A gear bar steel advantageous for speed change and lightweight and a manufacturing method thereof

By optimizing the alloy element ratio and efficient continuous casting production process, the existing gear steels are solved, and the efficient lightweighting and production efficiency of transmission gears are achieved.

CN116479327BActive Publication Date: 2024-12-03JIANGYIN XINGCHENG SPECIAL STEEL WORKS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310328782.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-12-03
Estimated Expiration
2043-03-30

AI Technical Summary

Technical Problem

Existing gear steels often rely on precious alloy elements when increasing strength, resulting in increased resource consumption and production costs, and low production efficiency, making it difficult to achieve lightweight transmissions.

Method used

By optimizing the alloy element ratio, especially using C, Si, Mn, Cr, Al and other elements, reducing or not using precious alloy elements such as Ni, Mo, and Cu, using efficient continuous casting production process and quenching + low-temperature tempering treatment , improve the tensile strength and lightweight properties of steel.

Benefits of technology

The high strength and lightweight steel are achieved, production costs and resource consumption are reduced, and the lightweight effect of transmission gears is improved. The weight of parts can be reduced by 15 to 30%, which significantly improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116479327B_ABST
    Figure CN116479327B_ABST
Patent Text Reader

Abstract

The present invention relates to a bar steel for gears which is beneficial to the lightweight of a gearbox and a manufacturing method thereof, and belongs to the field of metal materials. The chemical composition of the steel is C: 0.20-0.30%, Si: 0.15-0.35%, Mn: 1.10-1.30%, Cr: 0.90-1.20%, Al: 6.00-9.00% by mass percentage, and the remainder is Fe and inevitable impurity elements. Elements such as Ni, Mo, Cu, and B are not deliberately added. The steel solves the technical problem of nozzle nodules and interruption of production during continuous casting of this series of steels by controlling Al2O3 during steelmaking and continuous casting, and by specially designing the protective slag and the nozzle shape, so that this type of steel can be continuously cast, thereby ensuring production efficiency and reducing production costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of gear steel, and in particular relates to a lightweight gear steel bar and a manufacturing method thereof. Background Art

[0002] The pressure of resources, energy and environment requires the modern manufacturing industry to continuously improve in order to save resources, energy and reduce emissions. Taking the automobile industry as an example, lightweighting is an important measure to reduce costs and energy. For every 10% weight reduction of the car, fuel consumption can be reduced by about 8%. Gearboxes are widely used in the machinery industry, such as the automobile industry. Various gears are the core parts of gearboxes. If the gearbox is to be lightweight, the design of the steel used for the gears is particularly critical. First, the material strength is improved. Under the same load, the size of the parts can be reduced to achieve weight reduction; on the other hand, if lightweight steel is used, the weight of the parts can be reduced under the same size.

[0003] The patent contribution of patent application number 20190622620.1 discloses a new high-strength gear steel forging method, in which 15Cr14Co12Mo5Ni2WA steel is heated and forged, with a forging deformation of >40% and a final forging temperature of 800-810°C to obtain high-strength gear steel forgings. The steel has a high content of precious alloy elements such as Co, Mo, and Ni, which is not conducive to resource conservation, and the production cost will also increase significantly. The patent document of patent application number 202110039572.0 discloses a high-strength gear steel 23CrMnMoS and a manufacturing method thereof. The steel is mainly improved by adding Mo elements to improve the strength of the steel, with a yield strength of ≥980Mpa and a tensile strength of ≥1280MPa. The main idea of ​​the above-mentioned technologies is to increase the strength of steel by adding higher alloying elements. Patent Publication No. CN108396244A discloses a cold-rolled medium manganese high aluminum low density steel and a preparation method thereof, which also adopts the addition of a relatively high Al to reduce the density of the steel. However, the steel of the invention has a high alloy content and is produced by die casting, with low production efficiency and low billet yield. The Al content is as high as 9.5-10.0%, and the manganese content is as high as 10.7-11.3%. The tensile strength is 1280-1320 MPa, which is equivalent to the steel of the present invention. The steel of the present invention (Mn+Cr) is about 2.2%, which greatly reduces the amount of alloy used, is conducive to reducing costs and saving resources, and the steel of the present invention is produced by high-efficiency continuous casting, which overcomes the technical difficulties of high Al steel being prone to nodules and protective slag being easy to change, improves the yield rate, and greatly improves production efficiency.

[0004] To sum up, the invention optimizes alloy elements, especially improves the strength of steel without adding precious alloy elements, can make steel lighter, and can help make gear steel lighter in gearboxes. The steel of the invention adopts high-efficiency continuous casting during casting, which saves costs and resources and has very significant economic and social value. Summary of the invention

[0005] The purpose of the present invention is to provide a gear steel and a manufacturing method thereof that is beneficial to the lightweighting of a gearbox. The gear steel bar manufactured by the method has the remarkable characteristics of high strength and light weight, which is very beneficial to the lightweighting of gearboxes, thereby achieving lightweighting of automobiles, etc., saving resources and reducing emissions. In addition, the steel of the present application adopts more efficient continuous casting production during casting, which greatly improves production efficiency and significantly reduces manufacturing costs.

[0006] The gear bar steel developed by the present application is a round steel bar, which is beneficial to the lightweight gearbox. The series of steels use Fe as the matrix element, and add C, Si, Mn, Cr, Al and other main alloy elements. Depending on the situation, Ni, Mo, Cu and other alloy elements can also be added for metallographic strengthening. Since Ni, Mo, Cu and the like are precious alloys, which will cause the production cost to rise, it depends on the situation whether to add and the amount of addition. The chemical composition of the steel of the present invention is C: 0.20-0.30%, Si: 0.15-0.35%, Mn: 1.10-1.30%, Cr: 0.90-1.20%, Al: 6.00-9.00%, and the rest is Fe and unavoidable impurity elements.

[0007] In order to control production costs, the material designed by the present invention does not intentionally add alloy elements such as Ni, Mo, Cu, Ti, and B, and their content is usually ≤0.25%; however, in order to adjust the performance, one or more of the aforementioned elements may be appropriately added.

[0008] The steel performance of the present invention meets the following requirements: In order to achieve lightweight gearbox, through the above composition optimization design, the steel has a tensile strength of ≥1300MPa under the conditions of quenching + low temperature tempering (tempering temperature: 150-200°C). Due to the increased strength, the size of the gear produced by the higher strength material under the same load conditions can be reduced. This composition design makes the steel lighter, with an Al content of 6.00-9.00%, and a corresponding steel density of about 6.80-6.28g / cm 3 Compared with the steel without Al addition, its density is reduced by 13.4-20.0%, that is, the weight of the gear of the same size will be reduced by 13.4-20.0%. The combined strength improvement and density reduction will reduce the weight of the gear made of steel by 15-30%.

[0009] The gear steel of the present invention improves the strength of the steel and makes the steel lighter by optimizing the alloy element ratio without adding precious alloy elements.

[0010] The design principles of the main elements of the steel of the present invention are as follows:

[0011] C: 0.20-0.30%. The steel of the present invention is essentially a medium-low carbon alloy gear steel. The C content mainly determines the proportion of cementite phase in the material and affects the strength of the material. If the proportion of cementite phase is too low, the strength of the material cannot be guaranteed. The higher the C content, the higher the proportion of cementite phase, which will reduce the toughness of the steel. The gear is under alternating load for a long time. In order to ensure the toughness of the core, the C content should not be too high. The C content range of the steel of the present invention is set to 0.20-0.30%.

[0012] Si: 0.15-0.35%. It is used as a deoxidizing element during steelmaking. At the same time, Si has a strong solid solution strengthening effect in steel, which can significantly improve the strength of ferrite. It needs to be controlled within a reasonable range. The Si content is set in the range of 0.15-0.35%.

[0013] Mn: 1.10-1.30%. Mn is an element that acts as a deoxidizer. It improves the strength of steel through solid solution strengthening. Adding a certain amount of Mn is very important to ensure the mechanical properties of the material. In addition, Mn combines S and other substances in the steel to form sulfide inclusions, which improves the cutting performance. On the other hand, Mn is easy to segregate and is sensitive to overheating of steel. If the Mn content is too high, bainite structure is easily generated, which affects the processing performance. The Mn content range of the steel in the present invention is set to 1.10-1.30%.

[0014] Cr: 0.90-1.20%. Cr is also one of the effective and economical elements for coordinating the strength of steel. It is an element that promotes the stability of carbides, can reduce or prevent the appearance of graphite phase after carburization on the gear surface, and has a certain ability to improve the steel's resistance to high-temperature oxidation. The Cr content range of the steel of the present invention is set to 0.90-1.20%.

[0015] Al: 6.00~9.00%. Al is the most critical element of the present invention. Al is a light metal. In the present invention, the addition of Al can make the steel lighter and adjust the hardness and strength of the steel; at the same time, Al can also play a role in resisting surface oxidation and improve the surface quality of the steel. In addition, the addition of Al can improve the corrosion resistance of the steel. Too high Al will also cause adverse effects such as large-particle carbides in the steel. The Al content range of the steel of the present invention is set to 6.00~9.00%.

[0016] The residual elements P and S of the material designed by the present invention are usually ≤0.030%; in order to control production costs, the material designed by the present invention does not deliberately add alloy elements such as Ni, Mo, Cu, Ti, B, and their content is usually ≤0.25%; but in order to adjust the performance, one or more elements can be appropriately added.

[0017] This application belongs to low-density steel containing aluminum. As aluminum is a strong deoxidizing element, a high content of aluminum is easily oxidized to aluminum oxide and lost in molten steel. Therefore, it is necessary to improve the smelting of molten steel to match the element composition design requirements of this application. The specific production process of gear bar steel for this application is as follows:

[0018] Smelting and casting, hot rolling and annealing

[0019] Smelting and casting: This process is the key core process of the steel production of the present invention. On the one hand, due to the high Al content, Al2O3 produced during smelting can easily lead to nozzle nodules and protective slag modification during continuous casting. In view of the above technical difficulties, electric furnace or converter smelting plus traditional refining outside the furnace are adopted. Strict non-oxidation protection casting must be adopted during casting. The Al content of the invented steel is high, and Al is easily oxidized to generate Al2O3 when it encounters oxygen, which leads to nozzle nodules and affects casting. It also avoids the secondary oxidation of molten steel to produce non-metallic inclusions that are harmful to use, and ensures the stability of the chemical composition of molten steel. In order to improve the yield of Al and minimize the generation of Al2O3, a large amount of silicon carbide is added for deoxidation after the refining begins, and the oxygen content in the steel is rapidly reduced in the early stage. After the deoxidation is basically completed, the O content in the molten steel is ≤30ppm. Then continue to send electricity for smelting, and add aluminum particles before the end of smelting. The particle size of aluminum particles should not be greater than φ30mm×50mm to ensure that the aluminum particles melt quickly. After the aluminum content reaches the set range, the flow rate of argon stirring gas at the bottom of the ladle needs to be moderate. If the flow rate is too small, the components cannot be quickly homogenized. If the flow rate is too large, the molten steel is prone to churning and the molten steel is exposed to the atmosphere, causing the aluminum in the molten steel to be oxidized.

[0020] After refining, continuous casting is carried out. During continuous casting, mold protection slag is the key auxiliary material to ensure that continuous casting is carried out continuously and stably. Due to the high Al content in the invented steel, a certain amount of Al2O3 is inevitably produced during the continuous casting process. Most of it is captured by the protection slag after floating up, thereby changing the performance of the protection slag. In order to prevent the protection slag from degenerating due to the continuous accumulation of Al2O3 during the casting process, the protection slag needs to be specially designed. The invented steel adopts a special high-CaO protection slag with a CaO content of 35-40% to ensure that the Al2O3 captured by the protection slag combines with CaO to form low-melting-point calcium aluminum oxide, so that the slag surface remains continuously stable.

[0021] In order to prevent nodules from forming in the nozzle during continuous casting, the design of the nozzle is also very critical. If the nozzle size is too large, the molten steel flow rate will be too slow, and the molten steel will not be enough to wash away the nodule products adsorbed on the nozzle; if the nozzle size is too small, even if the nodule products are partially washed away, the remaining nodules on the inner wall of the nozzle will seriously affect the internal size of the nozzle, and even block the nozzle, stopping casting. When designing the internal shape of the nozzle, a gourd-shaped design is adopted to better solve the technical problem of nozzle nodule formation. The control of Al2O3 during steelmaking and continuous casting, the special design of protective slag and the special design of the nozzle are the key, which enables this type of steel to achieve continuous casting, improve production efficiency and reduce production costs.

[0022] Heating and rolling: The ingot is heated until the structure is completely austenitized, the elements are fully melted, and the structure is homogenized. Then, it is immediately taken out of the furnace for forging and forging into small square billets. The small square billets are put back into the furnace for equalization. The structure is completely austenitized, and hot-rolled bars are obtained after rough rolling, finish rolling, and final rolling.

[0023] Preferably, the ingot is heated in a walking beam heating furnace at 1120-1200°C for 4-6 hours, and then immediately taken out of the furnace for forging and opening into a 200*200mm 2 The billet is then heated and rolled in a walking beam heating furnace, and then passes through the preheating section, the heating section and the soaking section, where the temperature is kept at 1120-1200°C, and then rough rolling, finish rolling and final rolling to obtain of hot rolled bars.

[0024] Annealing: Since the Al content of the steel of the present invention is relatively high, reaching 6.00-9.00%, the rolled bars need to be annealed in time to control the structure (ferrite pearlite) and hardness (170-210 HBW) of the final rolled material, and to ensure that the steel is not cracked and scrapped. During annealing, the steel is kept at 800-900°C, and the holding time depends on the specifications of the rolled material. In order to ensure the heating effect, the holding time is usually not less than 1.2min / mm*D (D is the diameter of the steel, mm), and then cooled to 600-750°C for isothermal transformation, and the isothermal time is 1.8min / mm*D (D is the diameter of the steel, mm), followed by natural cooling with the furnace.

[0025] The advantages of the present invention are that the steel has a low content of precious alloy elements and high strength. Under the conditions of quenching + low temperature (150-200°C) tempering, the tensile strength of the steel is ≥1300MPa. The steel is lightweight, and the density is 80-86.6% of traditional steel. Gear parts made of this material can reduce the size of parts due to the increased strength, and the weight of parts is lower at the same size. Under the same load conditions, the overall weight can be reduced by 15-30%. On the other hand, under the premise of solving the technical difficulties of high Al steel continuous casting, the steel of this invention adopts more efficient continuous casting production, which improves production efficiency and reduces production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is the metallographic structure diagram of the rod material in Example 1 of the present invention;

[0027] Figure 2 This is the metallographic structure diagram of the rod material in Example 2 of the present invention;

[0028] Figure 3 This is the metallographic structure diagram of the rod according to Example 3 of the present invention. DETAILED DESCRIPTION

[0029] The present invention is further described in detail below in conjunction with examples. The examples are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0030] Examples 1 to 3

[0031] The gear steels for lightening the gearbox according to embodiments 1 to 3 of the present invention are manufactured according to the following process:

[0032] 1) Smelting: After smelting in a 100-ton steelmaking furnace (converter or electric furnace), refining is carried out outside the furnace, and the molten steel is then vacuum degassed, and the mass percentage of each chemical element is strictly controlled as required. When the LF refining is reached, the power is supplied for 5 minutes, and the Si70 deoxidizer is added. The O content in the molten steel is deoxidized to ≤30ppm in the early stage, so that the slag turns white as soon as possible. Then appropriately reduce the argon blowing flow rate at the bottom of the ladle and the arc power, and quickly add aluminum particles with a particle size not exceeding φ30mm*50mm to increase the Al recovery rate. After the aluminum content reaches the set range, argon is blown at the bottom of the ladle to stir the molten steel. After the LF refining is completed, it is vacuum degassed again, and the mass percentage of each chemical element is strictly controlled as required.

[0033] 2) Continuous casting: Continuous casting is adopted, and protective casting is adopted during casting to prevent secondary oxidation of molten steel. Special protective slag is used, and the CaO content of the protective slag is 35-40wt%. A special nozzle design is adopted, and the internal structure of the nozzle is gourd-shaped. The casting speed is 0.6-0.8m / min to ensure a reasonable molten steel flow rate. The chemical composition of the ingot is shown in Table 1 below.

[0034] Table 1. (wt%, the balance is Fe and other inevitable impurity elements)

[0035] Serial number C Si Mn P S Cr Al N 1 0.26 0.25 1.26 0.018 0.021 1.18 7.76 0.0135 2 0.24 0.24 1.20 0.015 0.022 1.20 6.39 0.0118 3 0.29 0.24 1.15 0.021 0.008 1.11 8.12 0.0122

[0036] 3) Heating and rolling: The billet is heated in a heating furnace at 1120-1200℃ for 4-6 hours, and then immediately taken out of the furnace for forging and forging into 200*200mm 2 The billet is then heated in a walking beam furnace and subjected to rough rolling, finish rolling and final rolling to obtain of hot rolled bars.

[0037] 4) Annealing: During annealing, the steel is kept at 870°C for 60 minutes, cooled to 670°C at a faster rate for isothermal transformation, kept for 90 minutes, and then cooled naturally to obtain the finished steel.

[0038] The gear steels of Examples 1 to 3 were subjected to relevant tests, and the measured mechanical properties are shown in Table 2 below:

[0039] Table 2. Mechanical and physical properties of the invented steel

[0040]

[0041] As can be seen from Table 2, the tensile strength of the steel in the embodiment is 1327-1389 MPa, meeting the target requirement of ≥13000 MPa; the annealing hardness of the steel is between 173 and 184 HW, and the structure is ferrite + pearlite; the density of the steel is 6.37-6.82 g / cm 3 .

[0042] It should be noted that the above examples are only specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, but there are many similar variations as needed. If a person skilled in the art directly derives or associates all variations from the contents disclosed in the present invention, they should all fall within the protection scope of the present invention.

Claims

1. A method for manufacturing a gear bar steel that is beneficial to the lightweighting of a gearbox, characterized in that: include Molten steel smelting: The chemical composition of the steel is C: 0.20-0.30%, Si: 0.15-0.35%, Mn: 1.10-1.30%, Cr: 0.90-1.20%, Al: 6.00-9.00%, and the balance is Fe and inevitable impurity elements; in the molten steel smelting stage, the alloy element content of the molten steel is adjusted according to the chemical composition of the steel; In the molten steel smelting stage, electric furnace or converter smelting and refining outside the furnace are adopted. After the refining starts, silicon carbide is first added for deoxidation, and the oxygen content in the steel is rapidly reduced in the early stage of refining until the oxygen content is ≤30ppm, and then the electric smelting is continued. Before the end of smelting, aluminum particles are added, and the particle size of the aluminum particles is not more than φ30mm×50mm, so that the aluminum particles are quickly melted. After the aluminum content reaches the set range, argon is blown from the bottom of the ladle for stirring; Continuous Casting: The continuous casting is carried out after the refining is completed. The molten steel is transferred to the crystallizer through the tundish. The CaO content in the crystallizer protective slag is 35-40wt%. The Al2O3 captured by the protective slag combines with CaO to form low-melting-point calcium aluminum oxide, so that the slag surface remains continuously stable. During continuous casting, the internal structure of the nozzle is gourd-shaped: the top and bottom are wide, and the middle is narrow. Heating rolling: The ingot is heated until the structure is completely austenitized, the elements are fully melted, and the structure is homogenized, and then it is immediately taken out of the furnace for forging and opening, forging into small square billets, and the small square billets are put back into the furnace for equalization, and the structure is completely austenitized, and then rough rolling, finish rolling, and final rolling are performed to obtain hot-rolled bars; annealing: In the annealing stage, the steel is kept at 800-900°C for a holding time that depends on the specifications of the rolled material and is not less than 1.2 min / mm*D, where D is the diameter of the steel in mm. The steel is then cooled to 600-750°C for isothermal transformation for a isothermal time of 1.8 min / mm*D, where D is the diameter of the steel in mm. The steel is then naturally cooled in the furnace to obtain a ferrite + pearlite structure after annealing.

2. The method for manufacturing a gear steel bar that is beneficial to the lightweighting of a gearbox according to claim 1, characterized in that: The chemical composition of the steel also includes one or more elements of Ni, Mo, Cu, Ti, and B, and the added amount is ≤0.25%; during the molten steel smelting stage, the alloy element content of the molten steel is adjusted according to the chemical composition of the steel.

3. The method for manufacturing a gear steel bar that is beneficial to the lightweighting of a gearbox according to claim 1, characterized in that: The residual elements P and S in the steel are usually ≤0.030%.

4. The method for manufacturing a gear steel bar that is beneficial to the lightweighting of a gearbox according to claim 1, characterized in that: In the heating stage of the casting, the heating temperature is 1120-1200°C and the temperature is kept for 4-6 hours; in the heating stage of the small square billet, the equalizing temperature is 1120-1200°C.

5. The method for manufacturing a gear steel bar that is beneficial to the lightweighting of a gearbox according to claim 1, characterized in that: During the hot rolling stage, the ingot is forged into 200×200 mm 2 The small square billets are finally rolled into hot-rolled bars with a diameter of 30 to 60 mm.

Citation Information

Patent Citations

  • Cold rolling medium-manganese high-aluminum low-density steel and preparation method thereof

    CN108396244A

  • Hardened martensitic steel having low cobalt content, process for manufacturing part from this steel, and parts thus obtained

    CN102131947A

  • Easy-cutting steel iron material for building and preparation method thereof

    CN110284074A

  • High-strength gear steel 23CrMnMoS and manufacturing method thereof

    CN112899560A

  • Lightweight crankdrive and method for manufacturing same

    WO2012065674A1