process is preferably air, but it can also be an inert gas such as nitrogen.
[0094] There is no particular restriction on the type of drying device used in the drying process. It is preferred to dry the impregnated body by contacting the drying medium (hot air, etc.) as the circulating airflow. Examples of drying devices include belt dryers and box dryers. It is preferred that the circulating airflow is not circulated but is passed through the dryer in one pass (one time). By setting it to one pass, the drying medium with low humidity can always be in contact with the impregnated body (the carrier carrying the catalyst), thereby increasing the constant rate drying speed.
[0095] The temperature of the drying medium is preferably in the range of 80 to 130° C., more preferably in the range of 100 to 120° C. When the temperature of the drying medium is 80° C. or higher, the drying rate can be maintained at a certain value or higher, and the supporting position of the heteropolyacid or its salt can be biased toward the support surface. On the other hand, when the temperature of the drying medium is 130° C. or lower, the decomposition of the heteropolyacid or its salt can be suppressed.
[0096] When hot air such as air and nitrogen is used as a drying medium, there is no particular restriction on its wind speed, but as a linear velocity, it is preferably in the range of 5 to 100 m / min, more preferably in the range of 10 to 70 m / min. If the linear velocity is more than 5 m / min, the drying speed can be increased, and the supporting position of the heteropolyacid or its salt can be effectively biased toward the carrier surface. On the other hand, if the linear velocity is less than 100 m / min, the catalyst (carrier) can be suppressed from flying in the drying process.
[0097] When air is used as the drying medium, its relative humidity is preferably in the range of 0 to 60% RH, more preferably in the range of 0 to 40% RH, and further preferably in the range of 0 to 20% RH, based on the drying medium temperature when it flows into the drying device. If the humidity of the drying medium is 60% RH or less, the drying speed can be increased, and the supporting position of the heteropolyacid or its salt can be effectively biased toward the carrier surface.
[0098] [Manufacture of ethyl acetate]
[0099] In one embodiment, ethyl acetate can be obtained by reacting acetic acid and ethylene in a gas phase using a heteropolyacid or a salt thereof supported on a silica carrier as a solid acid catalyst. In terms of removing the heat of reaction, acetic acid and ethylene are preferably diluted with an inert gas such as nitrogen. Specifically, by circulating a gas containing acetic acid and ethylene as raw materials in a container filled with a solid acid catalyst, it is contacted with the solid acid catalyst, thereby enabling them to react. From the viewpoint of maintaining the activity of the catalyst, it is preferred to add a small amount of water to the gas containing the raw materials. In one embodiment, the reaction is carried out in the presence of water vapor. However, if too much water is added, the amount of by-products such as alcohols and ethers may also increase. The amount of water added is preferably 0.5 to 15 mol%, more preferably 2 to 8 mol%, based on the molar ratio of water to the total of acetic acid, ethylene and water.
[0100] The ratio of ethylene and acetic acid used as raw materials is not particularly limited. The molar ratio of ethylene to acetic acid is preferably in the range of 1:1 to 40:1, more preferably in the range of 3:1 to 20:1, and even more preferably in the range of 5:1 to 15:1.
[0101] The reaction temperature is preferably in the range of 50°C to 300°C, more preferably in the range of 140°C to 250°C. The reaction pressure is preferably in the range of 0 PaG to 3 MPaG (gauge pressure), more preferably in the range of 0.1 MPaG to 2 MPaG (gauge pressure). In one embodiment, the reaction temperature is 150 to 170°C, and the reaction pressure is 0.1 to 2.0 MPaG.
[0102] There is no particular restriction on the SV (gas space velocity) of the gas containing the raw material. However, if it is too large, the raw material will pass through before the reaction is fully carried out. On the other hand, if it is too small, problems such as reduced productivity may occur. SV (volume of raw material passing through per 1L catalyst in 1 hour (L / L·h = h -1 )) is preferably 500 to 20000h -1 , more preferably 1000 to 10000h -1 .
[0103] Example
[0104] The present invention will be further described with reference to the following Examples and Comparative Examples, but the present invention is not limited to these Examples.
[0105] [Determination of volume density of silica carrier]
[0106] The bulk density of the silica support is measured by the following method.
[0107] 1. Add about 200 mL of carrier into a 1 L graduated cylinder.
[0108] 2. Use KIMTOWEL (registered trademark) or the like as a cushioning material, tap it on the table 20 times to tightly fill the carrier.
[0109] 3. Repeat steps 1 and 2 above several times.
[0110] 4. When the volume of the carrier reaches about 1L, add a small amount of carrier each time and repeat step 2.
[0111] 5. Measure 1L of carrier and determine its mass.
[0112] 6. Perform operations 1 to 5 three times in total, and take the average value of the mass as the bulk density (g / L).
[0113] [Determination of saturated water absorption capacity of silica carrier]
[0114] The saturated water absorption capacity of the silica support is measured at room temperature (23° C.) by the following measurement method.
[0115] 1. Weigh about 5 g (W1 g) of the carrier and place it in a 100 mL beaker.
[0116] 2. Add about 15 mL of pure water into the beaker in such a way that the carrier is completely covered.
[0117] 3. Leave it for 30 minutes.
[0118] 4. Place the contents of the beaker onto a metal net with a smaller mesh than the carrier and rinse off the pure water.
[0119] 5. Use a paper towel to gently press the water attached to the surface of the carrier to remove it until the surface gloss disappears.
[0120] 6. Determine the mass of the carrier after absorbing water (W2g).
[0121] 7. Calculate the saturated water absorption capacity of the carrier by the following formula.
[0122] Saturated water absorption capacity (volume of absorbed water (L) / apparent volume of carrier (L))
[0123] =[(W2-W1)(g) / density of water at 23°C (g / L)]×volume density of carrier (g / L) / W1(g)
[0124] [Permeation rate]
[0125] Impregnation rate (%)
[0126] = 100 × volume of heteropolyacid aqueous solution absorbed by the carrier of apparent volume 1L / saturated water absorption capacity of the carrier
[0127] [Calculation method of constant drying speed]
[0128] 1. Take a sample of about 5 g of the impregnated body and measure its water content using a heating balance.
[0129] 2. The impregnated body is dried under specified conditions. During the fixed rate drying period, about 5 g of a supported catalyst (catalyst component + carrier) sample is taken out and its water content is measured using a heating balance.
[0130] 3. The amount of water removed by drying (g) obtained from the water content in steps 1 and 2 is divided by the drying time (minutes) and the mass of the supported catalyst (kg) to calculate the constant drying rate (g). H2O / kg supcat ·minute).
[0131] The drying conditions using a heating balance (heating drying moisture meter, model: MF-50, manufactured by A&D Co., Ltd.) were: temperature: 200° C., and end condition: when the moisture content changes to 0.05% / min.
[0132] The moisture content of the impregnated body is calculated by the above calculation formula. The impregnated body before heat drying (before the measurement of moisture content) contains hydrated water of the heteropoly acid or its salt. The drying temperature of the heating balance is 200°C, and the hydrated water is removed after heat drying (after the measurement of moisture content), and the heteropoly acid or its salt is assumed to be a dehydrate. That is, the impregnation mass before heat drying = hydrate of heteropoly acid or its salt + silica carrier + water used to prepare the heteropoly acid aqueous solution, and the mass of the supported catalyst after heat drying = dehydrate of heteropoly acid or its salt + silica carrier.
[0133] [Example 1]
[0134] (Preparation of Catalyst A)
[0135] 120 g of commercially available Keggin-type silicotungstic acid 26 hydrate (H 4 S W 12 O 40 ·26H 2 O; manufactured by Japan Inorganic Chemical Industry Co., Ltd.) was dissolved in 75.8 g (75.8 mL) of pure water to prepare 108 mL (95% by volume of the saturated water absorption capacity of the carrier, impregnation rate 95%) of silicotungstic acid aqueous solution. Then, the obtained aqueous solution was added to 0.3 L (134 g) of commercially available silica carrier A (spherical, diameter about 5 mm, volume density 451 g / L, saturated water absorption capacity 379 g / L, BET specific surface area 280 m 2 / g) and stirred thoroughly to impregnate the carrier. After air drying for 1 hour, the impregnated body was dried in a ventilation box-type hot air dryer (experimental ventilation shed dryer, model: LABO-4CS, manufactured by Nagato Electric Works Co., Ltd.) with the hot air temperature set to 100°C and the wind speed set to 13m / min to obtain Catalyst A. The constant rate drying rate was calculated by sampling 15 minutes after the start of drying. The values of the constant rate drying rate are shown in Table 1.
[0136] [Example 2]
[0137] (Preparation of Catalyst B)
[0138] The impregnation body was obtained in the same manner as in Example 1 except that the amounts of silicotungstic acid, pure water and silica carrier used were changed to 36.6 kg, 22.7 kg and 90 L, respectively. The impregnation body was dried in the same manner as in Catalyst A except that the hot air temperature was changed to 100° C. and the air speed was changed to 30 m / min to obtain Catalyst B. The values of the constant rate drying speed are shown in Table 1.
[0139] [Example 3]
[0140] (Preparation of Catalyst C)
[0141] The procedure of Example 2 was repeated except that the hot air velocity was changed to 60 m / min to obtain Catalyst C. The values of the constant rate drying speed are shown in Table 1.
[0142] [Example 4]
[0143] (Preparation of Catalyst D)
[0144] The procedure of Example 3 was repeated except that the hot air temperature was changed to 120° C. to obtain Catalyst D. The values of the constant rate drying speed are shown in Table 1.
[0145] [Example 5]
[0146] (Preparation of Catalyst E)
[0147] The procedure of Example 1 was repeated except that the hot air temperature was changed to 130° C. and the air speed was changed to 98 m / min to obtain Catalyst E. The values of the constant rate drying speed are shown in Table 1.
[0148] [Example 6]
[0149] (Preparation of Catalyst F)
[0150] 120 g of commercially available Keggin-type silicotungstic acid 26 hydrate (H 4 S W 12 O 40 ·26H 2O; manufactured by Japan Inorganic Chemical Industry Co., Ltd.) was dissolved in 73.3 g (73.3 mL) of pure water to prepare 105.5 mL (95% by volume of the saturated water absorption capacity of the carrier, impregnation rate 95%) of silicotungstic acid aqueous solution. Then, the obtained aqueous solution was added to 0.3 L (144 g) of commercially available silica carrier B (spherical, diameter about 5 mm, volume density 480 g / L, saturated water absorption capacity 370 g / L, BET specific surface area 147 m 2 / g) and stirred thoroughly to impregnate the support. Then, the same operation as in Example 1 was repeated to obtain Catalyst F. The values of the constant rate drying speed are shown in Table 1.
[0151] [Comparative Example 1]
[0152] (Preparation of Catalyst G)
[0153] The procedure of Example 1 was repeated except that the dryer was changed to a natural convection box dryer (constant temperature dryer, model: DSR420DA, manufactured by Toyo Seisakusho Co., Ltd.) set at 100°C to obtain Catalyst G. The values of the constant rate drying speed are shown in Table 1.
[0154] [Comparative Example 2]
[0155] (Preparation of Catalyst H)
[0156] The procedure of Example 1 was repeated except that the hot air temperature was changed to 50° C. and the air speed was changed to 9 m / min to obtain Catalyst H. The values of the constant rate drying speed are shown in Table 1.
[0157] [Comparative Example 3]
[0158] (Preparation of Catalyst I)
[0159] The procedure of Example 1 was repeated except that the impregnation rate was changed to 70%, thereby obtaining Catalyst I. The values of the constant rate drying speed are shown in Table 1.
[0160] [Comparative Example 4]
[0161] (Preparation of Catalyst J)
[0162] 0.3 L (144 g) of carrier B was impregnated with the silicotungstic acid aqueous solution in the same manner as in Example 6. After air drying for 1 hour, the carrier was dried in the same manner as in Comparative Example 1 to obtain catalyst J. The values of the constant rate drying speed are shown in Table 1.
[0163] [EPMA analysis]
[0164] In order to confirm the loading position of the active ingredient, the tungsten concentration distribution of the catalysts of Example 1 and Comparative Example 1 was measured by EPMA analysis. As a pretreatment of the test sample, the sample was cut with a knife, the cross section was roughly ground with abrasive paper #400, #1000, and #1500 in this order, and the test surface was finely processed with #2000. The results obtained are as follows: Figure 1 and Figure 2 EPMA analysis was performed using the following apparatus and conditions.
[0165] Device: JXA-8530F (manufactured by JEOL Ltd.)
[0166] Accelerating voltage: 15 kV
[0167] WDS mapping (line analysis): WM line 3ch (PET)
[0168] Irradiation current: 1×10 -7 A
[0169] Measurement time: 50ms
[0170] Beam diameter: 10 μm
[0171] Pixel size: 15μm
[0172] Line analysis width: about 0.2mm
[0173] [Manufacture of ethyl acetate]
[0174] 40 mL of each catalyst obtained in the above examples and comparative examples was filled into a stainless steel reaction tube with an inner diameter of 25 mm, and the pressure was increased to 0.75 MPaG, and the temperature was increased to 155°C. At SV (the volume of raw material passing through 1 L of catalyst in 1 hour (L / L·h=h -1 ))=1500h -1 Under the conditions of SV = 1500h, a mixed gas of 85.5 mol% nitrogen, 10.0 mol% acetic acid and 4.5 mol% water was treated for 30 minutes. -1 A mixed gas of 78.5 mol % ethylene, 10 mol % acetic acid, 4.5 mol % water and 7.0 mol % nitrogen was introduced under the conditions of , and the reaction was carried out for 5 hours. The reaction was carried out by adjusting the reaction temperature so that the part with the highest temperature among the 10 parts of the catalyst layer reached 165.0°C. The gas passing through between 3 hours and 5 hours from the start of the reaction was condensed and recovered with cooling water (hereinafter referred to as "condensate") and analyzed. In addition, for the uncondensed gas that remained without condensation (hereinafter referred to as "uncondensed gas"), the gas flow rate at the same time as the condensate was measured, and 100 mL of it was taken out for analysis. The reaction results obtained are shown in Table 1.
[0175] [Analysis method of condensate]
[0176] The internal standard method was used. 1 ml of 1,4-dioxane was added as an internal standard to 10 mL of the reaction solution, and 0.2 μL of the solution was injected as the analysis solution. The analysis was performed under the following conditions.
[0177] Gas chromatograph: 7890B manufactured by Agilent Technologies
[0178] Column: Capillary column DB-WAX (length 30m, inner diameter 0.32mm, film thickness 0.5μm)
[0179] Carrier gas: nitrogen (split ratio 200:1, column flow rate 0.8mL / min)
[0180] Temperature conditions: detector temperature was 250°C, vaporizer temperature was 200°C, column temperature was maintained at 60°C for 5 minutes from the start of analysis, then increased to 80°C at a rate of 10°C / min, and then increased to 200°C at a rate of 30°C / min after reaching 80°C, and maintained at 200°C for 20 minutes.
[0181] Detector: FID(H 2 Flow rate 40mL / min, air flow rate 450mL / min)
[0182] [Analysis method of non-condensed gas]
[0183] Using the absolute calibration curve method, 100 mL of uncondensed gas was prepared and the total amount was flowed into the 1 ml gas sampler attached to the gas chromatograph and analyzed under the following conditions.
[0184] 1. Ethyl acetate
[0185] Gas chromatograph: 7890A manufactured by Agilent Technologies
[0186] Column: Agilent J&W GC column DB-624
[0187] Carrier gas: He (flow rate 1.7mL / min)
[0188] Temperature conditions: detector temperature was 230°C, vaporizer temperature was 200°C, column temperature was maintained at 40°C for 3 minutes from the start of analysis and then increased to 200°C at a rate of 20°C / min.
[0189] Detector: FID(H 2 Flow rate 40mL / min, air flow rate 400mL / min)
[0190] 2. Butene
[0191] Gas chromatograph: 7890A manufactured by Agilent Technologies
[0192] Column: SHIMADZU GC GasPro (30m), Agilent J&W GC column HP-1 Carrier gas: He (flow rate 2.7mL / min)
[0193] Temperature conditions: detector temperature was 230°C, vaporizer temperature was 200°C, column temperature was maintained at 40°C for 3 minutes from the start of analysis and then increased to 200°C at a rate of 20°C / min.
[0194] Detector: FID(H 2 Flow rate 40mL / min, air flow rate 400mL / min)
[0195] Figure 2 (Example 1) and Figure 3 (Comparative Example 1) shows the tungsten concentration distribution of each catalyst obtained by EPMA analysis. Figure 2 and Figure 3 It is found that by increasing the constant rate drying speed of the impregnated body, the supported position of the heteropolyacid or its salt can be shifted to the outside of the support.
[0196] Table 1 shows the catalyst performance results when ethyl acetate was produced. Comparison of Examples 1 to 5 with Comparative Examples 1 and 2, which have the same carrier, shows that increasing the constant rate drying rate increases the space-time yield of ethyl acetate and decreases the selectivity of butene as a by-product. In particular, Figure 4 As shown, it can be seen that there is a correlation between the constant rate drying speed and the butene selectivity. Since butene, one of the main by-products in this reaction, becomes the cause of catalyst coking, from the perspective of catalyst life, the smaller the butene selectivity, the better. The difference in butene selectivity of each catalyst in the short-term evaluation in this embodiment is about 0.00%, but considering that more than tens of thousands of tons of ethyl acetate are produced each year under long-term operation in actual manufacturing, it can be said that it is a significant difference. In addition, it can be seen that in Comparative Example 3 with an impregnation rate of less than 80%, compared with Examples 1 and 2 with the same carrier and similar constant rate drying rates, the space-time yield of ethyl acetate is reduced, and the butene selectivity is increased (deteriorated).
[0197] Table 1
[0198]
[0199] Industrial Applicability
[0200] The production method of the present invention can provide a catalyst for producing ethyl acetate with high productivity, in which the active component is present near the surface of the carrier and which exhibits high catalytic performance, and is therefore industrially useful.
Claims
1. A method for producing a catalyst for producing ethyl acetate, comprising the following steps in sequence: (1) an impregnation step of impregnating a silica support with an aqueous solution of a heteropolyacid or a salt thereof at 80 to 105% by volume of the saturated water absorption capacity of the support to form an impregnated body; and (2) 10 to 270 g H2O / kg supcat A drying step of drying the impregnated body at a constant drying rate of minutes.
2. The method for producing a catalyst for producing ethyl acetate according to claim 1, wherein the constant drying rate in the drying step is 10 to 150 g H2O / kg supcat ·minute.
3. The method for producing a catalyst for producing ethyl acetate according to claim 1 or 2, wherein the constant rate drying rate in the drying step is 15 to 50 g / cm2. H2O / kg supcat ·minute.
4. The method for producing a catalyst for producing ethyl acetate according to claim 1 or 2, wherein the temperature of the drying medium used in the drying step is 80 to 130°C.
5. The method for producing a catalyst for producing ethyl acetate according to claim 1 or 2, wherein the drying medium in the drying step is air having a relative humidity of 0 to 60% RH, and the air is brought into contact with the impregnated body as a circulating airflow to dry the impregnated body.
6. The method for producing a catalyst for ethyl acetate production according to claim 1 or 2, wherein the pressure in the drying step is normal pressure.
7. A method for producing ethyl acetate, comprising reacting ethylene and acetic acid as raw materials in the presence of a catalyst for producing ethyl acetate produced by the method according to any one of claims 1 to 6.