A preparation process of regenerated full-dull ultra-fine denier polyester fiber

By optimizing the production process of ultra-fine denier fibers, including crystallization drying, screw extrusion, side blow cooling and network forming, combined with slow cooling areas and improved yarn guides, the problem of poor performance of ultra-fine denier fibers in the existing technology has been solved and achieved Developed mass production of regenerated ultra-fine denier fibers with high performance and high spinnability.

CN116497472BActive Publication Date: 2024-10-01浙江佳人新材料有限公司
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310341135.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-03
Publication Date
2024-10-01
Estimated Expiration
2043-04-03

AI Technical Summary

Technical Problem

The existing ultra-fine denier fiber production process is complex and technically difficult, and the performance of regenerated ultra-fine denier fiber is average, which cannot fully meet market demand.

Method used

After crystallization and drying using regenerated semi-dull polyester chips, they are melted into primary filament bundles through a screw extruder, and then undergo heating, side blow cooling, cluster oiling, pre-networking, drafting and setting, and main network node creation, and finally rolled Winding molding to form regenerated fully matted ultra-fine denier polyester fiber. In this process, 800 mesh mesh and honeycomb panels are installed on the side blowing windows to form a slow cooling area, improve the spinnability of the fiber, and reduce friction through an improved yarn guide mechanism.

Benefits of technology

It has realized the mass production of high-performance, high-spinnability regenerated ultra-fine denier fiber to meet market demand, improved the strength and spinnability of the fiber, and reduced the wool content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116497472B_ABST
    Figure CN116497472B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation process of a regenerated full-dull ultra-fine denier polyester fiber, comprising the steps of: (a) adding a regenerated semi-dull polyester slice into a crystallization drying system for crystallization drying; (b) conveying the dried regenerated semi-dull polyester slice to a screw extruder for extrusion melting, and then conveying the melt to a spinning box, and after being metered by a metering pump, pressing the melt into a spinning assembly for extrusion to form a nascent tow; (c) the nascent tow is subjected to post-heating, side-blowing cooling, and bundle oiling treatment, and then to pre-networking, drafting and shaping, main network device network node beating, and winding to obtain a regenerated full-dull ultra-fine denier polyester fiber; the side-blowing window used for side-blowing cooling includes a filter screen, an 800-mesh mesh, and a honeycomb board installed from the inside to the outside, the mesh is installed on the upper part of the honeycomb board, and the mesh is 100 mm high. The invention realizes the mass production of high-performance, high-spinnability regenerated ultra-fine denier fibers, fully meeting market demand.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of spinning, in particular to a preparation process of regenerated full-dull ultra-fine denier polyester fiber. Background Art

[0002] With the development of social economy and the continuous improvement of material living standards, people have more demands on the functions and characteristics of textiles, which requires more differentiated products to meet people's different needs. Ultrafine denier fiber is finer than traditional fiber, so it is more fluffy and softer than ordinary fiber, and can overcome the characteristics of natural fiber wrinkle easily and artificial fiber airtightness. At the same time, because ultrafine denier fiber is extremely fine, it can increase the layered structure of silk, increase the surface area and capillary effect, make the reflected light inside the fiber more delicate on the surface, and make it have an elegant luster like silk. However, due to the extremely fine monofilament of ultrafine denier fiber, the production process is complex and the technical difficulty is great. In addition, most of the ultrafine denier fibers on the market are original fibers. There are few regenerated ultrafine denier fibers, but the performance is average, the spinnability is not ideal, and it cannot fully meet the use needs. Summary of the invention

[0003] The purpose of the present invention is to overcome the deficiencies of the above-mentioned prior art and provide a preparation process for regenerated full-dull ultrafine denier polyester fibers, thereby realizing the mass production of high-performance, high-spinnability regenerated ultrafine denier fibers and fully meeting market demand.

[0004] In order to achieve the above object, the present invention adopts the following technical solution:

[0005] A preparation process of regenerated full-dull ultra-fine denier polyester fiber, comprising the following steps:

[0006] (a) adding the regenerated semi-dull polyester chips into a crystallization drying system for crystallization drying;

[0007] (b) conveying the dried regenerated semi-gloss polyester chips to a screw extruder for extrusion melting, and then conveying the melt to a spinning box, and after being metered by a metering pump, pressing it into a spinning assembly for extrusion to form a primary filament bundle;

[0008] (c) The spun filament bundle is subjected to post-heating, side-blowing cooling, bundling and oiling treatment, and then to pre-networking, drawing and shaping, main network device network node beating, and winding to obtain regenerated full-dull ultrafine denier polyester fiber; the side-blowing air window used for side-blowing cooling includes a filter screen, an 800-mesh mesh and a honeycomb panel installed in sequence from the inside to the outside according to the air outlet direction, and the mesh is installed on the upper part of the honeycomb panel, and the mesh height is 100 mm.

[0009] In step (a), the crystallization temperature is 158° C., the drying temperature is 168° C., and the drying air pressure is 0.11 MPa.

[0010] In step (b), the diameter of the screw extruder is 120 mm, the aspect ratio is 25, there are six heating zones, and the temperatures of the heating zones are: 278° C. in zone 1, 282° C. in zone 2, 284° C. in zone 3, 286° C. in zone 4, 288° C. in zone 5, and 291° C. in zone 6; the extrusion pressure of the screw extruder is 12.5 MPa, and the pressure after filtration is 9.8 MPa.

[0011] In step (b), 70 g of 100-120 mesh metal sand is used in the spinning assembly.

[0012] The spinneret in the spinning assembly has an aspect ratio of 3, and the spinneret includes four circles of concentrically distributed spinnerets, the four circles of spinnerets (4) are the first circle, the second circle, the third circle, and the fourth circle from the inside to the outside, and the number of spinnerets in the first to fourth circles is two in a straight line, twelve in a prismatic shape, eighteen in a prismatic shape, and sixteen in a prismatic shape, respectively; the diameter of the spinneret is 0.14 mm.

[0013] In step (c), the post-heating temperature is 315° C. and the wind speed of the side blowing is 0.3 m / s.

[0014] In step (c), the bundle oiling adopts the nozzle oiling method, and the distance between the nozzle and the spinneret of the spinning assembly is 700mm; the oil pump specification used in the bundle oiling is 0.02cc / rec, the oil pump speed is 37r / min, and the oil concentration is 14wt%.

[0015] In step (c), the pre-network pressure is 0.07 MPa; the main network pressure is 0.25 MPa.

[0016] In step (c), the stretching ratio during stretching and shaping is 2.1, the rotation speeds of the first stretching roller and the second stretching roller are both 2182 / min, the temperature is both 80°C, the rotation speed of the third stretching roller is 4552m / min, and the temperature is 122°C.

[0017] In step (c), during the winding process, the winding speed is 4495 m / min, the winding angle is 6.3 degrees, the head pressure of the winding machine is 292 cN, and the winding tension is 6-7 cN.

[0018] The beneficial effects of the present invention are as follows: by optimizing and improving the production process, the mass production of regenerated full-dull ultrafine denier polyester fibers that meet the performance indicators of original ultrafine denier fibers is achieved, and the market demand for regenerated ultrafine denier fibers is fully met; by installing a 100mm high 800-mesh mesh on the upper part of the honeycomb plate, a slow cooling area is formed above the side-blowing window to prevent the filament bundle from cooling too quickly, thereby increasing the spinnability of the regenerated ultrafine denier fibers. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a side view of the mesh installation structure in the present invention;

[0020] Figure 2 It is a front view showing the mesh sheet installed on the honeycomb panel in the present invention;

[0021] Figure 3 Schematic diagram of the spinneret hole distribution of the spinneret of the present invention;

[0022] Figure 4 It is a structural diagram of the wire guide mechanism of the present invention;

[0023] Figure 5 for Figure 4 Cross-section view along the AA direction.

[0024] In the figure: filter screen 1, mesh 2, honeycomb plate 3, spinneret hole 4, ventilation pipe 5, through hole 51, positioning sleeve 6, sleeve member 61, step portion 62, wire guide 7, wire guide groove 71, micropore 72, cavity 8. DETAILED DESCRIPTION

[0025] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments:

[0026] Example

[0027] A preparation process of regenerated full-dull ultra-fine denier polyester fiber, comprising the following steps:

[0028] (a) Adding the regenerated semi-dull polyester chips into a crystallization drying system for crystallization drying; the crystallization temperature is 158° C., the drying temperature is 168° C., and the drying air pressure is 0.11 MPa.

[0029] (b) conveying the dried regenerated semi-gloss polyester chips to a screw extruder for extrusion melting, and then conveying the melt to a spinning box, and after being metered by a metering pump, pressing it into a spinning assembly for extrusion to form a primary filament bundle;

[0030] In step (b), the diameter of the screw extruder is 120 mm, the aspect ratio is 25, there are six heating zones, and the temperatures of the heating zones are: 278°C in zone one, 282°C in zone two, 284°C in zone three, 286°C in zone four, 288°C in zone five, and 291°C in zone six; the extrusion pressure of the screw extruder is 12.5 MPa, and the pressure after filtration is 9.8 MPa. 70 g of 100-120 mesh metal sand is used in the spinning assembly. The aspect ratio of the spinneret in the spinning assembly is 3, and the spinneret includes four circles of concentrically distributed spinnerets 4, and the diameter of the spinneret 4 is 0.14 mm. The four circles of spinneret holes 4 are, from the inside to the outside, the first circle, the second circle, the third circle, and the fourth circle, and the number of spinneret holes 4 from one to four circles are, respectively, two distributed in a straight line, twelve distributed in a prismatic shape, eighteen distributed in a prismatic shape, and sixteen distributed in a prismatic shape. Further, as Figure 1As shown, the two spinnerets 4 of the first circle are distributed on the center line L of the spinneret, and the two spinnerets 4 are symmetrically distributed with the center line M perpendicular to the center line L as the axis of symmetry; the four vertices of the prism formed by the spinneret 4 of the second circle are located on the center line L and the center line M, and spinnerets 4 are arranged at the four vertices of the prism, and four spinnerets 4 are distributed on each side of the prism; the prism formed by the spinneret 4 of the third circle has the center line L and the center line M as the axis of symmetry, a pair of vertices of the prism is located on the center line M and spinnerets 4 are arranged at the two vertices, no spinnerets 4 are arranged at the other two prism vertices, and five spinnerets 4 are distributed on each side of the prism; the prism formed by the fourth circle of spinneret holes 4 has the center line L and the center line M as the axis of symmetry, no spinnerets 4 are arranged at the four vertices of the prism, and four spinnerets 4 are distributed on each side of the prism.

[0031] (c) The spun tow is subjected to post-heating, side-blowing cooling, bundling and oiling treatment, and then to pre-networking, drafting and shaping, main network device network node beating, and winding to obtain a regenerated full-dull ultrafine denier polyester fiber; the side-blowing air window used for side-blowing cooling includes a filter screen 1, an 800-mesh mesh 2 and a honeycomb panel 3 installed in sequence from the inside to the outside according to the air outlet direction, the mesh 2 is installed on the upper part of the honeycomb panel 3, the mesh 2 is 100 mm high, and the mesh 2 is 100 mm high. Figure 2 As shown. The mesh is arranged above the side-blowing window to form a slow cooling area to prevent the filament bundle from cooling too quickly, thereby increasing the spinnability of the ultra-fine denier filament.

[0032] In this step (c), the post-heating temperature is 315°C; the wind speed of the side blowing is 0.3m / s. The nozzle oiling method is used for cluster oiling, and the distance between the nozzle and the spinneret of the spinning assembly is 700mm; the oil pump specification used for cluster oiling is 0.02cc / rec, the oil pump speed is 37r / min, and the oil concentration is 14wt%. The pre-network pressure is 0.07Mpa; the main network pressure is 0.25Mpa. The stretching ratio during stretching and shaping is 2.1, the speeds of the first stretching roller and the second stretching roller are both 2182 / min, the temperature is 80°C, the speed of the third stretching roller is 4552m / min, and the temperature is 122°C. During the winding process, the winding speed is 4495m / min, the winding angle is 6.3 degrees, the head pressure of the winder is 292cN, and the winding tension is 6-7cN.

[0033] The properties of the regenerated full-dull ultra-fine denier polyester fiber produced in the embodiment of the present invention are shown in the following table:

[0034] project Measured value Line density 22.6dtex Linear density coefficient of variation 0.66% Breaking strength 4.25cN / dtex Coefficient of variation of strength 2.58% Elongation at break 28.86% Coefficient of variation of elongation at break 9.36% Boiling water shrinkage 7.78% 60% elongation strength 70.92cN Strip uniformity cv 1.83% Oil content 1.11% Network Degree 36 pieces / m

[0035] Regenerated full-dull ultrafine polyester fibers were prepared according to the method of the embodiment but without installing the mesh. It was found that the resulting fibers had a breaking strength of 3.98 cN / dtex, an elongation at break of 25.45%, a boiling water shrinkage of 7.21%, a yarn uniformity of 1.47%, and poor spinnability.

[0036] A yarn guide is required in the spinning production of regenerated full-dull ultrafine denier polyester fibers, but the yarn guides in the prior art are fixedly installed, and the yarn bundles produce sliding friction when passing through the yarn guides. Since the single-filament fineness of ultrafine denier fibers is relatively low, the surface area of ​​the yarn bundles increases, the spinning tension increases, and the friction increases when in contact with the yarn guides, which makes it easier to produce fuzzy yarns and broken ends, affecting product quality and production efficiency.

[0037] Based on the above reasons, the present invention improves the wire guide mechanism, such as Figure 4-5 As shown, the wire guide mechanism includes a ventilation pipe 5, a plurality of positioning sleeves 6 installed along the length direction of the ventilation pipe 5, and a wire guide 7 circumferentially rotatably sleeved on the positioning sleeve 6, the positioning sleeve 6 includes a pair of sleeve members 61 arranged at intervals, the outer wall of the sleeve member 61 is provided with a step portion 62, the two step portions 62 of the positioning sleeve 6 are arranged opposite to each other, the wire guide 7 is a hollow cylindrical structure, the wire guide 7 is slidably sleeved between the step portions 62 of a pair of sleeve members 61, the annular inner wall of the wire guide 7 and the pair of step portions 62 and the annular outer wall of the ventilation pipe 5 form an annular cavity 8, the annular outer wall of the wire guide 7 is recessed to form an annular wire guide groove 71, the wire guide groove 71 is connected with the cavity 8 through a plurality of groups of micropores 72, the plurality of groups of micropores 72 are circumferentially evenly distributed, the ventilation pipe 5 is provided with a plurality of groups of through holes 51, and a group of through holes 51 is correspondingly connected to a cavity 8.

[0038] Each group of micro-holes 72 includes a plurality of micro-holes 72, and the micro-holes 72 of the same group are distributed on the same radial surface. Each group of micro-holes 72 is distributed in a fan shape with the center point of the arc surface of the wire guide groove 71 as the center point. That is, the intersection point of a group of micro-holes 72 on the same radial surface is the center point of the arc surface of the wire guide groove 71 on the same radial surface.

[0039] Each group of through holes 51 includes a plurality of through holes distributed around the circumference.

[0040] The wire guide 7 is slidably connected to the positioning sleeve 6, so that rolling friction is generated between the wire bundle passing through the wire guide groove 71 and the wire guide 7, thereby reducing friction; each micropore 72 is connected to the cavity 8, and is connected to the inner cavity of the ventilation pipe 5 through the through hole 51. The gas in the ventilation pipe 5 flows into the wire guide groove 71. Due to the fan-shaped distribution of each group of micropores 72 and the ultra-fine denier characteristics of the fiber, the gas forms a cushion-like effect between the wire bundle and the inner wall of the wire guide groove 71, further reducing the friction between the wire bundle and the wire guide.

[0041] The improved yarn guide mechanism is used to carry out batch production of regenerated full-dull ultra-fine denier polyester fibers according to the method of the embodiment. Compared with the batch production of fibers according to the method of the embodiment, the fuzz rate of the regenerated full-dull ultra-fine denier polyester fibers is reduced by 16.2%, and the strength of the obtained regenerated full-dull ultra-fine denier polyester fibers is increased by 5.8%.

[0042] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A process for preparing regenerated full-dull ultrafine denier polyester fiber, characterized in that: The following steps are involved: (a) adding the regenerated semi-dull polyester chips into a crystallization drying system for crystallization drying; (b) conveying the dried regenerated semi-gloss polyester chips to a screw extruder for extrusion melting, and then conveying the melt to a spinning box, and after being metered by a metering pump, pressing it into a spinning assembly for extrusion to form a primary filament bundle; (c) the spun filament bundle is subjected to post-heating, side-blowing cooling, bundling and oiling treatment, and then to pre-networking, drafting and shaping, main network device network node beating, and winding to obtain a regenerated full-dull ultra-fine denier polyester fiber; the side-blowing window used for side-blowing cooling comprises a filter screen (1), an 800-mesh mesh (2) and a honeycomb panel (3) which are installed in sequence from the inside to the outside according to the air outlet direction, the mesh (2) being installed on the upper part of the honeycomb panel (3), and the mesh (2) being 100 mm high; The yarn guide mechanism in spinning production comprises a vent pipe (5), a plurality of positioning sleeves (6) installed along the length direction of the vent pipe (5), and a yarn guide (7) rotatably sleeved on the positioning sleeve (6), wherein the positioning sleeve (6) comprises a pair of sleeve members (61) arranged at intervals, the outer wall of the sleeve member (61) is provided with a step portion (62), the two step portions (62) of the positioning sleeve (6) are arranged opposite to each other, the yarn guide (7) is a hollow cylindrical structure, the yarn guide (7) is slidably sleeved between the step portions (62) of the pair of sleeve members (61), the annular inner wall of the yarn guide (7) is rotatably sleeved between the pair of step portions (62), the vent pipe (5), and the yarn guide (7) is rotatably sleeved on the pair of step portions (62). The annular outer wall of the tube (5) forms an annular cavity (8), the annular outer wall of the wire guide (7) is recessed to form an annular wire guide groove (71), the wire guide groove (71) is connected to the cavity (8) through a plurality of groups of micropores (72), the plurality of groups of micropores (72) are evenly distributed in the circumferential direction, each group of the micropores (72) includes a plurality of micropores (72), the same group of the micropores (72) are distributed on the same radial plane, each group of the micropores (72) is distributed in a fan shape with the center point of the arc surface of the wire guide groove (71) as the center, the ventilation tube (5) is provided with a plurality of groups of through holes (51), and a group of through holes (51) is correspondingly connected to a cavity (8).

2. A process for preparing a regenerated full-dull ultra-fine denier polyester fiber as claimed in claim 1, characterized in that: In step (a), the crystallization temperature is 158° C., the drying temperature is 168° C., and the drying air pressure is 0.11 MPa.

3. The process for preparing a regenerated full-dull ultra-fine denier polyester fiber as claimed in claim 1, characterized in that: In step (b), the diameter of the screw extruder is 120 mm, the aspect ratio is 25, there are six heating zones, and the temperatures of the heating zones are: zone 1 278°C, zone 2 282°C, zone 3 284°C, zone 4 286°C, zone 5 288°C, zone 6 291°C; the extrusion pressure of the screw extruder is 12.5 MPa, and the pressure after filtration is 9.8 MPa.

4. The process for preparing a regenerated full-dull ultra-fine denier polyester fiber as claimed in claim 1, characterized in that: In step (b), 70 g of 100-120 mesh metal sand is used in the spinning assembly.

5. The process for preparing a regenerated full-dull ultra-fine denier polyester fiber as claimed in claim 1, characterized in that: The spinneret in the spinning assembly has an aspect ratio of 3, and the spinneret comprises four circles of concentrically distributed spinneret holes (4). The four circles of spinneret holes (4) are, from the inside to the outside, the first circle, the second circle, the third circle, and the fourth circle. The number of the spinneret holes (4) in the first to fourth circles is, respectively, two in a straight line, twelve in a prismatic shape, eighteen in a prismatic shape, and sixteen in a prismatic shape. The diameter of the spinneret holes (4) is 0.14 mm.

6. The process for preparing a regenerated full-dull ultra-fine denier polyester fiber as claimed in claim 1, characterized in that: In step (c), the post-heating temperature is 315° C. and the wind speed of the side blowing is 0.3 m / s.

7. The process for preparing a regenerated full-dull ultra-fine denier polyester fiber as claimed in claim 1, characterized in that: In step (c), the bundle oiling adopts the nozzle oiling method, and the distance between the nozzle and the spinneret of the spinning assembly is 700 mm; the oil pump specification used in the bundle oiling is 0.02cc / rec, the oil pump speed is 37r / min, and the oil concentration is 14wt%.

8. The process for preparing a regenerated full-dull ultra-fine denier polyester fiber as claimed in claim 1, characterized in that: In step (c), the pre-network pressure is 0.07 MPa; the main network pressure is 0.25 MPa.

9. The process for preparing a regenerated full-dull ultra-fine denier polyester fiber as claimed in claim 1, characterized in that: In step (c), the stretching ratio during stretching and shaping is 2.1, the rotation speeds of the first stretching roller and the second stretching roller are both 2182 m / min, the temperatures are both 80°C, and the rotation speed of the third stretching roller is 4552 m / min, the temperature is 122°C.

10. The process for preparing a regenerated full-dull ultra-fine denier polyester fiber as claimed in claim 1, characterized in that: In step (c), during the winding process, the winding speed is 4495 m / min, the winding angle is 6.3 degrees, the head pressure of the winding machine is 292 cN, and the winding tension is 6-7 cN.

Citation Information

Patent Citations

  • Method for preparing superfine denier flat terylene drawn yarn

    CN102031575A

  • Complete-extinction thin and light meshy polyamide fiber 6 draw textured yarn (DTY) manufacture method

    CN103046147A

  • Production method of environment-friendly regenerated FDY lustrous fine denier fiber

    CN113668077A

  • Spinning machine

    CN205398788U

  • Melt spinning machine

    JP2000034614A