A kind of transparent polyimide with high heat resistance and low expansion and preparation method thereof
By designing the molecular structure, introducing hydrogen bonds and crosslinking structures, the problem of high expansion properties of transparent polyimide materials is solved, and a transparent polyimide with high heat resistance and low expansion is prepared, achieving high glass transition temperature and excellent Optical and mechanical properties.
Patent Information
- Application Number
- CN202310455548.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-04-25
AI Technical Summary
Conventional transparent polyimide materials have low intermolecular forces, resulting in a high linear expansion coefficient, which is prone to peeling off from the matrix due to thermal expansion and contraction, and are not suitable for flexible packaging.
By designing the molecular structure, changing the linearity and rigidity of the molecular chain, introducing hydrogen bonds and crosslinking structures, a transparent polyimide material with high glass transition temperature is prepared to reduce the expansion coefficient.
A transparent polyimide material with high heat resistance and low expansion is achieved, maintaining excellent optical and mechanical properties.
Smart Images

Figure CN116478402B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of transparent polyimide materials, and more specifically to a transparent polyimide with high heat resistance and low expansion and a preparation method thereof. Background Art
[0002] Modern flexible packaging technology requires that the cover material has good optical properties (such as high transmittance, low yellowness index, low haze, etc.), high heat resistance (high glass transition temperature) and higher dimensional stability (low linear thermal expansion coefficient) while being flexible. Transparent polyimide (CPI) material has attracted much attention due to its good flexibility, good optical properties and good mechanical properties.
[0003] However, conventional transparent polyimide materials use large fluorine-containing groups, which leads to low intermolecular forces and high linear expansion coefficients. They are easily peeled off from the substrate due to thermal expansion and contraction during high and low temperature cyclic use, which is not conducive to flexible packaging. Summary of the invention
[0004] The purpose of the present invention is to provide a transparent polyimide with high heat resistance and low expansion. By designing the molecular structure, changing the linearity and rigidity of the molecular chain, and introducing hydrogen bonds and cross-linking structures, the material has a higher glass transition temperature and a lower expansion coefficient, so as to solve the technical problems existing in the above-mentioned background technology.
[0005] The technical solution of the present invention provides a transparent polyimide with high heat resistance and low expansion, comprising the following components by weight: 2.2417-4.6188g of dianhydride compound, 2.7357-3.2023g of diamine compound, 22-40g of N-methylpyrrolidone, 5.1g of acetic anhydride, and 2.6g of triethylamine;
[0006] The dianhydride compound includes one or more of flexible dianhydride, alicyclic dianhydride, rigid and amide-containing dianhydride; the diamine compound includes one or more of fluorine / carbonyl-containing diamine, amide or condensed ring structure-containing diamine, and cross-linking diamine.
[0007] In a preferred embodiment, the content of the flexible dianhydride is 20-80%, the content of the alicyclic dianhydride is 20-80%, the content of the rigid and amide-containing dianhydride is 5-30%; the content of the fluorine / carbonyl-containing diamine is 40-80%, the content of the amide or condensed ring structure diamine is 10-60%, and the content of the cross-linking diamine is 0-10%.
[0008] In a preferred embodiment, the flexible dianhydride includes 4,4'-(hexafluoroisopropylene) diphthalic anhydride (6FDA), the alicyclic dianhydride includes 1,2,3,4-cyclobutanetetracarboxylic dianhydride (CBDA), 1,2,4,5-cyclohexanetetracarboxylic dianhydride (HPMDA), and the rigid and amide-containing dianhydride N,N'-(2,2-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(1,3-dihydroxy-1,3-dihydroisobenzofuran-5-carboxyamide) (TA-TFMB).
[0009] In a preferred embodiment, the fluorine / carbonyl-containing diamine includes 2,2'-bis(trifluoromethyl)diaminobiphenyl (TFMB), 9,9-bis(4-amino-3-fluorophenyl)fluorene (BAFL), the diamine containing amide or condensed ring structure includes 3',4-diaminobenzanilide (DABA), and the cross-linking diamine includes 1,3,5-tri(4-aminophenyl)benzene.
[0010] A method for preparing a transparent polyimide with high heat resistance and low expansion, comprising the following preparation steps:
[0011] S1: Add 2.7357-3.2023 g of a diamine compound and 22-40 g of N-methylpyrrolidone into a reaction container filled with nitrogen, and stir to dissolve;
[0012] S2: Then, 2.2417-4.6188 g of dianhydride compound was added to the solution obtained in S1, and the polymerization reaction was carried out at 0°C for 24 hours to form a transparent polyamic acid precursor solution;
[0013] S3: Add 5.10 g of acetic anhydride and 2.60 g of triethylamine to the body solution, continue stirring for 12 h to perform chemical imidization, and obtain a polyimide solution;
[0014] S4: pouring the polyimide solution into methanol to precipitate a white filamentous precipitate, filtering out the filamentous precipitate and washing it twice with methanol, and drying it to obtain a polyimide powder;
[0015] S5: Dissolve the polyimide powder in N,N-dimethylformamide to form a solution with a mass fraction of 18%, apply it on the inside and outside of a clean glass plate, place it in an oven at 80°C for 12 hours to evaporate the solvent, keep it at 200°C for 1 hour, then raise the temperature to 300°C and continue to keep it at this temperature for 1 hour to obtain a transparent polyimide film.
[0016] The beneficial effects of the technical solution of the present invention are:
[0017] By designing the molecular structure, changing the linearity and rigidity of the molecular chain, and introducing hydrogen bonds and cross-linking structures, the material has a higher glass transition temperature and a lower expansion coefficient, and has excellent optical and mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a graph showing the test results of Examples 2, 4, and 5 of the present invention.
[0019] Figure 2 These are the test result diagrams of Examples 1, 3, 6 and 7 of the present invention. DETAILED DESCRIPTION
[0020] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. The embodiments of the present invention are provided for the sake of illustration and convenience of description, and are not intended to be exhaustive or to limit the present invention to the disclosed forms. Many modifications and variations will be apparent to those of ordinary skill in the art. The embodiments are selected and described in order to better illustrate the principles and practical applications of the present invention, and to enable those of ordinary skill in the art to understand the present invention and thereby design various embodiments with various modifications suitable for specific uses.
[0021] Example 1
[0022] 3.2023 g of diamine compound TFMB and 30 g of N-methylpyrrolidone were added to a reaction vessel filled with nitrogen and stirred to dissolve. 4.4424 g of dianhydride compound 6FDA were added in sequence and polymerized at 0°C for 24 hours to form a transparent polyamic acid (PAA) solution, and its intrinsic viscosity was tested to be 0.95 dL / g.
[0023] Add 5.10 g of acetic anhydride and 2.60 g of triethylamine to the precursor solution, continue stirring for 12 h for chemical imidization, and obtain a polyimide solution. Pour the solution into methanol to precipitate a white filamentous precipitate. Filter out the filamentous precipitate and rinse it twice with methanol, and dry it to obtain a polyimide powder.
[0024] The polyimide powder was dissolved in N,N-dimethylformamide to form a solution with a mass fraction of 18%, coated on the inside and outside of a clean glass plate, placed in an oven at 80°C for 12 hours to evaporate the solvent, kept at 200°C for 1 hour, then raised to 300°C and kept for another hour to obtain a transparent polyimide film.
[0025] Example 2
[0026] 3.2023 g of diamine compound TFMB and 22 g of N-methylpyrrolidone were added to a reaction vessel filled with nitrogen and stirred to dissolve. 2.2417 g of dianhydride compound HPMDA was added in sequence and polymerized at 0°C for 24 hours to form a transparent polyamic acid (PAA) solution, and its intrinsic viscosity was tested to be 0.86 dL / g.
[0027] Add 5.10 g of acetic anhydride and 2.60 g of triethylamine to the precursor solution, continue stirring for 12 h for chemical imidization, and obtain a polyimide solution. Pour the solution into methanol to precipitate a white filamentous precipitate. Filter out the filamentous precipitate, rinse it twice with methanol, and dry it. Obtain a polyimide powder.
[0028] The polyimide powder was dissolved in N,N-dimethylformamide to form a solution with a mass fraction of 18%, coated on the inside and outside of a clean glass plate, placed in an oven at 80°C for 12 hours to evaporate the solvent, kept at 200°C for 1 hour, then raised to 300°C and kept for another hour to obtain a transparent polyimide film.
[0029] Example 3
[0030] 1.6012g of diamine compound TFMB and 1.1363g of diamine compound DABA (total 2.7357) and 40g of N-methylpyrrolidone were added to a reaction vessel filled with nitrogen and stirred to dissolve. 2.2212g of dianhydride compound 6FDA and 0.9806g of dianhydride compound CBDA (3.2018) were added in sequence, and the polymerization reaction was carried out at 0°C for 24 hours to form a transparent polyamic acid (PAA) solution, and its intrinsic viscosity was tested to be 1.10dL / g.
[0031] Add 5.10 g of acetic anhydride and 2.60 g of triethylamine to the precursor solution, continue stirring for 12 h for chemical imidization, and obtain a polyimide solution. Pour the solution into methanol to precipitate a white filamentous precipitate. Filter out the filamentous precipitate, rinse it twice with methanol, and dry it. Obtain a polyimide powder.
[0032] The polyimide powder was dissolved in N,N-dimethylformamide to form a solution with a mass fraction of 18%, coated on the inside and outside of a clean glass plate, placed in an oven at 80°C for 12 hours to evaporate the solvent, kept at 200°C for 1 hour, then raised to 300°C and kept for another hour to obtain a transparent polyimide film.
[0033] Example 4
[0034] 3.2023g of diamine compound TFMB and 30g of N-methylpyrrolidone were added to a reaction vessel filled with nitrogen and stirred to dissolve. 1.1209g of dianhydride compound HPMDA and 3.3423g of dianhydride compound TA-TFMB (4.4637) were added in sequence and polymerized at 0°C for 24h to form a transparent polyamic acid (PAA) solution, and its intrinsic viscosity was tested to be 0.98dL / g.
[0035] Add 5.10 g of acetic anhydride and 2.60 g of triethylamine to the precursor solution, continue stirring for 12 h for chemical imidization, and obtain a polyimide solution. Pour the solution into methanol to precipitate a white filamentous precipitate. Filter out the filamentous precipitate, rinse it twice with methanol, and dry it. Obtain a polyimide powder.
[0036] The polyimide powder was dissolved in N,N-dimethylformamide to form a solution with a mass fraction of 18%, coated on the inside and outside of a clean glass plate, placed in an oven at 80°C for 12 hours to evaporate the solvent, kept at 200°C for 1 hour, then raised to 300°C and kept for another hour to obtain a transparent polyimide film.
[0037] Example 5
[0038] 1.6012g of diamine compound TFMB and 1.7422g of diamine compound BAFL (2.8034) and 22g of N-methylpyrrolidone were added to a reaction vessel filled with nitrogen and stirred to dissolve. 1.1209g of dianhydride compound HPMDA and 3.3423g of dianhydride compound TA-TFMB (4.4637) were added in sequence and polymerized at 0°C for 24h to form a transparent polyamic acid (PAA) solution, and its intrinsic viscosity was tested to be 0.88dL / g.
[0039] Add 5.10 g of acetic anhydride and 2.60 g of triethylamine to the precursor solution, continue stirring for 12 h for chemical imidization, and obtain a polyimide solution. Pour the solution into methanol to precipitate a white filamentous precipitate. Filter out the filamentous precipitate, rinse it twice with methanol, and dry it. Obtain a polyimide powder.
[0040] The polyimide powder was dissolved in N,N-dimethylformamide to form a solution with a mass fraction of 18%, coated on the inside and outside of a clean glass plate, placed in an oven at 80°C for 12 hours to evaporate the solvent, kept at 200°C for 1 hour, then raised to 300°C and kept for another hour to obtain a transparent polyimide film.
[0041] Example 6
[0042] 1.6012g of diamine compound TFMB and 1.7422g of diamine compound BAFL ((2.8034)) and 26g of N-methylpyrrolidone were added to a reaction vessel filled with nitrogen and stirred to dissolve. 2.2212g of dianhydride compound 6FDA and 0.9806g of dianhydride compound CBDA (3.2018) were added in sequence and polymerized at 0°C for 24h to form a transparent polyamic acid (PAA) solution, and its intrinsic viscosity was tested to be 1.09dL / g.
[0043] Add 5.10 g of acetic anhydride and 2.60 g of triethylamine to the precursor solution, continue stirring for 12 h for chemical imidization, and obtain a polyimide solution. Pour the solution into methanol to precipitate a white filamentous precipitate. Filter out the filamentous precipitate, rinse it twice with methanol, and dry it. Obtain a polyimide powder.
[0044] The polyimide powder was dissolved in N,N-dimethylformamide to form a solution with a mass fraction of 18%, coated on the inside and outside of a clean glass plate, placed in an oven at 80°C for 12 hours to evaporate the solvent, kept at 200°C for 1 hour, then raised to 300°C and kept for another hour to obtain a transparent polyimide film.
[0045] Example 7
[0046] 1.6012g of diamine compound TFMB, 1.3938g of diamine compound BAFL, 0.7029g of diamine compound 1,3,5-tris(4-aminophenyl)benzene (2.995), and 26g of N-methylpyrrolidone were added to a reaction vessel filled with nitrogen and stirred to dissolve. 2.2212g of dianhydride compound 6FDA, 2.0054g of dianhydride compound TA-TFMB, and 0.3922g of dianhydride compound CBDA (4.6188) were added in sequence, and the polymerization reaction was carried out at 0°C for 24h to form a transparent polyamic acid (PAA) solution, and its intrinsic viscosity was tested to be 1.03dL / g.
[0047] Add 5.10 g of acetic anhydride and 2.60 g of triethylamine to the precursor solution, continue stirring for 12 h for chemical imidization, and obtain a polyimide solution. Pour the solution into methanol to precipitate a white filamentous precipitate. Filter out the filamentous precipitate, rinse it twice with methanol, and dry it. Obtain a polyimide powder.
[0048] The polyimide powder was dissolved in N,N-dimethylformamide to form a solution with a mass fraction of 18%, coated on the inside and outside of a clean glass plate, placed in an oven at 80°C for 12 hours to evaporate the solvent, kept at 200°C for 1 hour, then raised to 300°C and kept for another hour to obtain a transparent polyimide film.
[0049] The transparent polyimide films prepared in Examples 1-7 were tested for performance, and the results are shown in Table 1 below:
[0050]
[0051] Table 1
[0052] In the table: BAFL50 means that the molar ratio of substance BAFL is 50, and the rest is the same as above.
[0053] And draw the above results into a column to get a comparison Figure 1 and contrast Figure 2, and the above results are analyzed and the results are as follows:
[0054] (1) Through analysis and comparison Figure 1 Compared with Example 2, Example 4 has a significant improvement in Tg and CTE. This is because the TA-TFMB group introduced in Example 4 contains an amide bond and a rigid structure, which increases the interaction between molecular chains and affects the Tg and CTE performance of the product. Compared with Example 4, Example 5 has a significant improvement in Tg due to the introduction of BAFL with a large side group, but due to the introduction of a large side group, CTE also increases.
[0055] (2) Through analysis and comparison Figure 2 Compared with Example 1, Example 6 and Example 3 have significant improvements in Tg and CTE, which is due to the introduction of CBDA and DABA monomers. The introduction of CBDA and DABA increases the linear rigidity of the molecular chain, increases the content of amide bonds in the molecular chain, increases the content of hydrogen bonds in the molecular chain, reduces CTE, and increases Tg. The increase in CTE in Example 6 compared with Example 3 is due to the introduction of the large-volume side group of BAFL, which increases the distance between molecular chains and increases CTE. Compared with Example 6 and Example 3, Example 7 has better performance than Example 6 and Example 3 because it introduces a cross-linking structure in the molecular chain, so that cross-linking can be formed between molecular chains, and the mutual influence between chains is increased.
[0056] Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field and related fields without creative work should fall within the scope of protection of the present invention. The structures, devices and operating methods not specifically described and explained in the present invention are implemented according to the conventional means in the field unless otherwise specified and limited.
Claims
1. A transparent polyimide with high heat resistance and low expansion, characterized in that: The raw materials include the following components by weight: 26 g N-methylpyrrolidone, 5.1 g acetic anhydride, 2.6 g triethylamine, 2.2212 g 4,4'-(hexafluoroisopropylene) diphthalic anhydride (6FDA), 0.3922 g 1,2,3,4-cyclobutanetetracarboxylic dianhydride (CBDA), 2.0054 g N,N'-(2,2-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(1,3-dioxy-1,3-dihydroisobenzofuran-5-carboxamide) (TA-TFMB), 1.6012 g 2,2'-bis(trifluoromethyl)diaminobiphenyl (TFMB), 1.3938 g 9,9-bis(4-amino-3-fluorophenyl)fluorene (BAFL), and 0.7029 g 1,3,5-tris(4-aminophenyl)benzene.
2. The method for preparing a transparent polyimide with high heat resistance and low expansion according to claim 1, characterized in that: The method comprises the following preparation steps: S1: Add 1.6012 g of 2,2'-bis(trifluoromethyl)diaminobiphenyl (TFMB), 1.3938 g of 9,9-bis(4-amino-3-fluorophenyl)fluorene (BAFL), 0.7029 g of 1,3,5-tri(4-aminophenyl)benzene, and 26 g of N-methylpyrrolidone into a reaction container filled with nitrogen, and stir to dissolve; S2: Then, 2.2212 g of 4,4'-(hexafluoroisopropylene) diphthalic anhydride (6FDA), 0.3922 g of 1,2,3,4-cyclobutanetetracarboxylic dianhydride (CBDA), and 2.0054 g of N,N'-(2,2-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(1,3-dihydroxy-1,3-dihydroisobenzofuran-5-carboxyamide) (TA-TFMB) were added to the solution obtained in S1, and the polymerization reaction was carried out at 0°C for 24 hours to form a transparent polyamic acid precursor solution; S3: Add 5.10 g of acetic anhydride and 2.60 g of triethylamine to the precursor solution, and continue stirring for 12 h to perform chemical imidization to obtain a polyimide solution; S4: pouring the polyimide solution into methanol to precipitate a white filamentous precipitate, filtering out the filamentous precipitate and washing it twice with methanol, and drying it to obtain a polyimide powder; S5: Dissolve the polyimide powder in N,N-dimethylformamide to form a solution with a mass fraction of 18%, apply it on the surface and inside of a clean glass plate, place it in an oven at 80°C for 12 hours to evaporate the solvent, keep it at 200°C for 1 hour, then raise the temperature to 300°C and continue to keep it at this temperature for 1 hour to obtain a transparent polyimide film.
Citation Information
Patent Citations
Flexible transparent polyimide thin film and preparation method thereof
CN103044916A
Thermally stable, flexible substrates for electronic devices
CN104379635A
Polyimide resin, transparent polyimide film and preparation method of transparent polyimide film
CN107501551A
Cross-linked polyimide film, preparation method and applications thereof
CN110734559A
Transparent polyimide film with high heat resistance and low thermal expansion coefficient and preparation method
CN111675902A