Hydrophobic lithium-type oxygen-generating molecular sieve adsorbent, preparation method and application thereof
By performing organosilane coupling and surface modification on the lithium molecular sieve adsorbent, the problems of deactivation by water absorption and easy breakage are solved, the adsorption and separation performance is improved, and the preparation cost is reduced, making it suitable for industrial applications.
Patent Information
- Application Number
- CN202310100767.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-10
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-02-10
AI Technical Summary
Existing lithium molecular sieve adsorbents are easily deactivated by water absorption and easily broken, resulting in reduced adsorption and separation performance. The preparation process is complex and costly, making it difficult to achieve industrialization.
Organosilanes with different hydrophobicities are coupled on the surface of zeolite molecular sieves to prepare hydrophobic lithium oxygen-generating molecular sieve adsorbents. Small spherical agglomerates are prepared through agglomeration technology, and the adsorbent's performance is improved through lithium ion exchange and surface modification. stability and performance.
It overcomes the problems of water absorption and fragmentation of lithium molecular sieve adsorbents, improves adsorption and separation performance, reduces preparation costs, is suitable for large-scale industrial production, and ensures the production efficiency of the PSA air separation process.
Smart Images

Figure BDA0004085657700000051 
Figure BDA0004085657700000052 
Figure BDA0004085657700000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of molecular sieve adsorbent aggregates, and in particular relates to a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent and a preparation method and application thereof. Background Art
[0002] The interaction between the cations on the zeolite molecular sieve and the quadrupole moment of the nitrogen molecule is strong, so the adsorption capacity of nitrogen on the molecular sieve is stronger than that of oxygen (the ratio of the adsorption amount of the pure components is greater than 2), which is why molecular sieves can be used for PSA air separation oxygen production. The traditional oxygen-enriched adsorbents 5A and 13X molecular sieves have severely restricted the development of PSA oxygen production technology due to their small nitrogen adsorption capacity and low nitrogen-oxygen separation coefficient. Compared with traditional oxygen-enriched adsorbents, the new air separation oxygen-enriched adsorbent has greatly improved the adsorption capacity of nitrogen and the separation coefficient of oxygen and nitrogen, making a qualitative leap in the comprehensive technical and economic indicators of the PSA oxygen production device.
[0003] Because Li + It is the metal ion with the smallest radius among all elements, has a very high charge density, and has the strongest reaction with nitrogen. Therefore, the commonly used oxygen-generating adsorbents are lithium-exchanged 5A, 13X and LSX molecular sieves, especially LiX and LiLSX molecular sieves.
[0004] Patent CN1302687A discloses a method for preparing an adsorbent by exchanging X-type zeolite with a preferred Si / Al atomic ratio of 0.9-1.1 with cations. The zeolite suspension is first exchanged with other cations and then with lithium ions. After the exchange, the zeolite contains about 50-95% lithium ions, about 4-50% single or mixed trivalent ions, and less than 15% sodium, potassium, ammonium or hydronium ions. However, this method cannot control the high exchange rate of lithium ions. Patent US5268023 points out that the adsorption capacity of LiX molecular sieve will only increase rapidly when the exchange degree is greater than 70%. Patent US4859217 reports that the starting material is sodium X zeolite, and the lithium exchange degree must be greater than 88%. When Li + When the exchange degree is 99%, the adsorption capacity of nitrogen under normal pressure can reach 1.03mmol / g, which is equivalent to 23.07ml / g. + The exchange degree becomes the key to efficient oxygen production adsorbent.
[0005] Patent CN102160990A discloses a method for preparing a lithium-type oxygen-generating adsorbent, comprising the following steps: mixing the molecular sieve to be modified with a lithium salt aqueous solution in a molar ratio of 1:1-6, and the molar concentration of the lithium salt aqueous solution is 0.4-4 mol / L; the exchange pressure of the mixed suspension is 0.04MPa-0.26MPa, the temperature is 110°C-140°C, and the exchange is performed 2-4 times, with each exchange time being 2h-10h; by increasing the pressure and temperature of the molecular sieve exchange system, the exchange rate between the molecular sieve and the metal ions and the utilization efficiency of the exchanged metal ions are increased, thereby increasing the adsorption capacity of the molecular sieve for nitrogen.
[0006] Patent CN101125664A proposes an ion exchange method that alternates aqueous solution exchange and high-temperature solid phase roasting exchange. First, at 90°C, a LiCl solution with a molar concentration of 0.4 mol / L is used for exchange twice, each time for 2 hours, and the exchange degree can reach more than 86.6%. Then, the solid phase exchange method is used according to the molar ratio of sodium ions to lithium ions in the zeolite molecular sieve of 1:1.5, and the temperature is kept at 350°C for 180 minutes. Finally, the exchange degree can reach more than 96%. Although this method of combining aqueous solution exchange with solid phase roasting exchange solves the problem of waste of potassium salt in the later exchange, the mixing of solid phases will inevitably lead to uneven distribution of lithium salts and molecular sieves, which also leads to uneven exchange of molecular sieves. In addition, the salt exchanged from the molecular sieve may also enter the cage in the molecular sieve at high temperature. If the washing is not thorough, it will lead to a decrease in the adsorption performance of the molecular sieve.
[0007] Patent CN 101766987A discloses a method for preparing a lithium-modified low-silicon aluminum X-type molecular sieve adsorbent, and proposes a modification method of alternating exchange and calcination, first obtaining a LSX molecular sieve that is double-crossed and double-calcined, and finally exchanging it with a LiCl solution with a molar concentration of 1.8 mol / L at 100°C for 4 hours, and filtering and washing to obtain a Li-LSX molecular sieve raw powder with a Li exchange degree of 95.3%. Although the method of alternating exchange and calcination can improve the stability of the molecular sieve framework and reduce the damage to the molecular sieve framework by subsequent treatment processes, this method of calcining after each exchange obviously makes the entire modification process complicated and increases energy consumption. Obviously, this complex process is difficult to implement in large-scale industrial production.
[0008] Patent US4557736 reported X zeolite molecular sieve exchanged with divalent cations calcium and strontium, claiming that it has high nitrogen adsorption and good nitrogen selectivity in air separation, but strontium resources are scarce and expensive. Patent CN1034913 reported the application of potassium X zeolite oxygen and nitrogen separation adsorbent exchanged with divalent cations, which improved the oxygen and nitrogen separation capacity, and divalent cation selection white Ba 2+ ,Co 2+ , Cu2+ ,Cr 2+ , Fe 2+ Mg 2+ ,Mn 2+ 、Zn 2+ However, Li is still the main component, Li is expensive, and the preparation process is complicated, and the Li utilization rate is low, which makes the adsorbent cost high.
[0009] Due to Li + It is easy to form hydrated ions in aqueous solution, which makes it difficult to exchange with metal ions on the molecular sieve framework. In order to improve its exchange rate, the traditional atmospheric pressure hydrothermal exchange method is often based on extending the exchange time, increasing the number of exchanges, and increasing the amount of exchange metal salts. It consumes a lot of energy, produces a lot of waste liquid, and is difficult to industrialize. In addition, the exchanged lithium ion molecular sieve adsorbent is loaded into the PSA oxygen production device. It is easy to absorb water vapor in the air during long-term operation. Water molecules are easily adsorbed on Li + The active sites of the molecular sieve reduce the ability to adsorb N2 molecules, which ultimately reduces the oxygen output concentration to below industry and national standards and greatly shortens the oxygen production life of the molecular sieve. Therefore, how to reduce the ability of such molecular sieve adsorbents to adsorb water molecules is a key performance issue.
[0010] Although there are many reports in the literature on cation exchange X zeolite with greatly improved nitrogen adsorption performance, especially high exchange degree lithium exchange X zeolite with good nitrogen adsorption performance is known. However, it is difficult to prepare high exchange degree lithium exchange X zeolite and it is expensive, which makes the adsorbent cost very high. In reality, it is necessary to provide a pressure swing adsorption air separation oxygen production adsorbent with low cost and good oxygen and nitrogen separation performance. Summary of the invention
[0011] The purpose of the present invention is to provide a hydrophobic lithium-type oxygen-generating molecular sieve adsorbent and its preparation method and application, the purpose is to solve the problem that the lithium-type small ball adsorbent is easy to absorb water and deactivate and easy to break and reduce activity, and to provide a simple and easy method suitable for hydrophobic modification of molecular sieve adsorbents. Organic silanes with different hydrophobicities are selected and coupled on the surface of zeolite molecular sieves to obtain zeolite molecular sieve adsorbents with different hydrophobicities, which overcomes the problem of water absorption and deactivation of lithium-type molecular sieve adsorbents in the prior art during contact with air, and solves the problem that the adsorbent is broken during operation and reduces the adsorption and separation performance.
[0012] In order to solve the above technical problems, the technical solution of the present invention is:
[0013] In a first aspect, the present invention provides a method for preparing a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent, which is carried out according to the following steps:
[0014] (1) Mixing molecular sieve raw powder, binder and additive in a mass ratio of (82-92): (7.5-15): (0.15-3.0) to obtain a mixed powder; forming the mixed powder into a small ball agglomerate with a ball diameter of less than 1 mm, and then sieving the particle size Agglomerates of small globules;
[0015] (2) The pellet agglomerates are first dried at room temperature for a period of time, then heated and dried at 80-120°C to make the dry basis weight ratio >80%, and then calcined at 100-550°C to obtain a formed sodium sieve pellet adsorbent with a dry basis weight ratio >98%;
[0016] (3) saturating the sodium sieve ball adsorbent with water in an environment at a temperature of 25-30° C. so that the moisture content in the adsorbent is ≥20wt%, and then wetting it in deionized water to prepare a wetted material; exchanging lithium ions with a soluble lithium salt solution to control the lithium exchange degree to be greater than 97% to obtain a lithium exchange material; washing the lithium exchange material with a LiOH solution with a pH value of 8-10 to obtain a washed material;
[0017] (4) dissolving a hydrophobic organosilane in toluene to prepare an organosilane-toluene solution; adding the washed material to the organosilane-toluene solution for surface modification to obtain a surface-modified adsorbent; after unloading the surface-modified adsorbent, first air-dry it at room temperature, then heat and dry it at 80-120° C., controlling the dry basis of the surface-modified adsorbent to be ≥85%, to obtain lithium adsorbent pellets;
[0018] (5) The lithium adsorbent beads are dehydrated and activated by controlling the temperature to rise to 100-550° C. under negative pressure, and the water content of the lithium adsorbent beads is controlled to be ≤0.5 wt %, and then the temperature is lowered to 80-120° C. in an isolated water vapor environment to obtain a hydrophobic lithium-type oxygen-generating molecular sieve adsorbent.
[0019] In the above step (1), the molecular sieve raw powder is one or more of X zeolite, EMT zeolite, RHO molecular sieve, ZSM-3, ZSM-5, mordenite, and clinoptilolite. Preferably, it is X zeolite, the X zeolite has a molar ratio of silicon to aluminum of 2.0-2.2, and the content of K2O is ≤0.5wt%.
[0020] In the above step (1), the binder is one or more of attapulgite, kaolin, eucalyptus, high clay, halloysite, terephthalite and bentonite.
[0021] In the above step (1), the auxiliary agent is one or more of bayberry gum, sesbania powder, SG plant gum, cellulose, sodium carboxymethyl cellulose, polyethylene glycol PEG, polyvinyl alcohol PVA, methyl cellulose and its derivatives, acrylic emulsion, anhydrous sodium pyrophosphate, and starch.
[0022] In the above step (2), The pellet aggregates are first dried at room temperature for 4-24 hours.
[0023] In the above step (3), the lithium salt in the soluble lithium salt solution includes any one of lithium chloride, lithium nitrate, lithium sulfate and lithium hydroxide.
[0024] In the above step (3), the lithium ion concentration in the soluble lithium salt solution is 0.3-3.0 mol / L, preferably 0.5-2.5 mol / L.
[0025] In the above step (3), the wetted material is placed in an exchange tank and heated for 0.5-5 hours. -1 The soluble lithium salt solution is input at a space velocity (LHSV) to exchange lithium ions with the wetted material; preferably, the exchange degree is controlled to be >98%.
[0026] In the above step (4), the organosilane in the organosilane-toluene solution has the structural formula of RnSiX 4-n , wherein R=alkyl or aryl or benzyl, X=Cl or alkoxy, n=0 to 4; the mass concentration of the organosilane is 0.2-5%.
[0027] In the above step (4), in the organosilane-toluene solution, the organosilane includes at least one of 3-chloropropyltrimethoxysilane, phenyltrimethoxysilane, methylphenyldimethoxysilane, chloromethyltrimethoxysilane, diphenyldimethoxysilane, diisobutyldimethoxysilane, 3-chloropropylmethyldimethoxysilane, isobutylisopropyldimethoxysilane, ethyltrimethoxysilane, styreneethyltrimethoxysilane, 4-(chloromethyl)phenyltrimethoxysilane, chloromethylmethyldimethoxysilane, methylphenyldichlorosilane, phenyldimethylchlorosilane, benzyldimethylchlorosilane, 3-chloropropyltrichlorosilane, 3-chloropropylmethyldichlorosilane, 2-phenylpropyltrichlorosilane, dimethyloctylchlorosilane, phenethyltrichlorosilane, benzyltrichlorosilane and dichlorophenyltrichlorosilane.
[0028] In the above step (4), the washed material is heated for 0.5-5 hours. -1 The surface is modified by introducing an organosilane-toluene solution at an air velocity, wherein the volume of the organosilane-toluene solution used is 5-20 times the volume of the washed material.
[0029] In a second aspect, the present invention provides a hydrophobic lithium-type oxygen-generating molecular sieve adsorbent obtained by the above-mentioned preparation method. The particle size diameter of the molecular sieve adsorbent is Particle abrasion rate <0.3%, 1.0cm 3The particle accumulation of the molecular sieve adsorbent has a breakage rate of ≤3% and ≤8% respectively under a pressure of 150N and 250N for 5s; the nitrogen and oxygen separation coefficient is ≥6.0, and the N2 gas adsorption capacity is ≥21ml / g at 1atm; the water droplet contact angle on the surface is ≥90°, and the surface is hydrophobic.
[0030] In a third aspect, the present invention also provides an application of a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent in a PSA / VPSA oxygen production process, wherein the application includes: using the molecular sieve adsorbent to adsorb nitrogen in the air during the nitrogen and oxygen separation process to obtain high-purity O2.
[0031] The beneficial effects of the present invention are as follows: 1. The present invention adopts agglomeration technology to prepare small ball agglomerates, and the agglomeration technology includes but is not limited to extrusion spheronization or disc granulation or disc granulation. The product is then roasted to strengthen the agglomerate, solidify the binder and remove any removable components used during the previous stage, thereby obtaining a shaped sodium sieve ball with good stability and high quality, which provides a guarantee for the subsequent modification of the shaped sodium sieve ball.
[0032] 2. The present invention further exchanges the formed sodium sieve beads with lithium metal ions and controls the lithium exchange degree to be greater than 97% to improve the utilization efficiency of the exchange metal ions and the adsorption capacity of the molecular sieve for nitrogen. In addition, the improvement in the utilization efficiency of the exchange metal ions can reduce waste liquid while simplifying the waste liquid recovery process, reducing environmental pollution and preparation costs.
[0033] 3. The present invention uses hydrophobic organosilane to couple on the surface of zeolite molecular sieve to obtain a zeolite molecular sieve adsorbent with hydrophobic properties, so as to overcome the problem of water absorption and deactivation of lithium-type molecular sieve adsorbents in the prior art during contact with air, and solve the problem of adsorbent breakage during operation and use, which reduces the adsorption and separation performance.
[0034] 4. The preparation method of the present invention is universal for almost all zeolite molecular sieve adsorbents, and the entire process is simple and easy to operate, with mild conditions, and is suitable for large-scale industrial production.
[0035] 5. When the molecular sieve adsorbent of the present invention is applied to the air separation process, it has both high stability and high separation performance, and can fully guarantee the production efficiency of the PSA air separation process. DETAILED DESCRIPTION
[0036] The embodiments of the present invention and the effects produced are further illustrated by examples and comparative examples, but the protection scope of the present invention is not limited to the contents listed in the examples.
[0037] The space velocity in the embodiment of the present invention is LHSV (volume space velocity).
[0038] In the embodiment of the present invention, the lithium exchange material is washed with a LiOH solution with a pH value of 8-10 to obtain a washed material: the free lithium salt solution is washed out by LiOH; the exchanged lithium ions are reduced from being released from the adsorption sites during the washing process, and the lithium ions are also reduced from being absorbed by H + Ion exchange: After washing, the free lithium salt solution between the pores of the adsorbent is replaced, and the excess lithium salt solution can be recycled and applied to the lithium ion exchange process.
[0039] In the embodiment of the present invention, the lithium exchange material is washed with a LiOH solution with a pH value of 8-10, and the lithium exchange material is washed by a column washing method to ensure that the OH - The concentration of other anions besides ions is <200ppm, and the concentration of anions such as chloride ions and sulfate ions is lower than 200ppm as a sign.
[0040] In the embodiment of the present invention, the nitrogen-oxygen separation coefficient (ratio) α and the adsorption capacity are measured:
[0041] 1) According to the static determination method of nitrogen and oxygen separation of molecular sieves (GB / T 35109-2017); the nitrogen and oxygen separation coefficient (ratio) α is the ratio of the equilibrium adsorption amount of nitrogen and oxygen in the adsorption phase to the equilibrium molar fraction of nitrogen and oxygen in the gas phase;
[0042]
[0043] In formula (1), X is the equilibrium adsorption amount of the adsorbate in the adsorption phase; Y is the equilibrium mole fraction of the adsorbate in the gas phase;
[0044] 2) The adsorption amount (X and Y) of nitrogen and oxygen by the molecular sieve sample at different partial pressures is determined by the static adsorption capacity method; the capacity method uses the gas state equation (i.e., pV=nRT) to calculate the adsorption amount of the gas by the adsorbent by measuring the pressure p and volume V of the gas before and after contact with a certain mass of the adsorbent at a certain temperature.
[0045] Molecular sieve nitrogen adsorption capacity X N2 , values in cm 3 / g indicates that it is calculated according to (2):
[0046]
[0047] In formula (2): V N2 The value of the nitrogen equilibrium adsorption of the sample under the conditions of 25°C and a set pressure of 79.113 kPa, in cubic centimeters (cm) 3 ;m N2 It is the value of the sample mass when testing the nitrogen adsorption, in grams. The calculation result is expressed to two decimal places.
[0048] Molecular sieve oxygen adsorption capacity X O2 , values in cm 3 / g indicates that it is calculated according to (3)
[0049]
[0050] In formula (3): V O2 The value of the oxygen equilibrium adsorption of the sample under the conditions of 25°C and a set pressure of 21.221 kPa, in cubic centimeters (cm) 3 ;m O2 It is the value of the sample mass when testing the oxygen adsorption, in grams. The calculation result is expressed to two decimal places.
[0051] In the embodiments of the present invention, the hydrophobicity of the adsorbent particles is characterized by:
[0052] Take 0.05g of hydrophobic modified nanoparticles and put them into a small reagent bottle, and use a pipette to add 2.5mL of anhydrous ethanol into the reagent bottle, ultrasonicate and stir to disperse the hydrophobic modified nanoparticles in the ethanol solvent; then take a pre-treated clean slide and use a spraying method to spray the hydrophobic modified nanoparticle ethanol suspension on the surface of the slide; after spraying, put it in a vacuum oven to dry so that the solvent ethanol can be completely evaporated; use a contact angle tester to test the contact angle of its surface.
[0053] In the embodiment of the present invention, the compressive strength test method of the adsorbent pellets is as follows:
[0054] ①Sieve a 20-40 mesh ball adsorbent sample and place it in the air to allow it to adsorb various gases and water vapor in the air until the quality is stable;
[0055] ② Accurately weigh the empty weight of the sample cell G 柱 , sieve out samples above 50 mesh;
[0056] ③ Take 1.0mL of sample and put it into the sample pool, and accurately weigh the total weight of the sample pool and the sample G. 初 ;
[0057] ④ Place the test pin in the sample pool, hold it vertically against the sample and gently rotate it for a circle to compact and level the accumulated sample particles. Press once under a pressure of 150N and pour it out. Sieve through a 50-mesh standard sieve to remove the broken powder. Put the remaining small balls back into the sample pool using a small glass funnel and weigh the total weight G. 150N ;
[0058] ⑤ Calculate the crushing rate of the ball under a pressure of 150N based on the initial weight of the sample and the remaining weight after crushing, which is the crushing rate K of the sample. 150N ; K 150N =(G 初 -G 150N ) / (G 初 -G柱 )*100%;
[0059] Repeat steps ④ and ⑤ of the sample put back into the sample pool under a pressure of 250N to calculate the crushing rate K at 250N. 250N ; K 250N =(G 初 –G 250N ) / (G 初 -G 柱 )*100%; Repeat the determination of the breaking rate K at 150N and 250N for the same adsorbent particle sample 150N and K 250N .
[0060] In the embodiment of the present invention, the molecular sieve attrition rate is detected:
[0061] A certain amount of calcined sample is run in the grinding tube under specified conditions, so that the sample rubs and collides in the tube, and the powderization percentage of the sample is measured to express its wear rate; the measurement steps are as follows:
[0062] ① Use the quartering method to divide the sample into two parts, each part is approximately equal to the amount used for the abrasion test: 25±2g;
[0063] ② Weigh the mass of two porcelain crucibles that have been calcined at 550℃ to a constant weight (accurate to 0.001g), and this mass is M0;
[0064] ③ Pour the two samples into a standard sample sieve with a pore size of 0.85 mm, remove the pre-grinding powder, and transfer them to two weighed porcelain crucibles respectively;
[0065] ④ Place the porcelain crucible and the crucible cover (not on the crucible) into a box-type electric furnace and bake at 550℃ for 2h;
[0066] ⑤Take out the porcelain crucible and put it into the vacuum dryer. Immediately cover the crucible and vacuum dryer lids, turn on the vacuum pump, and when the air pressure is less than 1.0×10 3 Pa, turn off the vacuum pump and cool the sample to room temperature;
[0067] ⑥ Slowly rotate the piston of the vacuum dryer to allow the atmosphere to slowly enter the dryer, open the vacuum dryer, take out the porcelain crucible, and weigh it immediately (accurate to 0.001g). This mass is M1;
[0068] ⑦Immediately load the samples into the two grinding cylinders, tighten the glands, and then install the grinding cylinders symmetrically on the abrasion tester. Start the abrasion tester and the grinding cylinders will start running until they rotate 1000 times.
[0069] ⑧ Remove the sample grinding tube, sieve the sample with a 0.6mm standard sample sieve and pour it back into the original porcelain crucible;
[0070] ⑨ Place the porcelain crucible and the crucible cover (not covering the crucible) into a box-type electric furnace and bake at 550℃ for 1h. Then operate in the same way, weigh the porcelain crucible, grind it and sieve it. The mass of the sample on the sieve after baking (accurate to 0.001g) is M2; the wear rate %X = (M2-M1) / (M1-M0).
[0071] In the embodiment of the present invention, the bulk density of the molecular sieve is determined by using the method for determining the bulk density of the molecular sieve in the national standard GB / T 6286-2021.
[0072] Example 1
[0073] The present embodiment provides a hydrophobic lithium-type oxygen-generating molecular sieve adsorbent and a preparation method thereof. The molecular sieve adsorbent is prepared from initial raw material components and initial auxiliary material components; the initial raw material composition is molecular sieve raw powder, adhesive and auxiliary agent; the mass content of the molecular sieve raw powder is 87%, the mass content of the adhesive is 12%, and the mass content of the auxiliary agent is 1%; the initial auxiliary material components are soluble lithium salt solution and organosilane-toluene solution; in the soluble lithium salt solution, the lithium ion concentration is 0.5 mol / L; the mass concentration of organosilane in the organosilane-toluene solution is 1.5%; after the molecular sieve raw powder is exchanged with lithium, lithium ions occupy 98.83% of the exchangeable cation sites.
[0074] Particle size diameter of molecular sieve adsorbent Particle wear rate 0.21%, 1.0cm 3 The breakage rates of the adsorbent particle accumulation under pressures of 150N and 250N for 5s were 2.4% and 5.5% respectively; the nitrogen and oxygen separation coefficient was 6.36, and the N2 gas adsorption capacity was 22.21ml / g at 1atm; the water droplet contact angle was 105.6°, and the surface was hydrophobic.
[0075] The preparation method of the molecular sieve adsorbent is carried out according to the following steps:
[0076] 1) The molecular sieve raw powder is mixed with the binder and the additive in a mass ratio of 87:12:1 to obtain a mixed powder; then the mixed powder is placed in a rolling ball forming device, deionized water is added during rotation and the dry basis weight ratio of all materials is kept in the range of 70-80%, the ball diameter is controlled to be less than 1 mm, and the particle size is screened to be Agglomerates of small balls;
[0077] The molecular sieve raw powder is X zeolite; the X zeolite has a silicon-aluminum ratio of SiO2 / Al2O3=2.0, wherein the mass content of K2O is less than 0.5%;
[0078] The binder is attapulgite;
[0079] The auxiliary agent is bayberry glue;
[0080] 2) drying the pellet aggregate for 24 hours, then drying at 80-120° C. to obtain a dry basis weight ratio of >80%, and then calcining at 500-550° C. to obtain a formed sodium sieve pellet adsorbent having a dry basis weight ratio of >98%;
[0081] 3) The sodium sieve ball adsorbent is saturated with water in the air to a moisture content of ≥ 20 wt%, and then put into deionized water for wetting to prepare a wetted material; the wetted material is placed in an exchange tank and heated for 0.5 h. -1 Inputting a soluble lithium salt solution at a space velocity to perform lithium ion exchange, controlling the lithium exchange degree to 98.83%, and obtaining a lithium exchange material; washing the lithium exchange material with a LiOH solution with a pH value of 8, and finally obtaining a washed material with a chloride ion concentration lower than 200 ppm;
[0082] In the soluble lithium salt solution, the lithium salt is lithium chloride; the lithium ion concentration is 0.5 mol / L;
[0083] 4) dissolving the organosilane in toluene to prepare an organosilane-toluene solution; the mass concentration of the organosilane in the organosilane-toluene solution is 1.5%; -1 The organic silane-toluene solution is introduced at a space velocity for surface modification, wherein the volume of the organic silane-toluene solution used is 15 times the volume of the washed material, to obtain a surface modified adsorbent; after the surface modified adsorbent is discharged, it is first air-dried, and then dried at 80-120° C., and the dry basis of the surface modified adsorbent is controlled to be ≥85%, to obtain lithium adsorbent beads;
[0084] In the organosilane-toluene solution, the organosilane is 3-chloropropyltrimethoxysilane;
[0085] 5) Controlling the temperature of the lithium adsorbent pellets to 100-550°C under negative pressure programmed temperature dehydration activation (normal pressure pre-calcination furnace temperature: zone 1: 100-200°C, zone 2: 200-300°C, zone 3: 300-400°C; vacuum calcination furnace temperature: zone 1: 350-400°C; zone 2: 400-450°C; zone 3: 450-475°C; zone 4: 475-500°C; zone 5: 500-525°C; zone 6: 525-550°C (the above are furnace wall apparent temperatures, vacuum degree <-50kPa), controlling the water content of the lithium adsorbent pellets to ≤0.5wt%, and then cooling to 80-120°C in an isolated water vapor environment to obtain a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent;
[0086] The types of binders and additives used in Example 1, the weight ratio of the molecular sieves, the types of organosilanes and the exchange multiples of organosilanes are shown in Table 1; the strength, water content, particle size, nitrogen-oxygen separation coefficient, nitrogen adsorption capacity, water drop contact angle and other parameters of the obtained molecular sieve product (having a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent) are shown in Table 2;
[0087] The hydrophobic lithium-type oxygen-generating molecular sieve adsorbent obtained by the above preparation method is used in the PSA / VPSA oxygen-generating process to adsorb a large amount of N2 in the nitrogen-oxygen separation to obtain high-purity O2. The oxygen concentration results after the PSA process on a 5L oxygen generator are shown in Tables 4 and 5.
[0088] Example 2
[0089] The present embodiment provides a hydrophobic lithium-type oxygen-generating molecular sieve adsorbent and a preparation method thereof. The molecular sieve adsorbent is prepared from initial raw material components and initial auxiliary material components; the initial raw material composition is molecular sieve raw powder, adhesive and auxiliary agent; the mass content of the molecular sieve raw powder is 88%, the mass content of the adhesive is 11%, and the mass content of the auxiliary agent is 1%; the initial auxiliary material components are soluble lithium salt solution and organosilane-toluene solution; in the soluble lithium salt solution, the lithium ion concentration is 1.5 mol / L; the mass concentration of organosilane in the organosilane-toluene solution is 0.6%; after the molecular sieve raw powder is exchanged with lithium ions, lithium ions occupy 98.73% of the exchangeable cation sites.
[0090] Particle size diameter of molecular sieve adsorbent Particle wear rate 0.26%, 1.0cm 3 The breakage rates of the adsorbent particle accumulation under 150N and 250N pressure for 5s were 1.7% and 7% respectively; the nitrogen and oxygen separation coefficient was 6.75, and the N2 gas adsorption capacity was 27.08ml / g at 1atm; the water droplet contact angle was 96.6°, and the surface was hydrophobic.
[0091] The preparation method of the molecular sieve adsorbent is carried out according to the following steps:
[0092] 1) The molecular sieve raw powder is mixed with the binder and the additive in a mass ratio of 88:11:1 to obtain a mixed powder; then the mixed powder is placed in a rolling ball forming device, deionized water is added during rotation and the dry basis weight ratio of all materials is kept in the range of 70-80%, the ball diameter is controlled to be less than 1 mm, and the particle size is screened to be Agglomerates of small balls;
[0093] The molecular sieve raw powder is EMT zeolite;
[0094] The binder is kaolin;
[0095] The auxiliary agent is sesbania powder;
[0096] 2) drying the pellet aggregate for 22 hours, then drying at 80-120° C. to obtain a dry basis weight ratio of >80%, and then calcining at 500-550° C. to obtain a formed sodium sieve pellet adsorbent having a dry basis weight ratio of >98%;
[0097] 3) The sodium sieve ball adsorbent is saturated with water in the air to a moisture content of ≥ 20 wt%, and then put into deionized water for wetting to prepare a wetted material; the wetted material is placed in an exchange tank for 1 hour. -1 Inputting a soluble lithium salt solution at a space velocity to perform lithium ion exchange, controlling the lithium exchange degree to 98.73%, and obtaining a lithium exchange material; washing the lithium exchange material with a LiOH solution having a pH value of 9, and finally obtaining a washed material with a sulfate ion concentration lower than 200 ppm;
[0098] In the soluble lithium salt solution, the lithium salt is lithium sulfate; the lithium ion concentration is 1.5 mol / L;
[0099] 4) dissolving the organosilane in toluene to prepare an organosilane-toluene solution; the mass concentration of the organosilane in the organosilane-toluene solution is 0.6%; -1 The surface of the surface-modified adsorbent is modified by introducing an organic silane-toluene solution at an air velocity, wherein the volume of the organic silane-toluene solution used is 10 times the volume of the washed material, and a surface-modified adsorbent is obtained; after the surface-modified adsorbent is discharged, it is first air-dried and then dried at 80-120° C., and the dry basis of the surface-modified adsorbent is controlled to be ≥85%, and a lithium adsorbent pellet is obtained;
[0100] In the organosilane-toluene solution, the organosilane is phenyltrimethoxysilane;
[0101] 5) The lithium adsorbent beads are dehydrated and activated by controlling the temperature to rise to 100-550° C. under negative pressure (the temperature setting is similar to that in Example 1), and the water content of the lithium adsorbent beads is controlled to be ≤0.5wt%, and then the temperature is lowered to 80-120° C. in an isolated water vapor environment to obtain a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent.
[0102] The types of binders and additives used in Example 2, the weight ratio of the molecular sieves, the types of organosilanes and the exchange multiples of organosilanes are shown in Table 1; the strength, water content, particle size, nitrogen-oxygen separation coefficient, nitrogen adsorption capacity, water drop contact angle and other parameters of the obtained molecular sieve product (having a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent) are shown in Table 2;
[0103] The hydrophobic lithium-type oxygen-generating molecular sieve adsorbent obtained by the above preparation method is used in the PSA / VPSA oxygen-generating process to adsorb a large amount of N2 in the nitrogen-oxygen separation to obtain high-purity O2. The oxygen concentration results after the PSA process on a 5L oxygen generator are shown in Tables 4 and 5.
[0104] Example 3
[0105] The present embodiment provides a hydrophobic lithium-type oxygen-generating molecular sieve adsorbent and a preparation method thereof. The molecular sieve adsorbent is prepared from initial raw material components and initial auxiliary material components; the initial raw material composition is molecular sieve raw powder, adhesive and auxiliary agent; the mass content of the molecular sieve raw powder is 89%, the mass content of the adhesive is 10%, and the mass content of the auxiliary agent is 1%; the initial auxiliary material components are soluble lithium salt solution and organosilane-toluene solution; in the soluble lithium salt solution, the lithium ion concentration is 2 mol / L; the mass concentration of organosilane in the organosilane-toluene solution is 0.8%; after the molecular sieve raw powder is exchanged with lithium ions, lithium ions occupy 98.29% of the exchangeable cation sites.
[0106] Particle size diameter of molecular sieve adsorbent Particle wear rate 0.25%, 1.0cm 3 The breakage rates of the adsorbent particle accumulation under 150N and 250N pressures for 5s were 1.5% and 8% respectively; the nitrogen and oxygen separation coefficient was 6.16, and the N2 gas adsorption capacity was 24.06ml / g at 1atm; the water droplet contact angle was 104.6°, and the surface was hydrophobic.
[0107] The preparation method of the molecular sieve adsorbent is carried out according to the following steps:
[0108] 1) The molecular sieve raw powder is mixed with the binder and the additive in a mass ratio of 89:10:1 to obtain a mixed powder; then the mixed powder is placed in a rolling ball forming device, deionized water is added during rotation and the dry basis weight ratio of all materials is kept in the range of 70-80%, the ball diameter is controlled to be less than 1 mm, and the particle size is screened to be Agglomerates of small balls;
[0109] The molecular sieve raw powder is X zeolite; the X zeolite has a silicon-aluminum ratio of 2.2 according to the molecular molar ratio, wherein the mass content of K2O is less than 0.5%;
[0110] The adhesive is terra cotta;
[0111] The auxiliary agent is SG plant gum;
[0112] 2) drying the pellet aggregate for 20 hours, then drying at 80-120° C. to obtain a dry basis weight ratio of >80%, and then calcining at 500-550° C. to obtain a formed sodium sieve pellet adsorbent having a dry basis weight ratio of >98%;
[0113] 3) The sodium sieve ball adsorbent is saturated with water in the air to a moisture content of ≥ 20 wt%, and then put into deionized water for wetting to prepare a wetted material; the wetted material is placed in an exchange tank for 2 h. -1 Inputting a soluble lithium salt solution at a space velocity to perform lithium ion exchange, controlling the lithium exchange degree to 98.29%, and obtaining a lithium exchange material; washing the lithium exchange material with a LiOH solution having a pH value of 10, and finally obtaining a washed material with a chloride ion concentration lower than 200 ppm;
[0114] In the soluble lithium salt solution, the lithium salt is lithium chloride, and the lithium ion concentration is 2 mol / L;
[0115] 4) dissolving the organosilane in toluene to prepare an organosilane-toluene solution; the mass concentration of the organosilane in the organosilane-toluene solution is 0.8%; -1 The surface of the surface-modified adsorbent is modified by introducing an organic silane-toluene solution at an air velocity, wherein the volume of the organic silane-toluene solution used is 8 times the volume of the washed material, and a surface-modified adsorbent is obtained; after the surface-modified adsorbent is discharged, it is first air-dried and then dried at 80-120° C., and the dry basis of the surface-modified adsorbent is controlled to be ≥85%, and a lithium adsorbent pellet is obtained;
[0116] In the organosilane-toluene solution, the organosilane is methylphenyldimethoxysilane;
[0117] 5) The lithium adsorbent beads are dehydrated and activated by controlling the temperature to rise to 100-550° C. under negative pressure (the temperature setting is similar to that in Example 1), and the water content of the lithium adsorbent beads is controlled to be ≤0.5wt%, and then the temperature is lowered to 80-120° C. in an isolated water vapor environment to obtain a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent.
[0118] The types of binders and additives used in Example 3, the weight ratio of the molecular sieves, the types of organosilanes and the exchange multiples of organosilanes are shown in Table 1; the strength, water content, particle size, nitrogen-oxygen separation coefficient, nitrogen adsorption capacity, water drop contact angle and other parameters of the obtained molecular sieve product (having a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent) are shown in Table 2;
[0119] The hydrophobic lithium-type oxygen-generating molecular sieve adsorbent obtained by the above preparation method is used in the PSA / VPSA oxygen-generating process to adsorb a large amount of N2 in the nitrogen-oxygen separation to obtain high-purity O2. The oxygen concentration results after the PSA process on a 5L oxygen generator are shown in Tables 4 and 5.
[0120] Example 4
[0121] The present embodiment provides a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent and a preparation method thereof. The molecular sieve adsorbent is prepared from initial raw material components and initial auxiliary material components; the initial raw material composition is molecular sieve raw powder, adhesive and auxiliary agent; the mass content of the molecular sieve raw powder is 90%, the mass content of the adhesive is 9.85%, and the mass content of the auxiliary agent is 0.15%; the initial auxiliary material components are soluble lithium salt solution and organosilane-toluene solution; in the soluble lithium salt solution, the lithium ion concentration is 2.5 mol / L; the mass concentration of organosilane in the organosilane-toluene solution is 1%; after the molecular sieve raw powder is exchanged with lithium ions, lithium ions occupy 98.08% of the exchangeable cation sites.
[0122] Particle size diameter of molecular sieve adsorbent Particle wear rate 0.24%, 1.0cm 3 The breakage rates of the adsorbent particle accumulation under 150N and 250N pressures for 5s were 2.7% and 4.9% respectively; the nitrogen and oxygen separation coefficient was 6.24, and the N2 gas adsorption capacity was 25.94ml / g at 1atm; the water droplet contact angle was 122.8°, and the surface was hydrophobic.
[0123] The preparation method of the molecular sieve adsorbent is carried out according to the following steps:
[0124] 1) The molecular sieve raw powder is mixed with the binder and the additive in a mass ratio of 90:9.85:0.15 to obtain a mixed powder; then the mixed powder is placed in a rolling ball forming device, deionized water is added during rotation and the dry basis weight ratio of all materials is kept in the range of 70-80%, the ball diameter is controlled to be less than 1mm, and the particle size is screened to be Agglomerates of small balls;
[0125] The molecular sieve raw powder is EMT type zeolite;
[0126] The binder is high clay;
[0127] The auxiliary agent is sodium carboxymethyl cellulose;
[0128] 2) drying the pellet aggregate for 18 hours, then drying at 80-120° C. to obtain a dry basis weight ratio of >80%, and then calcining at 100-550° C. to obtain a formed sodium sieve pellet adsorbent having a dry basis weight ratio of >98%;
[0129] 3) The sodium sieve ball adsorbent is saturated with water in the air to a moisture content of ≥ 20 wt%, and then put into deionized water for wetting to prepare a wetted material; the wetted material is placed in an exchange tank for 3 hours. -1Inputting a soluble lithium salt solution at a space velocity to perform lithium ion exchange, controlling the lithium exchange degree to 98.08%, and obtaining a lithium exchange material; washing the lithium exchange material with a LiOH solution with a pH value of 8, and finally obtaining a washed material with a sulfate ion concentration lower than 200 ppm;
[0130] In the soluble lithium salt solution, the lithium salt is lithium sulfate, and the lithium ion concentration is 2.5 mol / L;
[0131] 4) dissolving the organosilane in toluene to prepare an organosilane-toluene solution; the mass concentration of the organosilane in the organosilane-toluene solution is 1%; -1 The surface of the surface-modified adsorbent is modified by introducing an organic silane-toluene solution at an air velocity, wherein the volume of the organic silane-toluene solution used is 6 times the volume of the washed material, and a surface-modified adsorbent is obtained; after the surface-modified adsorbent is discharged, it is first air-dried and then dried at 80-120° C., and the dry basis of the surface-modified adsorbent is controlled to be ≥85%, and a lithium adsorbent pellet is obtained;
[0132] In the organosilane-toluene solution, the organosilane is chloromethyltrimethoxysilane;
[0133] 5) The lithium adsorbent beads are dehydrated and activated by controlling the temperature to rise to 100-550° C. under negative pressure (the temperature setting is similar to that in Example 1), and the water content of the lithium adsorbent beads is controlled to be ≤0.5wt%, and then the temperature is lowered to 80-120° C. in an isolated water vapor environment to obtain a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent.
[0134] The types of binders and additives used in Example 4, the weight ratio of the molecular sieves, the types of organosilanes and the exchange multiples of organosilanes are shown in Table 1; the strength, water content, particle size, nitrogen-oxygen separation coefficient, nitrogen adsorption capacity, water drop contact angle and other parameters of the obtained molecular sieve product (having a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent) are shown in Table 2;
[0135] The hydrophobic lithium-type oxygen-generating molecular sieve adsorbent obtained by the above preparation method is used in the PSA / VPSA oxygen-generating process to adsorb a large amount of N2 in the nitrogen-oxygen separation to obtain high-purity O2. The oxygen concentration results after the PSA process on a 5L oxygen generator are shown in Tables 4 and 5.
[0136] Example 5
[0137] The present embodiment provides a hydrophobic lithium-type oxygen-generating molecular sieve adsorbent and a preparation method thereof. The molecular sieve adsorbent is prepared from initial raw material components and initial auxiliary material components; the initial raw material composition is molecular sieve raw powder, adhesive and auxiliary agent; the mass content of the molecular sieve raw powder is 91%, the mass content of the adhesive is 8%, and the mass content of the auxiliary agent is 1%; the initial auxiliary material components are soluble lithium salt solution and organosilane-toluene solution; in the soluble lithium salt solution, the lithium ion concentration is 0.5 mol / L; the mass concentration of organosilane in the organosilane-toluene solution is 1.5%; after the molecular sieve raw powder is exchanged with lithium, lithium ions occupy 98.34% of the exchangeable cation sites.
[0138] Particle size diameter of molecular sieve adsorbent Particle wear rate 0.30%, 1.0cm 3 The breakage rates of the adsorbent particle accumulation under 150N and 250N pressures for 5s were 2% and 6.2% respectively; the nitrogen and oxygen separation coefficient was 6.15, and the N2 gas adsorption capacity was 21.45ml / g at 1atm; the water droplet contact angle was 91.5°, and the surface was hydrophobic.
[0139] The preparation method of the molecular sieve adsorbent is carried out according to the following steps:
[0140] 1) The molecular sieve raw powder is mixed with the binder and the additive in a mass ratio of 91:8:1 to obtain a mixed powder; then the mixed powder is placed in a rolling ball forming device, deionized water is added during rotation and the dry basis weight ratio of all materials is kept in the range of 70-80%, the ball diameter is controlled to be less than 1 mm, and the particle size is screened to be Agglomerates of small balls;
[0141] The molecular sieve raw powder is X zeolite; the silicon-aluminum ratio is 2.1 according to the molecular molar ratio, wherein the mass content of K2O is less than 0.5%;
[0142] The binder is halloysite;
[0143] The auxiliary agent is polyethylene glycol PEG;
[0144] 2) drying the pellet aggregate for 16 hours, drying at 80-120° C. to obtain a dry basis weight ratio of >80%, and then calcining at 500-550° C. to obtain a formed sodium sieve pellet adsorbent having a dry basis weight ratio of >98%;
[0145] 3) The sodium sieve ball adsorbent is saturated with water in the air to a moisture content of ≥20wt%, and then put into deionized water for wetting to prepare a wetted material; the wetted material is placed in an exchange tank for 4 hours. -1Inputting a soluble lithium salt solution at a space velocity to perform lithium ion exchange, controlling the lithium exchange degree to 98.34%, and obtaining a lithium exchange material; washing the lithium exchange material with a LiOH solution having a pH value of 9, and finally obtaining a washed material with a chloride ion concentration lower than 200 ppm;
[0146] In the soluble lithium salt solution, the lithium salt is lithium chloride, and the lithium ion concentration is 0.5 mol / L;
[0147] 4) dissolving the organosilane in toluene to prepare an organosilane-toluene solution; the mass concentration of the organosilane in the organosilane-toluene solution is 1.5%; -1 The surface of the surface-modified adsorbent is modified by introducing an organic silane-toluene solution at an air velocity, wherein the volume of the organic silane-toluene solution used is 12 times the volume of the washed material, and a surface-modified adsorbent is obtained; after the surface-modified adsorbent is discharged, it is first air-dried and then dried at 80-120° C., and the dry basis of the surface-modified adsorbent is controlled to be ≥85%, and a lithium adsorbent pellet is obtained;
[0148] In the organosilane-toluene solution, the organosilane is isobutylisopropyldimethoxysilane;
[0149] 5) The lithium adsorbent beads are dehydrated and activated by controlling the temperature to rise to 100-550° C. under negative pressure (the temperature setting is similar to that in Example 1), and the water content of the lithium adsorbent beads is controlled to be ≤0.5wt%, and then the temperature is lowered to 80-120° C. in an isolated water vapor environment to obtain a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent.
[0150] The types of binders and additives used in Example 5, the weight ratio of the molecular sieves, the types of organosilanes and the exchange multiples of organosilanes are shown in Table 1; the strength, water content, particle size, nitrogen-oxygen separation coefficient, nitrogen adsorption capacity, water drop contact angle and other parameters of the obtained molecular sieve product (having a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent) are shown in Table 2;
[0151] The hydrophobic lithium-type oxygen-generating molecular sieve adsorbent obtained by the above preparation method is used in the PSA / VPSA oxygen-generating process to adsorb a large amount of N2 in the nitrogen-oxygen separation to obtain high-purity O2. The oxygen concentration results after the PSA process on a 5L oxygen generator are shown in Tables 4 and 5.
[0152] Example 6
[0153] The present embodiment provides a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent and a preparation method thereof. The molecular sieve adsorbent is prepared from initial raw material components and initial auxiliary material components; the initial raw material composition is molecular sieve raw powder, adhesive and auxiliary agent; the mass content of the molecular sieve raw powder is 86%, the mass content of the adhesive is 13%, and the mass content of the auxiliary agent is 1%; the initial auxiliary material components are soluble lithium salt solution and organosilane-toluene solution; in the soluble lithium salt solution, the lithium ion concentration is 1 mol / L; the mass concentration of organosilane in the organosilane-toluene solution is 2%; the lithium ions in the molecular sieve raw powder occupy 99.28% of the exchangeable cation sites.
[0154] Particle size diameter of molecular sieve adsorbent Particle wear rate 0.23%, 1.0cm 3 The breakage rates of the adsorbent particle accumulation under 150N and 250N pressures for 5s were 0.9% and 5.2% respectively; the nitrogen and oxygen separation coefficient was 6.74, and the N2 gas adsorption capacity was 25.97ml / g at 1atm; the water droplet contact angle was 102.6°, and the surface was hydrophobic.
[0155] The preparation method of the molecular sieve adsorbent is carried out according to the following steps:
[0156] 1) The molecular sieve raw powder is mixed with the binder and the additive in a mass ratio of 86:13:1 to obtain a mixed powder; then the mixed powder is placed in a rolling ball forming device, deionized water is added during rotation and the dry basis weight ratio of all materials is kept in the range of 70-80%, the ball diameter is controlled to be less than 1 mm, and the particle size is screened to be Agglomerates of small balls;
[0157] The molecular sieve raw powder is X zeolite; the silicon-aluminum ratio is 2.2 according to the molecular molar ratio, wherein the mass content of K2O is less than 0.5%;
[0158] The adhesive is decanted soil;
[0159] The auxiliary agent is polyvinyl alcohol (PVA);
[0160] 2) drying the pellet aggregate for 14 hours, then drying at 80-120° C. to obtain a dry basis mass ratio of >80%, and then calcining at 500-550° C. to obtain a formed sodium sieve pellet adsorbent having a dry basis mass ratio of >98%;
[0161] 3) The sodium sieve ball adsorbent is saturated with water in the air to a moisture content of ≥20wt%, and then put into deionized water for wetting to prepare a wetted material; the wetted material is placed in an exchange tank for 5 hours. -1Inputting a soluble lithium salt solution at a space velocity to perform lithium ion exchange, controlling the lithium exchange degree to 99.28%, and obtaining a lithium exchange material; washing the lithium exchange material with a LiOH solution having a pH value of 10, and finally obtaining a washed material with a sulfate ion concentration lower than 200 ppm;
[0162] In the soluble lithium salt solution, the lithium salt is lithium sulfate, and the lithium ion concentration is 1 mol / L;
[0163] 4) dissolving the organosilane in toluene to prepare an organosilane-toluene solution; the mass concentration of the organosilane in the organosilane-toluene solution is 2%; -1 The surface of the surface-modified adsorbent is modified by introducing an organic silane-toluene solution at an air velocity, wherein the volume of the organic silane-toluene solution used is 18 times the volume of the washed material, and a surface-modified adsorbent is obtained; after the surface-modified adsorbent is discharged, it is first air-dried and then dried at 80-120° C., and the dry basis of the surface-modified adsorbent is controlled to be ≥85%, and a lithium adsorbent pellet is obtained;
[0164] In the organosilane-toluene solution, the organosilane is methylphenyldichlorosilane;
[0165] 5) The lithium adsorbent beads are dehydrated and activated by controlling the temperature to rise to 100-550° C. under negative pressure (the temperature setting is similar to that in Example 1), and the water content of the lithium adsorbent beads is controlled to be ≤0.5wt%, and then the temperature is lowered to 80-120° C. in an isolated water vapor environment to obtain a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent.
[0166] The types of binders and additives used in Example 6, the weight ratio of the molecular sieves, the types of organosilanes and the exchange multiples of organosilanes are shown in Table 1; the strength, water content, particle size, nitrogen-oxygen separation coefficient, nitrogen adsorption capacity, water drop contact angle and other parameters of the obtained molecular sieve product (having a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent) are shown in Table 2;
[0167] The hydrophobic lithium-type oxygen-generating molecular sieve adsorbent obtained by the above preparation method is used in the PSA / VPSA oxygen-generating process to adsorb a large amount of N2 in the nitrogen-oxygen separation to obtain high-purity O2. The oxygen concentration results after the PSA process on a 5L oxygen generator are shown in Tables 4 and 5.
[0168] Example 7
[0169] The present embodiment provides a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent and a preparation method thereof. The molecular sieve adsorbent is prepared from initial raw material components and initial auxiliary material components; the initial raw material composition is molecular sieve raw powder, adhesive and auxiliary agent; the mass content of the molecular sieve raw powder is 92%, the mass content of the adhesive is 7.5%, and the mass content of the auxiliary agent is 0.5%; the initial auxiliary material components are soluble lithium salt solution and organosilane-toluene solution; in the soluble lithium salt solution, the lithium ion concentration is 1.5 mol / L; the mass concentration of organosilane in the organosilane-toluene solution is 3%; the lithium ions in the molecular sieve raw powder occupy at least 98.29% of the exchangeable cation sites.
[0170] Particle size diameter of molecular sieve adsorbent Particle wear rate 0.22%, 1.0cm 3 The breakage rates of the adsorbent particle accumulation under pressures of 150N and 250N for 5s were 2.8% and 7.4% respectively; the nitrogen and oxygen separation coefficient was 6.45, and the N2 gas adsorption capacity was 23.51ml / g at 1atm; the water droplet contact angle was 111.05°, and the surface was hydrophobic.
[0171] The preparation method of the molecular sieve adsorbent is carried out according to the following steps:
[0172] 1) The molecular sieve raw powder is mixed with the binder and the additive in a mass ratio of 92:7.5:0.5 to obtain a mixed powder; then the mixed powder is placed in a rolling ball forming device, deionized water is added during rotation and the dry basis weight ratio of all materials is kept in the range of 70-80%, the ball diameter is controlled to be less than 1 mm, and the particle size is screened to be Agglomerates of small balls;
[0173] The molecular sieve raw powder is X zeolite, the silicon-aluminum ratio is 2.2 according to the molecular molar ratio, and the mass content of K2O is less than 0.5%;
[0174] The binder is bentonite;
[0175] The auxiliary agent is acrylic emulsion;
[0176] 2) drying the pellet aggregate for 12 hours, then drying at 80-120° C. to obtain a dry basis weight ratio of >80%, and then calcining at 500-550° C. to obtain a formed sodium sieve pellet adsorbent having a dry basis weight ratio of >98%;
[0177] 3) The sodium sieve ball adsorbent is saturated with water in the air to a moisture content of ≥20wt%, and then put into deionized water for wetting to prepare a wetted material; the wetted material is placed in an exchange tank for 4 hours. -1Inputting a soluble lithium salt solution at a space velocity to perform lithium ion exchange, controlling the lithium exchange degree to 98.29%, and obtaining a lithium exchange material; washing the lithium exchange material with a LiOH solution with a pH value of 8, and finally obtaining a washed material with a chloride ion concentration lower than 200 ppm;
[0178] In the soluble lithium salt solution, the lithium salt is lithium chloride, and the lithium ion concentration is 1.5 mol / L;
[0179] 4) dissolving the organosilane in toluene to prepare an organosilane-toluene solution; the mass concentration of the organosilane in the organosilane-toluene solution is 3%; -1 The surface of the surface-modified adsorbent is modified by introducing an organic silane-toluene solution at a space velocity, wherein the volume of the organic silane-toluene solution used is 14 times the volume of the washed material, and a surface-modified adsorbent is obtained; after the surface-modified adsorbent is discharged, it is first air-dried and then dried at 80-120° C., and the dry basis of the surface-modified adsorbent is controlled to be ≥85%, and a lithium adsorbent pellet is obtained;
[0180] In the organosilane-toluene solution, the organosilane is benzyldimethylchlorosilane;
[0181] 5) The lithium adsorbent beads are dehydrated and activated by controlling the temperature to rise to 100-550° C. under negative pressure (the temperature setting is similar to that in Example 1), and the water content of the lithium adsorbent beads is controlled to be ≤0.5wt%, and then the temperature is lowered to 80-120° C. in an isolated water vapor environment to obtain a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent.
[0182] The types of binders and additives used in Example 7, the weight ratio of the molecular sieves, the types of organosilanes and the exchange multiples of organosilanes are shown in Table 1; the strength, water content, particle size, nitrogen-oxygen separation coefficient, nitrogen adsorption capacity, water drop contact angle and other parameters of the obtained molecular sieve product (having a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent) are shown in Table 2;
[0183] The hydrophobic lithium-type oxygen-generating molecular sieve adsorbent obtained by the above preparation method is used in the PSA / VPSA oxygen-generating process to adsorb a large amount of N2 in the nitrogen-oxygen separation to obtain high-purity O2. The oxygen concentration results after the PSA process on a 5L oxygen generator are shown in Tables 4 and 5.
[0184] Example 8
[0185] The present embodiment provides a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent and a preparation method thereof. The molecular sieve adsorbent is prepared from initial raw material components and initial auxiliary material components; the initial raw material composition is molecular sieve raw powder, adhesive and auxiliary agent; the mass content of the molecular sieve raw powder is 82%, the mass content of the adhesive is 15%, and the mass content of the auxiliary agent is 3%; the initial auxiliary material components are soluble lithium salt solution and organosilane-toluene solution; in the soluble lithium salt solution, the lithium ion concentration is 2 mol / L; the mass concentration of organosilane in the organosilane-toluene solution is 4%; the lithium ions in the molecular sieve raw powder occupy at least 98.00% of the exchangeable cation sites.
[0186] Particle size diameter of molecular sieve adsorbent Particle wear rate 0.30%, 1.0cm 3 The breakage rates of the adsorbent particle accumulation under pressures of 150N and 250N for 5s were 2.3% and 7.8% respectively; the nitrogen and oxygen separation coefficient was 6.52, and the N2 gas adsorption capacity was 22.41ml / g at 1atm; the water droplet contact angle was 106.2°, and the surface was hydrophobic.
[0187] The preparation method of the molecular sieve adsorbent is carried out according to the following steps:
[0188] 1) Mix the molecular sieve powder, the binder and the additive in a mass ratio of 82:15:3 to obtain a mixed powder; then place the mixed powder in a rolling ball forming device, add deionized water during rotation and keep the dry basis of all materials in the range of 70-80%, control the ball diameter to <1mm, and sieve the particle size to Agglomerates of small balls;
[0189] The molecular sieve raw powder is X zeolite; the silicon-aluminum ratio is 2.1 according to the molecular molar ratio, wherein the mass content of K2O is less than 0.5%;
[0190] The binder is kaolin;
[0191] The auxiliary agent is anhydrous sodium pyrophosphate;
[0192] 2) drying the pellet aggregate for 10 hours, drying at 80-120°C to obtain a dry basis of >80%, and then calcining at 500-550°C to obtain a shaped sodium sieve pellet adsorbent with a dry basis of >98%;
[0193] 3) The sodium sieve ball adsorbent is saturated with water in the air to a moisture content of ≥ 20 wt%, and then put into deionized water for wetting to prepare a wetted material; the wetted material is placed in an exchange tank for 3 hours. -1Inputting a soluble lithium salt solution at a space velocity to perform lithium ion exchange, controlling the lithium exchange degree to 98.00%, and obtaining a lithium exchange material; washing the lithium exchange material with a LiOH solution having a pH value of 9, and finally obtaining a washed material with a sulfate ion concentration lower than 200 ppm;
[0194] In the soluble lithium salt solution, the lithium salt is lithium sulfate, and the lithium ion concentration is 2 mol / L;
[0195] 4) dissolving the organosilane in toluene to prepare an organosilane-toluene solution; the mass concentration of the organosilane in the organosilane-toluene solution is 4%; -1 The surface of the surface-modified adsorbent is modified by introducing an organic silane-toluene solution at an air velocity, wherein the volume of the organic silane-toluene solution used is 16 times the volume of the washed material, and a surface-modified adsorbent is obtained; after the surface-modified adsorbent is discharged, it is first air-dried and then dried at 80-120° C., and the dry basis of the surface-modified adsorbent is controlled to be ≥85%, and a lithium adsorbent pellet is obtained;
[0196] In the organosilane-toluene solution, the organosilane is 3-chloropropylmethyldimethoxysilane;
[0197] 5) The lithium adsorbent beads are dehydrated and activated by controlling the temperature to rise to 100-550° C. under negative pressure (the temperature setting is similar to that in Example 1), and the water content of the lithium adsorbent beads is controlled to be ≤0.5wt%, and then the temperature is lowered to 80-120° C. in an isolated water vapor environment to obtain a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent.
[0198] The types of binders and additives used in Example 8, the weight ratio of the molecular sieves, the types of organosilanes and the exchange multiples of organosilanes are shown in Table 1; the strength, water content, particle size, nitrogen-oxygen separation coefficient, nitrogen adsorption capacity, water drop contact angle and other parameters of the obtained molecular sieve product (having a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent) are shown in Table 2;
[0199] The hydrophobic lithium-type oxygen-generating molecular sieve adsorbent obtained by the above preparation method is used in the PSA / VPSA oxygen-generating process to adsorb a large amount of N2 in the nitrogen-oxygen separation to obtain high-purity O2. The oxygen concentration results after the PSA process on a 5L oxygen generator are shown in Tables 4 and 5.
[0200] Comparative Example 1
[0201] According to the patent "CN102500315A", LiX molecular sieve adsorbent is prepared:
[0202] 1) 2 kg of molecular sieve raw powder (Si / A1=1.1) was mixed with attapulgite and sesbania powder in a dry weight ratio of 1:0.15:0.05, and rolled into small balls with a diameter of 0.4-0.8 mm, and then dried at 250°C for 4 hours and calcined at 550°C for 2 hours to obtain calcined matrix small balls.
[0203] 2) 1 kg of the calcined matrix pellets were placed in 5 L of 1.0 mol / L NaOH solution, heated to 90°C for 3 hours, and then washed with 5 times of water to obtain alkali-treated matrix pellets. The alkali-treated matrix pellets were exchanged with 1.0 mol / L ammonium sulfate aqueous solution at 40°C for 4 times, each time with a liquid-to-solid ratio of 8:1, and then washed with 10 times of water, filtered and dried to obtain ammonium exchange pellets. The Na2O content was 2.3%wt, the water content was 8.3%wt, and the exchange degree was 97.5%.
[0204] 3) 500 g of ammonium exchange beads and 610 ml of 2.5 mol / L lithium chloride salt solution are saturatedly impregnated in an impregnation reactor, that is, 610 ml of lithium chloride solution is divided into 4 equal parts, one part is taken each time and fully mixed with the ammonium exchange beads for impregnation, and then dried at 200° C. for 4 hours, and the impregnation and drying steps are repeated until the lithium chloride solution is completely absorbed by the ammonium exchange beads to obtain impregnated matrix beads.
[0205] 4) The impregnated matrix beads were dried at 250° C. for 30 minutes, and then calcined and activated at 550° C. for 2 hours to obtain the LiX molecular sieve adsorbent VS-1.
[0206] Comparative Examples 2-9
[0207] The preparation methods are the same as those in Examples 1-8, except that: the step of dissolving the organosilane in toluene to prepare an organosilane-toluene solution and using the solution to modify the surface of the washing material in step 4) is cancelled, and the washing material is first air-dried and then dried to control the dry basis of the surface-modified adsorbent to be ≥85% to obtain lithium adsorbent beads; then the lithium adsorbent beads are dehydrated and activated by controlling the negative pressure program temperature rise of 100-550° C. (the temperature setting is similar to that in Example 1) to obtain a molecular sieve adsorbent;
[0208] The molecular sieve adsorbents of Comparative Examples 2-9 were tested in the same manner as in Examples 1-8 for their strength, water content, particle size, nitrogen-oxygen separation coefficient, nitrogen adsorption capacity, and water drop contact angle. The results are shown in Table 3.
[0209] Table 1
[0210]
[0211] Table 2
[0212]
[0213]
[0214] Table 3
[0215]
[0216] The results of Table 2 and Table 3 show that the molecular sieve adsorbents prepared in Examples 1-8 of the present invention have lower wear rate and 150N / 250N crushing rate than the adsorbents in Comparative Examples 1-9, the static adsorption of N2 reaches more than 20ml / g and the N2 / O2 separation coefficient is higher, and the water drop contact angle reaches more than 90°, indicating that the molecular sieve adsorbent of the present invention has good hydrophobicity. In addition, the molecular sieve adsorbent of the present invention has a high proportion of particles with a particle size in the range of 0.4-0.8mm, and other properties are balanced and stable, and the water content is moderate.
[0217] Application Cases
[0218] The hydrophobic lithium-type oxygen-generating molecular sieve adsorbent obtained in Example 1 was loaded into a 5L oxygen generator with double adsorption cylinders, with a loading amount of 1.1-1.4 kg, a bulk density of 0.64 g / ml, a test environment temperature of 25°C, and a relative humidity of 31%. The oxygen generator was continuously operated for 1440 min, during which the system adsorption pressure, desorption pressure, oxygen concentration, oxygen flow rate, and equilibrium pressure values at 0, 30, 150, 280, 400, 520, 670, 850, and 1440 min were measured, and the results are shown in Table 4.
[0219] Table 4
[0220]
[0221]
[0222] The adsorbent beads obtained in Examples 2 to 8 were further loaded into a 5L oxygen generator molecular sieve cartridge, and the oxygen output concentration was tested under the adsorption pressure, desorption pressure, equilibrium pressure and oxygen flow rate shown in Table 5. The test environment temperature was 20 to 30°C and the relative humidity was 25 to 40%. The results were obtained after continuous operation of the oxygen generator for 1440 min.
[0223] Table 5
[0224] Example Adsorption pressure(KPa) Desorption pressure(KPa) Oxygen concentration (%) Oxygen flow rate (L / min) Balance pressure(KPa) Example 1 30 -60 93.43 4.8~5.2 14-22 Example 2 25 -60 93.42 4.8~5.2 12~20 Example 3 30 -65 93.55 4.8~5.2 12~22 Example 4 25 -65 93.40 4.8~5.2 11~19 Example 5 40 -60 93.35 4.8~5.2 23-33 Example 6 45 -60 93.45 4.8~5.2 27-38 Example 7 35 -65 93.55 4.8~5.2 18-28 Example 8 40 -65 93.52 4.8~5.2 23-33 Comparative Example 1 30 -60 90.42 4.8~5.2 26-38 Comparative Example 2 30 -60 91.54 4.8~5.2 21-33 Comparative Example 3 30 -60 90.43 4.8~5.2 23-35
[0225] The results of Table 4 and Table 5 show that when the molecular sieve adsorbent of the present invention is used in the air separation process, high-purity oxygen can be obtained, and it has high stability and high separation performance, which can fully guarantee the production efficiency of the PSA air separation process.
[0226] The above-mentioned embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a hydrophobic lithium-type oxygen-generating molecular sieve adsorbent, Features: Follow these steps: (1) Mixing molecular sieve raw powder, binder and additive in a mass ratio of (82-92): (7.5-15): (0.15-3.0) to obtain a mixed powder; forming the mixed powder into a small ball agglomerate with a ball diameter of less than 1 mm, and then sieving the small ball agglomerate with a particle size of φ0.1-0.8 mm; (2) The 0.1-0.8 mm sphere aggregate is first dried at room temperature for a period of time, then heated and dried at 80-120°C to make the dry basis weight ratio greater than 80%, and then calcined at 100-550°C to obtain a formed sodium sieve sphere adsorbent with a dry basis weight ratio greater than 98%; (3) saturating the sodium sieve ball adsorbent with water in an environment at a temperature of 25-30° C. so that the water content in the adsorbent is ≥20wt%, and then wetting the adsorbent in deionized water to prepare a wetted material; exchanging lithium ions with a soluble lithium salt solution to control the lithium exchange degree to be greater than 97% to obtain a lithium exchange material; washing the lithium exchange material with a LiOH solution with a pH value of 8-10 to obtain a washed material; (4) dissolving a hydrophobic organosilane in toluene to prepare an organosilane-toluene solution; adding the washed material to the organosilane-toluene solution for surface modification to obtain a surface modified adsorbent; after unloading the surface modified adsorbent, first air-drying it at room temperature, and then heating and drying it at 80-120° C. to control the dry basis of the surface modified adsorbent to be ≥85%, thereby obtaining lithium adsorbent beads; (5) dehydrating and activating the lithium adsorbent beads by controlling the temperature to rise to 100-550°C under negative pressure, controlling the water content of the lithium adsorbent beads to be ≤0.5wt%, and then cooling the beads to 80-120°C in an isolated water vapor environment to obtain a hydrophobic lithium-type oxygen-generating molecular sieve adsorbent; In step (1), the molecular sieve raw powder is one or more of X zeolite, EMT zeolite, RHO molecular sieve, ZSM-3, ZSM-5, mordenite, and clinoptilolite; the adhesive is one or more of attapulgite, kaolin, chamomile, high clay, halloysite, talc, and bentonite; the auxiliary agent is one or more of bayberry gum, sesbania powder, SG plant gum, cellulose, sodium carboxymethyl cellulose, polyethylene glycol PEG, polyvinyl alcohol PVA, methyl cellulose and its derivatives, acrylic emulsion, anhydrous sodium pyrophosphate, and starch; In step (4), the organosilane in the organosilane-toluene solution comprises at least one of 3-chloropropyltrimethoxysilane, phenyltrimethoxysilane, methylphenyldimethoxysilane, chloromethyltrimethoxysilane, diphenyldimethoxysilane, diisobutyldimethoxysilane, 3-chloropropylmethyldimethoxysilane, isobutylisopropyldimethoxysilane, ethyltrimethoxysilane, styreneethyltrimethoxysilane, 4-chloromethylphenyltrimethoxysilane, chloromethyldimethoxysilane, methylphenyldichlorosilane, phenyldimethylchlorosilane, benzyldimethylchlorosilane, 3-chloropropyltrichlorosilane, 3-chloropropylmethyldichlorosilane, 2-phenylpropyltrichlorosilane, dimethyloctylchlorosilane, phenethyltrichlorosilane, benzyltrichlorosilane and dichlorophenyltrichlorosilane; and the mass concentration of the organosilane in the organosilane-toluene solution is 0.2-5%; In step (4), the washed material is heated for 0.5-5 hours. -1 Toluene solution is introduced at a high space velocity for surface modification, and the volume of the organosilane-toluene solution used is 5-20 times the volume of the material after washing.
2. A method for preparing a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent according to claim 1, Features: In step (2), the 0.1-0.8 mm sphere aggregate is first dried at room temperature for 4-24 hours.
3. A method for preparing a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent according to claim 1, Features: In step (3), the lithium salt in the soluble lithium salt solution includes any one of lithium chloride, lithium nitrate, lithium sulfate, and lithium hydroxide; and the lithium ion concentration in the soluble lithium salt solution is 0.3-3.0 mol / L.
4. A method for preparing a hydrophobic lithium-type oxygen-producing molecular sieve adsorbent according to claim 1, Features: In step (3), the wetted material is placed in an exchange tank and heated for 0.5-5 hours. -1 Soluble lithium salt solution is input at a high speed to exchange lithium ions with the wetted material; the exchange degree is controlled to be >98%.
5. A hydrophobic lithium-type oxygen-generating molecular sieve adsorbent, It is characterized in that The method is obtained by the preparation method according to any one of claims 1 to 4.
6. Use of the hydrophobic lithium-type oxygen-producing molecular sieve adsorbent obtained by the preparation method according to any one of claims 1 to 4 or the hydrophobic lithium-type oxygen-producing molecular sieve adsorbent according to claim 5, It is characterized in that Used in PSA / VPSA oxygen production process, the molecular sieve adsorbent is used to adsorb N in the nitrogen and oxygen separation process 2 , and then obtain high-purity O 2 .
Citation Information
Patent Citations
Ion exchange method for preparing lithium type low silicon aluminum X-shape zeolite molecular sieve
CN101125664A
Lithium-containing modified low silicon-aluminum X type molecular sieve adsorbent and preparation method thereof
CN101766987A
Method for preparing lithium oxygen generation adsorbent
CN102160990A
LiX molecular sieve adsorbent and preparation method thereof
CN102500315A
X-zeolite for lithium exchange, its preparation method and its application as nitrogen adsorber
CN1302687A
Cited By
Preparation method and application of X-type oxygen production molecular sieve
CN120553729B