A Cf / (Ti, Zr, Hf)C medium-entropy ceramic-based composite material and preparation method thereof

By depositing a high-textured pyrolysis carbon interface layer and multiple rounds of impregnation and cracking technology on the carbon fiber surface, the problems of poor brittleness and toughness of medium-entropy ceramic materials in high-temperature environments are solved, and Cf/(Ti,Zr,Hf)C are improved. The mechanical properties and oxidation and ablation resistance of entropy ceramic matrix composite materials meet the needs of high-temperature structural parts of hypersonic aircraft.

CN116514565BActive Publication Date: 2024-11-12BEIJING INST OF TECH +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310596768.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-11-12
Estimated Expiration
2043-05-25

AI Technical Summary

Technical Problem

Medium entropy ceramic materials have problems of high brittleness and poor toughness in high temperature environments, and the corrosion of the fibers by the precursor in traditional preparation processes leads to low mechanical properties of composite materials, which is difficult to meet the requirements of high-temperature structural parts of hypersonic aircraft.

Method used

Using multiple rounds of impregnation and cracking processes with different viscosity, Cf/(Ti, Zr, Hf) with good interface bonding is prepared by depositing a high texture pyrolysis carbon interface layer on the surface of carbon fibers, combined with chemical vapor deposition method and vacuum impregnation technology. C medium entropy ceramic matrix composite material reduces preparation temperature and improves component uniformity and mechanical properties.

Benefits of technology

Efficient preparation of composite materials is achieved at lower temperatures, significantly improving the interface combination between ceramics and fibers, improving the mechanical properties and oxidation and ablation resistance of composite materials, and can perform excellent in an environment of 2600℃~2800℃ The ablation resistance performance meets the requirements of high-temperature structural parts of hypersonic aircraft.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116514565B_ABST
    Figure CN116514565B_ABST
Patent Text Reader

Abstract

The invention discloses a Cf / (Ti, Zr, Hf)C medium entropy ceramic-based composite material and a preparation method thereof, comprising the following steps: step 1: preparing a high-texture pyrolytic carbon interface phase on the surface of a composite material preform; step 2: impregnating the composite material preform; step 3: cross-linking and curing the impregnated composite material preform; step 4: cracking the cross-linked and cured composite material preform; step 5: repeating steps 2, 3 and 4 until the density of the obtained composite material preform reaches 2.5 to 3.5 g / cm 3 The present invention adopts the above-mentioned Cf / (Ti, Zr, Hf)C medium-entropy ceramic-based composite material and its preparation method, which effectively improves the interface bonding between ceramics, pyrolytic carbon and carbon fiber, alleviates the problem of precursor erosion of fibers, and adopts multiple rounds of different viscosities to achieve efficient impregnation and cracking of the composite material at a lower temperature, thereby improving the composition uniformity and bending mechanical properties of the composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ceramic-based composite materials, and in particular to a Cf / (Ti, Zr, Hf)C medium-entropy ceramic-based composite material and a preparation method thereof. Background Art

[0002] The development of a new generation of spacecraft has aroused people's strong interest in ultra-high temperature refractory materials. When the Mach number of hypersonic vehicles increases from Mach 6 to Mach 10 or above, the surface temperature of its high-temperature structural parts such as the end and leading edge can reach 2000-2800℃, accompanied by strong oxidation and airflow scouring environment. Therefore, the corresponding materials need to have a higher melting point. At present, ultra-high temperature ceramic matrix composites based on zirconium carbide-silicon carbide, zirconium boride-silicon carbide, hafnium carbide-silicon carbide, etc. are difficult to meet such harsh high-temperature use environments, and the matrix components of ceramic matrix composites need to be improved.

[0003] In recent years, medium-entropy carbide ceramics have attracted much attention due to their extremely high melting point, high hardness, high thermal conductivity and good oxidation resistance. Compared with single-phase ceramics, medium-entropy ceramics have higher mechanical properties and better oxidation resistance, and are expected to become candidate materials for high-temperature structural parts of future higher Mach number aircraft. However, medium-entropy ceramic materials have problems such as high brittleness and poor toughness. In addition, the commonly used process methods for preparing continuous fiber-reinforced ceramic-based composites include slurry impregnation, chemical vapor deposition, reactive melt infiltration, and precursor impregnation pyrolysis. Compared with other preparation processes, the precursor impregnation pyrolysis (PIP) method can be carried out at a lower preparation temperature, which effectively reduces the damage to the fiber preform during the preparation process and improves the mechanical properties of the composite material. More importantly, the elements in the polymer precursor are evenly dispersed at the molecular level, and the uniform distribution of the elements is maintained during the curing and pyrolysis process, which is conducive to obtaining completely chemically uniform solid solution ceramics. However, the preparation of ceramic-based composites by the PIP method requires multiple rounds of impregnation and pyrolysis processes. The ultra-high temperature ceramic precursors are prone to react with the carbon fiber interface during the pyrolysis process, corroding the fiber matrix, causing fiber bundle deformation, forming large defects inside the composite, and resulting in low mechanical properties of the prepared composite. Therefore, how to ensure that the ceramic and fiber fabric inside the prepared composite have a good interface bonding, and adjust the fiber bending fracture mode to improve the mechanical properties of the composite is a key issue. f There are key problems that need to be solved urgently in the preparation and use of medium-entropy ceramic-based composites in / (Ti,Zr,Hf)C. Summary of the invention

[0004] The purpose of the present invention is to provide a Cf / (Ti, Zr, Hf)C medium-entropy ceramic-based composite material and a preparation method thereof, which effectively improves the interface bonding between ceramics, pyrolytic carbon and carbon fibers, alleviates the problem of precursor erosion of fibers, and uses multiple rounds of different viscosities to achieve efficient impregnation and cracking of the composite material at a lower temperature, thereby improving the composition uniformity and bending mechanical properties of the composite material.

[0005] To achieve the above object, the present invention provides a Cf / (Ti, Zr, Hf)C medium-entropy ceramic-based composite material and a preparation method thereof, comprising the following steps:

[0006] Step 1: preparing a high-textured pyrolytic carbon interface phase on the surface of the composite material preform;

[0007] Step 2: impregnating the composite material preform;

[0008] Step 3: cross-linking and curing the impregnated composite material preform;

[0009] Step 4: cracking the cross-linked and cured composite material preform;

[0010] Step 5: Repeat steps 2, 3 and 4 until the density of the composite material preform reaches 2.5-3.5 g / cm 3 .

[0011] Preferably, in step 1, the fiber volume fraction of the composite material preform is 45-55%, the composite material preform is placed in a chemical vapor deposition furnace, the heating rate is 3-5°C / min, and the deposition temperature is kept at 900-1000°C for 1 hour, and a methane deposition gas source is introduced into the chemical vapor deposition furnace, the heating rate is 3-5°C / min, and the deposition temperature is kept at 900-1000°C for 1 hour, and a density of 1.1-1.4 g / cm 3 A composite preform with a highly textured pyrolytic carbon interfacial phase.

[0012] Preferably, in step 2, the obtained composite material preform with a high-textured pyrolytic carbon interface phase is placed in an impregnation tank, which is then sealed and evacuated to a pressure of -0.1 MPa to -0.05 MPa inside the tank, and the precursor solution is drawn in by vacuum suction and impregnated under vacuum pressure conditions for 1 to 2 hours.

[0013] Preferably, the solute of the precursor solution includes a precursor and a carbon source precursor, the solvent of the precursor solution is an organic solvent, and the viscosity of the precursor solution is divided into a low viscosity of 100 to 150 mPa.s and a high viscosity of 250 to 300 mPa.s.

[0014] Preferably, the precursor is prepared by co-hydrolysis and condensation of titanate propyl, zirconate propyl and hafnium propyl; the carbon source precursor is one or more of phenolic resin, furfural resin, sucrose and furan resin; the organic solvent is one or more of methanol, isopropanol, ethanol, n-propanol, isobutanol, n-butanol, ethylene glycol methyl ether and ethylene glycol ethyl ether.

[0015] Preferably, in step 3, after the impregnation work is completed, the composite material preform and the precursor solution after vacuum impregnation are transferred to a pressurized impregnation kettle, an inert gas is introduced into the impregnation kettle, and the mixture is impregnated for 1 hour at a pressure of 2 to 5 MPa and a temperature of 100°C. The composite material preform is released and taken out for cross-linking and curing in a blast oven.

[0016] Preferably, the inert gas is argon or nitrogen, and the flow rate of the introduced gas is 1 to 1000 sccm.

[0017] Preferably, in step 4, the obtained cross-linked and cured composite material preform is placed in a cracking furnace under vacuum environment or inert atmosphere protection for cracking, the temperature of low-temperature cracking is 1400-1500°C, the temperature of high-temperature cracking is 1700-1800°C, and the heating rate is 5-20°C / min.

[0018] A Cf / (Ti, Zr, Hf)C medium-entropy ceramic-based composite material prepared according to the above-mentioned method for preparing a Cf / (Ti, Zr, Hf)C medium-entropy ceramic-based composite material.

[0019] Preferably, the Cf / (Ti, Zr, Hf)C medium-entropy ceramic-based composite material has a carbon fiber preform as a skeleton, the volume fraction of the carbon fiber preform is 45-55%, and a high-texture pyrolytic carbon interface phase is deposited on the surface of the carbon fiber preform; and the (Ti, Zr, Hf)C medium-entropy ceramic is used as a matrix, and the oxygen content in the matrix is ​​not higher than 2%.

[0020] Therefore, the present invention adopts the above-mentioned Cf / (Ti, Zr, Hf)C medium-entropy ceramic-based composite material and its preparation method, which has the following beneficial effects:

[0021] (1) Compared with the conventional method of sintering a plurality of carbide powders or incorporating carbide powders into prepreg, the method of the present invention can obtain a nano-scale single-phase (Ti, Zr, Hf) C ceramic product at a relatively low temperature of 1400°C to 1500°C, and each element component is evenly distributed from micrometer to nanometer. The prepared composite material has good mechanical properties and excellent anti-oxidation and ablation performance for a long time of 1000s under an extreme environment of 2600°C to 2800°C.

[0022] (2) The high fiber volume content preform used in the present invention utilizes chemical vapor deposition to deposit a pyrolytic carbon interface layer with a high texture on the surface of the carbon fiber. The pyrolytic carbon grows around the fiber bundle during the deposition process, has a higher microcrystalline crystallinity, fewer defects, and more obvious guidance. At the junction of the remaining fibers, there are sublayers and bridge structures, which can effectively improve the interface bonding between the ceramic and the fiber, alleviate the erosion of the precursor on the fiber, and thus achieve better interface matching. The high-texture pyrolytic carbon interface layer can not only significantly reduce the physical and chemical damage to the fiber bundle during the cracking process, but also make the cracks transmitted from the ceramic matrix to the carbon fiber preferentially deflected at the high-texture interface layer, reducing the generation of cracks inside the fiber bundle, thereby promoting the energy consumption of fiber pull-out and improving the bending strength of the composite.

[0023] (3) The precursor of the present invention has an adjustable carbon source ratio content, which minimizes the erosion of the fiber bundle and the high-texture pyrolytic carbon interface on the surface of the fiber bundle during the PIP process while ensuring carbon vacancy. In conjunction with the viscosity of the precursor, a multi-round impregnation and cracking process at different temperatures is designed to ensure a smaller grain size of the ceramic and achieve efficient impregnation preparation of the composite material.

[0024] (4) The method of the present invention has a simple process, a short preparation period, is easy to implement industrially, and can prepare complex and special-shaped components of various sizes. f / (Ti,Zr,Hf)C medium-entropy ceramic-based composite materials have good mechanical properties and excellent anti-ablation properties. They have passed the 1000s, 3000K atmospheric plasma wind tunnel ablation test, and can meet the service requirements of high-temperature structural parts of hypersonic aircraft. They can be widely used in the preparation of high-temperature structural parts of hypersonic aircraft, such as in the leading edge, engine, and end of new aircraft, and have broad application prospects.

[0025] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a microscopic morphology of a preform having a high-textured pyrolytic carbon interface layer prepared by chemical vapor deposition in Example 1 of the present invention;

[0027] Figure 2 The single-phase C obtained after the pyrolysis of the precursor obtained in Example 1 of the present invention f / (Ti 0.17 Zr 0.33 Hf 0.5 )C High-resolution transmission photograph of entropy ceramics, the inset of which is the diffraction pattern after Fourier transformation of this area;

[0028] Figure 3The C obtained in Example 1 of the present invention f / (Ti 0.17 Zr 0.33 Hf 0.5 ) X-ray diffraction spectrum of entropy ceramic matrix composite material in C;

[0029] Figure 4 C obtained in Example 1 of the present invention f / (Ti 0.17 Zr 0.33 Hf 0.5 ) Microstructure of the fracture surface of C-type entropy ceramic matrix composite material after three-point bending fracture. DETAILED DESCRIPTION

[0030] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0031] The present invention provides a method for preparing a Cf / (Ti, Zr, Hf)C medium entropy ceramic-based composite material, comprising the following steps:

[0032] Step 1: Prepare a high-texture pyrolytic carbon interface phase on the surface of the composite material preform: Place a fine-woven punctured carbon fiber fabric with a high fiber volume fraction into a chemical vapor deposition furnace, and heat it to 1000-1300°C at a rate of 2-5°C / min for 1-1.5 hours. Introduce a 99% pure methane deposition gas source, control the deposition pressure to 10-18kPa, the gas residence time to 0.3-0.5s, the deposition rate to 1500-2200nm / h, the deposition time to 0.5-1.5 hours, and then cool to room temperature with the furnace to deposit a high-texture pyrolytic carbon interface phase on the carbon fiber surface. The density of the preform after the interface phase is deposited reaches 1.1-1.4g / cm 3 . Then, the preform is cleaned with ultrasonic waves for 20 to 30 minutes, and placed in an oven at 100 to 150°C for 1 to 2 hours for drying;

[0033] Step 2: Impregnating the composite material preform: placing the obtained composite material preform with a high-textured pyrolytic carbon interface phase in an impregnation tank, then sealing and evacuating the impregnation tank to a pressure of -0.1 to -0.5 MPa, drawing the precursor solution in by vacuum suction, and impregnating for 1 to 2 hours under vacuum pressure conditions;

[0034] Step 3: Cross-linking and curing the impregnated composite material preform: After the impregnation work is completed, the composite material preform and the precursor solution after vacuum impregnation are transferred to a pressurized impregnation kettle, and an inert gas is introduced into the impregnation kettle. The inert gas is argon or nitrogen, and the flow rate of the gas is 1-1000sccm. The composite material preform is impregnated for 1 hour at a pressure of 2-5Mpa and a temperature of 100°C. The pressure is released and the composite material preform is taken out and cross-linked and cured in a blast oven. During the cross-linking and curing process, the heating rate is 3-5°C / min, and the temperature is kept at 100-120°C for 2-3 hours, 150-160°C for 2-3 hours, 200-220°C for 1-2 hours, and 250-300°C for 1-2 hours.

[0035] Step 4: cracking the cross-linked and cured composite material preform: placing the obtained cross-linked and cured composite material preform in a cracking furnace under vacuum or inert atmosphere for cracking, the temperature of low-temperature cracking is 1400-1500° C., the temperature of high-temperature cracking is 1700-1800° C., and the heating rate is 5-20° C. / min;

[0036] Step 5: Repeat steps 2, 3 and 4 until the density of the composite material preform reaches 2.5-3.5 g / cm 3 .

[0037] Specifically, in step 2, the solute of the precursor solution includes a precursor and a carbon source precursor, the solvent of the precursor solution is an organic solvent, and the viscosity of the precursor solution is divided into 100-150 mPa.s low viscosity and 250-300 mPa.s high viscosity. The precursor is prepared by co-hydrolysis and polycondensation of titanate propyl, zirconate propyl and hafnium propyl, and the ratio of titanium, zirconium and hafnium in the precursor is regulated by the feed ratio of the raw materials. The carbon source precursor is one or more of phenolic resin, furfural resin, sucrose and furan resin, wherein the phenolic resin is preferably allyl phenolic resin, and the mass ratio of allyl phenolic resin to the total amount of metal in the metal alkoxide copolymer is 18-22 g:1 mol. The mass ratio of the carbon source precursor to the titanium zirconium hafnium precursor copolymer is (10-20):1; the organic solvent is one or more of methanol, isopropanol, ethanol, n-propanol, isobutanol, n-butanol, ethylene glycol methyl ether, and ethylene glycol ethyl ether, preferably ethylene glycol methyl ether, and the mass ratio of the titanium zirconium hafnium precursor copolymer contained in the titanium zirconium hafnium ceramic precursor solution to the organic solvent is 10:(2-5).

[0038] Furthermore, the viscosity of the titanium zirconium hafnium precursor in step 2 is different in each round. Specifically, the viscosity of the precursor used in rounds 1 to 2 is 100 to 150 mPa.s, the viscosity of the precursor used in rounds 3 to 6 is 250 to 300 mPa.s, and the viscosity of the precursor used in rounds 7 to 8 is less than 100 mPa.s.

[0039] Furthermore, the cracking temperature of each round of step 4 is different. Specifically, the cracking temperature of each round in the first to sixth rounds is 1400-1500°C, and the cracking temperature of each round in the subsequent 7-8 rounds is 1700-1800°C; the cracking time is preferably 2-5 hours. If the preparation rounds are small, it is necessary to ensure that the last round of cracking is 1700-1800°C.

[0040] The present invention is further described below through specific examples.

[0041] Example 1

[0042] Step 1: Prepare a high-texture pyrolytic carbon interface phase on the surface of the composite material preform: Place a fine-woven punctured carbon fiber fabric with a fiber volume fraction of 53% into a chemical vapor deposition furnace, and heat it to 1100°C at a rate of 3°C / min for 1 hour. Introduce a 99% pure methane deposition gas source, control the deposition pressure to 15kPa, the gas residence time to 0.5s, the deposition rate to 2000nm / h, the deposition time to 1 hour, and cool to room temperature with the furnace to deposit a high-texture pyrolytic carbon interface phase on the carbon fiber surface. The density of the fine-woven punctured carbon fiber preform after the interface phase is deposited reaches 1.13g / cm 3 The preform with the pyrolytic carbon interface phase deposited was cleaned by ultrasonic cleaning for 20 minutes, and then dried in an oven at 120°C for 2 hours.

[0043] Step 2: Impregnation of the composite material preform: Place the composite material preform of step 1 in an impregnation tank, seal it, evacuate it for 15 minutes until the pressure in the tank is -0.1Mpa, and absorb the precursor solution, in which the molar ratio of titanium: zirconium: hafnium is 1:2:3. Impregnate it in a vacuum environment for 1 hour, then transfer the vacuum impregnated composite material and the impregnation solution to a pressure autoclave, introduce nitrogen, make the pressure at 3MPa, and heat it to 100℃ at a heating rate of 2℃ / min for 1 hour, so that the precursor solution is fully impregnated into the interior of the composite fabric.

[0044] Step 3: Cross-linking and curing the impregnated composite material preform: After the impregnation is completed, the pressure is released and the composite material preform is taken out, and the composite material preform is placed in a blast oven and heated at 3°C / min to 100°C for 3 hours, 150°C for 3 hours, 200°C for 1 hour, and 250°C for 2 hours to fully cross-link and cure the titanium zirconium hafnium precursor.

[0045] Step 4: Pyrolysis of the cross-linked and cured composite material preform: Place the fabric obtained in step 3 in a pyrolysis furnace for pyrolysis: Maintain a heating rate of 10°C / min, perform pyrolysis in an argon environment for 2 hours, cool to room temperature with the furnace, and take out the sample.

[0046] Step 5: Repeat steps 2, 3 and 4. In step 2, the viscosity of the titanium zirconium hafnium precursor is different in each round. The viscosity of the precursor used in rounds 1 to 2 is 150 mPa.s, the viscosity of the precursor used in rounds 3 to 6 is 250 mPa.s, and the viscosity of the precursor used in rounds 7 to 8 is 90 mPa.s. In step 4, the pyrolysis temperature in rounds 1 to 4 is 1500°C, and the pyrolysis temperature in rounds 6 to 8 is 1800°C. The density of the obtained composite material is 2.66 g / cm 3 .

[0047] The microscopic morphology of the preform with high fiber content and high texture interface phase prepared in this embodiment is as follows: Figure 1 As shown in the figure, the interface layer can wrap the entire fiber bundle well, which is not only beneficial to protect the fiber from the erosion of the precursor pyrolysis process, but also can achieve a good interface bonding with the ceramic phase and improve the mechanical properties of the composite material.

[0048] The single-phase C f / (Ti 0.17 Zr 0.33 Hf 0.5 ) High-resolution transmission electron microscopy images of C ceramics Figure 2 As shown, the inset is the diffraction pattern of the

[100] crystal plane after Fourier transformation in this area. The obtained product is a single phase (Ti 0.17 Zr 0.33 Hf 0.5 )C ceramics.

[0049] The C prepared in this example f / (Ti 0.17 Zr 0.33 Hf 0.5 The density of the composite material was tested by Archimedes drainage method, and the density was 2.92 g / cm 3 , the porosity is 8.9%, and the density of the composite material is relatively high.

[0050] The C prepared in this example f / (Ti 0.17 Zr 0.33 Hf 0.5 )C composite material was analyzed by XRD diffractometer, such as Figure 3 As shown, it can be seen that the material is mainly composed of C and single phase (Ti 0.17 Zr 0.33 Hf 0.5 )C composition, the characteristic diffraction peak is magnified without peak separation, and the single-phase ceramic solid solution effect is better.

[0051] The C prepared in this example f / (Ti 0.17 Zr0.33 Hf 0.5 ) The room temperature flexural strength test of C composite material was carried out by three-point bending method, and it was found that the room temperature flexural strength of the material was 252.64Mpa.

[0052] The C prepared in this example f / (Ti 0.17 Zr 0.33 Hf 0.5 )C composite material was tested for its ablation resistance in a plasma wind tunnel. 2 , the stagnation pressure is 5 kPa, and the ablation is carried out for 1000 s at a high temperature of 2973 K. The linear ablation rate is only 5.1×10 -4 mm / s, and has excellent resistance to ultra-high temperature ablation.

[0053] Example 2

[0054] The difference from Example 1 is that the present embodiment uses a stab-sewn carbon fiber fabric with a fiber volume fraction of 50%, and the density of the stab-sewn carbon fiber preform after deposition reaches 1.1 g / cm 3 The preparation method is the same as that in Example 1. The density of the prepared composite material is 2.67 g / cm 3 .

[0055] The C prepared in this example f / (Ti 0.17 Zr 0.33 Hf 0.5 The density of the composite material was tested by Archimedes drainage method, and the density was 2.76 g / cm 3 The porosity is 6.88%, and the density of the composite material is relatively high.

[0056] The C prepared in this example f / (Ti 0.17 Zr 0.33 Hf 0.5 )C composite material was analyzed by XRD diffractometer, and it can be seen that the material is mainly composed of C and single phase (Ti 0.17 Zr 0.33 Hf 0.5 )C ceramic composition, the characteristic diffraction peak is magnified but not separated, and the obtained single-phase ceramic solid solution effect is better.

[0057] The C prepared in this example f / (Ti 0.17 Zr 0.33 Hf 0.5 ) The room temperature flexural strength test of the C composite material was carried out by the three-point bending method, and it was found that the room temperature flexural strength of the material was 291.51Mpa. The fracture microstructure after the bending test is as follows Figure 4As shown, obvious fiber pull-out phenomenon can be observed.

[0058] The C prepared in this example f / (Ti 0.17 Zr 0.33 Hf 0.5 )C composite material was tested for oxyacetylene ablation resistance at a heat flux density of 5Mw / m 2 , 2700K high temperature ablation for 200s, the linear ablation rate is only 3.75×10 -4 mm / s, and has excellent resistance to ultra-high temperature ablation.

[0059] Example 3

[0060] As in Example 1, a fine-woven punctured carbon fiber fabric with a fiber volume fraction of 53% was selected for preparation, and the density of the fine-woven punctured carbon fiber preform obtained after the deposition interface phase reached 1.16 g / cm 3 The preparation method is the same as that in Example 1, and the density of the obtained composite material is 2.42 g / cm 3 .

[0061] The C prepared in this example f / (Ti 0.33 Zr 0.33 Hf 0.34 The density of the composite material was tested by Archimedes drainage method, and the density was 2.63 g / cm 3 The porosity is 7.98%, and the density of the composite material is relatively high.

[0062] The C prepared in this example f / (Ti 0.33 Zr 0.33 Hf 0.34 )C composite material was analyzed by XRD diffractometer, and it can be seen that the material is mainly composed of C and single-phase C f / (Ti 0.33 Zr 0.33 Hf 0.34 )C ceramic composition, the characteristic diffraction peak is magnified but not separated, and the obtained single-phase ceramic solid solution effect is better.

[0063] The C prepared in this example f / (Ti 0.33 Zr 0.33 Hf 0.34 ) The room temperature flexural strength test of C composite material was carried out by three-point bending method, and it was found that the room temperature flexural strength of the material was 270.45Mpa.

[0064] The C prepared in this example f / (Ti 0.33 Zr0.33 Hf 0.34 )C composite material was tested for oxyacetylene ablation resistance at a heat flux density of 5Mw / m 2 , ablation at 2700K for 200s, the linear ablation rate is only 5.12*10 -4 mm / s, and has excellent resistance to ultra-high temperature ablation.

[0065] The present invention does not describe in detail some technologies well known to those skilled in the art.

[0066] Therefore, the present invention adopts the above-mentioned Cf / (Ti, Zr, Hf)C medium-entropy ceramic-based composite material and its preparation method, which effectively improves the interface bonding between ceramics, pyrolytic carbon and carbon fiber, alleviates the problem of precursor erosion of fibers, and adopts multiple rounds of different viscosities to achieve efficient impregnation and cracking of the composite material at a lower temperature, thereby improving the composition uniformity and bending mechanical properties of the composite material.

[0067] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing a Cf / (Ti, Zr, Hf)C medium-entropy ceramic-based composite material, Features: The following steps are involved: Step 1: preparing a high-textured pyrolytic carbon interface phase on the surface of the composite material preform; Step 2: impregnating the composite material preform; Step 3: cross-linking and curing the impregnated composite material preform; Step 4: cracking the cross-linked and cured composite material preform; Step 5: Repeat steps 2, 3 and 4 until the density of the composite material preform reaches 2.5-3.5 g / cm 3 ; In the step 2, the obtained composite material preform with a high-textured pyrolytic carbon interface phase is placed in an impregnation tank, which is then sealed and evacuated to a pressure of -0.1Mpa to -0.05Mpa, and the precursor solution is drawn in by vacuum suction, and impregnated for 1 to 2 hours under vacuum pressure conditions; the solute of the precursor solution includes a precursor and a carbon source precursor, the solvent of the precursor solution is an organic solvent, and the viscosity of the precursor solution is divided into a low viscosity of 100 to 150mPa.s and a high viscosity of 250 to 300mPa.s. The viscosity of the precursor in each round is different, the viscosity of the precursor used in the first to second rounds is 100 to 150mPa.s, the viscosity of the precursor used in the third to sixth rounds is 250 to 300mPa.s, and the viscosity of the precursor used in the seventh to eighth rounds is less than 100mPa.s; In step 4, the obtained cross-linked and cured composite material preform is placed in a cracking furnace protected by a vacuum environment or an inert atmosphere for cracking, the temperature of low-temperature cracking is 1400-1500°C, the temperature of high-temperature cracking is 1700-1800°C, the heating rate is 5-20°C / min, and the cracking temperature of each round is different. The cracking temperature of each round in the first to sixth rounds is 1400-1500°C, and the cracking temperature of each round in the subsequent 7-8 rounds is 1700-1800°C. If the preparation rounds are small, it is necessary to ensure that the last round of cracking is 1700-1800°C.

2. A method for preparing a Cf / (Ti, Zr, Hf)C medium entropy ceramic-based composite material according to claim 1, Features: In the step 1, a fine-woven punctured carbon fiber fabric with a high fiber volume fraction of 45-55% is placed in a chemical vapor deposition furnace, and the temperature is increased to 1000-1300°C at a rate of 2-5°C / min for 1-1.5 hours, and then a methane deposition gas source with a purity of 99% is introduced, and the deposition pressure is controlled to be 10-18 kPa, the gas residence time is 0.3-0.5 s, the deposition rate is 1500-2200 nm / h, and the deposition time is 0.5-1.5 hours. Then, the fabric is cooled to room temperature with the furnace to obtain a density of 1.1-1.4 g / cm 3 A composite preform with a highly textured pyrolytic carbon interfacial phase.

3. A method for preparing a Cf / (Ti, Zr, Hf)C medium entropy ceramic-based composite material according to claim 1, Features: The precursor is prepared by co-hydrolysis and condensation of titanate propyl, zirconate propyl and hafnium propyl; the carbon source precursor is one or more of phenolic resin, furfural resin, sucrose and furan resin; the organic solvent is one or more of methanol, isopropanol, ethanol, n-propanol, isobutanol, n-butanol, ethylene glycol methyl ether and ethylene glycol ethyl ether.

4. A method for preparing a Cf / (Ti, Zr, Hf)C medium entropy ceramic-based composite material according to claim 1, Features: In step 3, after the impregnation work is completed, the composite material preform and the precursor solution after vacuum impregnation are transferred to a pressurized impregnation kettle, an inert gas is introduced into the impregnation kettle, and the mixture is impregnated for 1 hour at a pressure of 2 to 5 MPa and a temperature of 100° C. The composite material preform is released and taken out for cross-linking and curing in a blast oven.

5. A method for preparing a Cf / (Ti, Zr, Hf)C medium entropy ceramic-based composite material according to claim 4, Features: The inert gas is argon or nitrogen, and the flow rate of the introduced gas is 1-1000 sccm.

6. A Cf / (Ti, Zr, Hf)C medium-entropy ceramic-based composite material prepared by the method for preparing a Cf / (Ti, Zr, Hf)C medium-entropy ceramic-based composite material according to any one of claims 1 to 5.

7. The Cf / (Ti, Zr, Hf)C medium entropy ceramic matrix composite material according to claim 6, Features: The Cf / (Ti, Zr, Hf)C medium-entropy ceramic-based composite material uses a carbon fiber preform as a skeleton, the volume fraction of the carbon fiber preform is 45-55%, and a high-texture pyrolytic carbon interface phase is deposited on the surface of the carbon fiber preform; and uses (Ti, Zr, Hf)C medium-entropy ceramic as a matrix, and the oxygen content in the matrix is ​​not higher than 2%.

Citation Information

Patent Citations

  • Preparation method of silicon carbide and silicon carbide composite material member

    CN103387405A

  • Metal element containing polycarbosilane and preparation method and application thereof

    CN109485858A

  • Ceramic matrix composite material and preparation method thereof

    CN110028330A

  • Pyrolytic carbon interface phase, preparation method and application thereof, carbon fiber reinforced silicon carbide ceramic-based composite material and preparation method thereof

    CN114195537A

  • Carbon fiber toughened ceramic matrix composite material and preparation method thereof

    CN115745644A