A dendritic carbazole derivative and its preparation method and application

By designing dendritic carbazole derivatives to construct crosslinked conductive polymer films, the problem of insufficient conductivity and stability is solved, and the preparation of high-performance conductive polymers is realized, suitable for electronic devices and supercontainer materials.

CN116514702BActive Publication Date: 2024-11-15ZHEJIANG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310515007.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-15
Estimated Expiration
2043-05-09

AI Technical Summary

Technical Problem

The low conductivity and stability of existing conductive polymer materials limit their use in certain applications, and the molecular structure needs to be improved to improve conductivity and stability.

Method used

A dendritic carbazole derivative was designed to construct a cross-linked conductive polymer film through its non-coplanar structure, which increased the degree of polymerization and loose surface morphology, and the electrolyte ions were easily embedded and detached, improving electrochemical and thermodynamic stability. and high-performance conductive polymers are obtained by electrochemical polymerization preparation method.

Benefits of technology

High electrochemical and thermodynamic stability of conductive polymer films is achieved, enhanced electrochromic and energy storage properties, simplified the preparation process and improved yields, suitable for electronic devices and supercontainer materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116514702B_ABST
    Figure CN116514702B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of organic synthesis, and discloses a dendritic carbazole derivative and a preparation method and application thereof. The invention provides a dendritic carbazole derivative through structural design, which has abundant active sites, has a high degree of polymerization during the polymerization process, and constructs a conductive polymer film with a cross-linked structure, which has excellent electrochemical and thermodynamic stability. At the same time, the conductive polymer film has a loose surface morphology, and electrolyte ions are easy to embed and remove in the conductive polymer material, and the polymer film has good electrochromic properties and energy storage properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of organic synthesis, and in particular to a dendritic carbazole derivative and a preparation method and application thereof. Background Art

[0002] Carbazole and its derivatives are a well-known hole transport and light-emitting unit. Due to their excellent optoelectronic properties such as photoconductivity, electroluminescence, photochromism, and electrochromism, they have attracted great attention in the field of organic optoelectronic functional materials. Carbazole and its derivatives are commonly used conductive polymer matrix materials. Among them, carbazole structure is simple to synthesize, easy to modify, and the polymer has rich colors. In addition, it has good environmental stability and thermal stability during doping and dedoping, making it a research hotspot in conductive polymer material systems.

[0003] As one of the main electrode materials of electrochromic supercapacitors, high molecular conductive polymer materials stand out among many electrode materials due to their advantages such as high specific capacity, high conductivity, easy synthesis, rich colors and low cost during redox.

[0004] Compared with traditional metal conductors, conductive polymer materials have lower conductivity, which limits their use in some applications. At the same time, traditional conductive polymer materials have poor stability. The molecular structure of conductive polymer materials determines their conductive properties and stability. The molecular structure of current conductive polymer materials needs to be improved to improve their conductive properties and stability. Summary of the invention

[0005] In order to solve the technical problem of poor conductivity and stability of the above-mentioned conductive polymer materials, the present invention provides a dendritic carbazole derivative and a preparation method and application thereof. The dendritic carbazole derivative provided by the present invention has abundant active sites, has a high degree of polymerization during the polymerization process, and constructs a conductive polymer film with a cross-linked structure, which has excellent electrochemical and thermodynamic stability. At the same time, the conductive polymer film has a loose surface morphology, and electrolyte ions are easy to embed and remove in the conductive polymer material, and the polymer film has good electrochromic properties and energy storage properties.

[0006] The specific technical scheme of the present invention is:

[0007] In one aspect, the present invention provides a dendritic carbazole derivative having the chemical structural formula:

[0008]

[0009] Carbazole and its derivatives are commonly used hole transport and light-emitting units. The present invention provides a dendritic carbazole derivative through structural design. The dendritic carbazole derivative provided by the present invention has greater advantages in the application of electronic devices than the existing carbazole and its derivatives. First, the carbazole derivative has more abundant active sites. The conductive polymer film with a cross-linked structure is polymerized with the carbazole derivative as a monomer. During polymerization, it has six polymerizable active sites. Compared with the existing linear structure compounds, it is easier to prepare the corresponding cross-linked polymer film by electrochemical polymerization. It has a higher degree of polymerization and greatly improves the electrochemical and thermodynamic stability of the conductive polymer film. Another advantage is that the carbazole derivative provided by the present invention is a non-coplanar dendritic structure, which is conducive to breaking the planarity of the molecule. When preparing the conductive polymer film, the non-coplanarity of the molecule makes the connection between multiple monomers break the regularity of the polymer space structure after the molecule is polymerized to form a polymer, so that the obtained polymer film has a loose structure and a looser surface morphology. The electrolyte ions are easier to embed and remove in the conductive polymer material, thereby improving the electrochromic properties and energy storage properties of the polymer film.

[0010] At the same time, the present invention provides a method for preparing the above-mentioned dendritic carbazole derivatives, comprising the following steps (1) to (2):

[0011] (1) 9-phenylcarbazole reacts with N-bromosuccinimide to obtain an intermediate The chemical reaction equation is as follows:

[0012]

[0013] (2) The intermediate obtained in step (1) reacts with 4-(9-carbazolyl)phenylboronic acid to obtain the dendritic carbazole derivative. The chemical reaction equation is as follows:

[0014]

[0015] In the preparation of the above-mentioned dendritic carbazole derivatives, 9-phenylcarbazole is first reacted with N-bromosuccinimide to prepare the intermediate CB-3Br, and then CB-3Br is reacted with 4-(9-carbazolyl)phenylboronic acid to prepare the dendritic carbazole derivatives of the present invention.

[0016] As a preferred embodiment of the above technical solution of the present invention, in step (1), the reaction temperature is -5 to 10°C.

[0017] As a preferred embodiment of the above technical solution of the present invention, in step (2), the reaction is a Suzuki coupling reaction.

[0018] Specifically, the preparation method of the above-mentioned dendritic carbazole derivatives is preferably:

[0019] In step (1), 9-(4-bromophenyl)-carbazole and NBS are added to a single-mouth round-bottom flask in sequence, anhydrous N,N-dimethylformamide (20 mL) is added as a reaction solvent, stirred, and stirred in a 0°C ice-water mixed bath for 8 hours. After the reaction is completed, the reaction solution is purified to obtain the pure product CB-3Br. The purification method is as follows: the reaction solution is poured into 200 mL of deionized water, extracted with 400 mL of dichloromethane 5 times until the solvent N,N-dimethylformamide is extracted cleanly, the extract is concentrated and dried with anhydrous sodium sulfate to remove water, the sample is mixed with coarse silica gel, and then purified by column chromatography, with fine silica gel as the stationary phase, dichloromethane and petroleum ether as the mobile phase, the eluent containing the target compound is collected, the solvent is removed by rotary evaporation and dried.

[0020] Preferably, the molar ratio of 9-(4-bromophenyl)-carbazole to NBS is 1:3-6; the volume of anhydrous N,N-dimethylformamide added as solvent is 30-40 mL / g based on the mass of 9-(4-bromophenyl)-carbazole.

[0021] In step (2), under the protection of N2, the compound shown in formula (IV), tetrabutylammonium bromide, and 4-(9-carbazolyl)phenylboronic acid are dissolved in a mixed solvent of toluene and tetrahydrofuran, and tetrakis(triphenylphosphine)palladium is used as a catalyst, and the mixture is heated and refluxed for 18-24 hours. After the reaction is completed, the reaction solution is purified to obtain the target product 3CBCB shown in formula (I), that is, the dendritic carbazole derivative of the present invention. The purification method is: extract with dichloromethane three times, concentrate the extract, dry it with anhydrous sodium sulfate to remove water, mix the sample with coarse silica gel, and purify it by column chromatography, using fine silica gel as the stationary phase, dichloromethane and petroleum ether as the mobile phase (dichloromethane: petroleum ether = 1:5), collect the eluent containing the target compound, remove the solvent by rotary evaporation and dry it.

[0022] Preferably, the molar ratio of the intermediate compound represented by formula (IV) to 4-(9-carbazolyl)phenylboronic acid is 1:3 to 3.5; the volume ratio of the added solvent toluene and tetrahydrofuran is 1.5:1, and the total volume of the mixed solvent is 30 to 40 mL / g based on the mass of the intermediate compound represented by formula (IV).

[0023] The target product, the dendritic carbazole derivative, prepared by the preparation method provided by the present invention has good purity and high yield.

[0024] On the other hand, the present invention provides a carbazole conductive polymer using the above-mentioned dendritic carbazole derivative as a monomer, and the chemical structure is as follows:

[0025]

[0026] Wherein, n represents the average degree of polymerization, and n is 10-2000.

[0027] The dendritic carbazole derivatives provided by the present invention are easy to prepare electrochromic energy storage materials through electrochemical polymerization. Specifically, the dendritic carbazole derivatives and electrolytes are dissolved in a solvent, and electrochemical polymerization is performed to obtain a film, namely a carbazole conductive polymer. The research team of the present invention conducted ultraviolet-visible spectroscopy and electrochromic performance tests on the prepared compound film, and found that the polymer film is colorless and transparent in the neutral state, yellow in the semi-oxidized state, and green in the fully oxidized state, and has good electrochromic and energy storage properties.

[0028] The method used by the research team of the present invention to test the charge and discharge performance of the film is as follows: the electrolyte tetrabutylammonium hexafluorophosphate is dissolved in chromatographic grade dichloromethane and used as a blank supporting electrolyte solution. The blank electrolyte solution is used as the test solution, the polymer film is used as the working electrode, the platinum wire is used as the counter electrode, and Ag / AgCl is used as the reference electrode to form a three-electrode system to test the electrochromic properties and energy storage properties of the carbazole conductive polymer.

[0029] Specifically, the present invention provides a method for preparing the above-mentioned carbazole conductive polymer, comprising the following steps:

[0030] S1: dissolving the dendritic carbazole derivative according to claim 1 and a supporting electrolyte in a solvent;

[0031] S2: using a cyclic voltammetry electrochemical method to polymerize into a film to obtain the carbazole conductive polymer.

[0032] The present invention dissolves the above-mentioned dendritic carbazole derivatives and supporting electrolytes in a solvent, and then uses ITO glass (0.94 cm) as a working electrode, a platinum sheet as a counter electrode, and Ag / AgCl as a reference electrode to obtain a polymerized film p3CBCB, i.e., the above-mentioned carbazole conductive polymer, by cyclic voltammetry polymerization.

[0033] As a preferred embodiment of the above technical solution of the present invention, in step S1, the supporting electrolyte is selected from tetrabutylammonium hexafluorophosphate, tetrabutylammonium perchlorate, lithium tetrafluoroborate, and lithium perchlorate. Preferably, tetrabutylammonium hexafluorophosphate is selected. When tetrabutylammonium hexafluorophosphate is used as the supporting electrolyte, the preparation effect of the polymer is the best.

[0034] As a preferred embodiment of the above technical solution of the present invention, in step S1, the solvent is selected from dichloromethane, acetonitrile, propylene carbonate, preferably chromatographic grade. The preparation effect of the polymer is best when chromatographic grade dichloromethane is used as the solvent.

[0035] As a preferred embodiment of the above technical solution of the present invention, in step S2, the parameters of the cyclic voltammetry electrochemical method include: a voltage of 0 to 1.5 V, and a number of polymerization cycles of 15 to 20 cycles.

[0036] In the preparation process of the above-mentioned carbazole conductive polymer, specifically, after the cyclic voltammetry electrochemical polymerization film is formed, the polymer film is obtained by dedoping, washing and drying. Preferably, the dedoping conditions are voltage -0.8 to -0.5V, time 30 to 60s. The liquid system used for washing is a chromatographic grade mixed solution of dichloromethane: acetonitrile = 2:3.

[0037] Compared with the prior art, the present invention has the following technical effects:

[0038] (1) The present invention constructs a dendritic carbazole monomer through carbazole derivatives, which is a non-coplanar dendritic structure with large steric hindrance. At the same time, the dendritic non-planar structure can cause a certain structural distortion in the molecular structure of the polymerized film. Compared with the existing linear structure compounds or X-type and Y-type structure compounds, the structure of the polymer film after polymerization is looser, the electrolyte ions are easier to embed and release, and the material has excellent energy storage properties.

[0039] (2) The dendritic carbazole derivatives provided by the present invention have six polymerizable active sites during polymerization. Compared with existing linear structure compounds, they are easier to prepare corresponding polymer films through electrochemical polymerization and have a higher degree of polymerization, which greatly improves the electrochemical and thermodynamic stability of the conductive polymer film.

[0040] (3) The dendritic carbazole derivatives provided by the present invention have good reaction selectivity, a simple preparation process, few by-products, are easy to separate and have a high yield.

[0041] (4) The dendritic carbazole derivatives provided by the present invention can be used to prepare polymer films at a lower driving voltage through electrochemical polymerization.

[0042] (5) The polymer film prepared by the present invention can show a variety of color changes under different voltages, and has application value in the field of electrochromism; at the same time, it has excellent charge and discharge performance and has application value in the field of supercapacitance. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 is the cyclic voltammetric polymerization curve of the carbazole derivative 3CBCB in Example 7 of the present invention;

[0044] Figure 2 is the cyclic voltammetric polymerization curve of the carbazole derivative 3CBCB in Example 8 of the present invention;

[0045] Figure 3is the cyclic voltammetric polymerization curve of the carbazole derivative 3CBCB in Example 9 of the present invention;

[0046] Figure 4 is a UV-visible absorption spectrum of the polymer film obtained by testing in Example 10 of the present invention at different voltages;

[0047] Figure 5 This is an electrochromic optical contrast diagram obtained by testing Example 11 of the present invention;

[0048] Figure 6 This is a constant current charge and discharge curve diagram obtained by testing Example 12 of the present invention;

[0049] Figure 7 It is a comparison chart of charge and discharge performance test curves of the pCBCB film prepared in Comparative Example 1 of the present invention and the p3CBCB film prepared in Example 7. DETAILED DESCRIPTION

[0050] The present invention will be further described below in conjunction with embodiments and drawings.

[0051] Overall embodiment

[0052] 1. Preparation of CB-3Br:

[0053] The compound 9-phenylcarbazole represented by formula (II) and the compound N-bromosuccinimide (NBS) represented by formula (III) are subjected to bromination reaction to obtain the intermediate product represented by formula (IV). The chemical reaction schematic is shown below:

[0054]

[0055] 2. Preparation of 3CBCB:

[0056] The compound of formula (IV) prepared in 1. is subjected to Suzuki coupling reaction with 4-(9-carbazolyl)phenylboronic acid shown in formula (V) to obtain a dendritic carbazole derivative with a structure shown in formula (I). The chemical reaction schematic is shown below:

[0057]

[0058] 3. Preparation of polymer p3CBCB:

[0059] The dendritic carbazole derivatives described in the structural formula (I) are subjected to cyclic voltammetry electrochemical polymerization to obtain a conductive polymer as shown in the structure (VI). The chemical reaction schematic is shown below:

[0060]

[0061] Example 1 Preparation of CB-3Br

[0062] 9-(4-bromophenyl)-carbazole (500 mg, 1.55 mmol) and NBS (1.65 g, 9.30 mmol) were added to a single-mouth round-bottom flask in sequence, and anhydrous N,N-dimethylformamide (20 mL) was added as the reaction solvent. The mixture was stirred and stirred in a 0°C ice-water mixed bath for 8 hours. After the reaction was completed, the reaction solution was poured into 200 mL of deionized water and extracted with 400 mL of dichloromethane for 5 times until the solvent N,N-dimethylformamide was extracted completely. After the extract was concentrated, it was dried with anhydrous sodium sulfate to remove water. After mixing the sample with coarse silica gel, it was purified by column chromatography with fine silica gel as the stationary phase and dichloromethane and petroleum ether as the mobile phase. The eluent containing the target compound was collected, the solvent was removed by rotary evaporation and dried to obtain the pure product CB-3Br with a yield of 83%.

[0063] Example 2 Preparation of CB-3Br

[0064] 9-(4-bromophenyl)-carbazole (500 mg, 1.55 mmol) and NBS (1.65 g, 9.30 mmol) were added to a single-mouth round-bottom flask in sequence, and anhydrous N,N-dimethylformamide (20 mL) was added as the reaction solvent. The mixture was stirred and stirred in a -5°C ice-water mixed bath for 10 hours. After the reaction was completed, the reaction solution was poured into 200 mL of deionized water and extracted with 400 mL of dichloromethane for 5 times until the solvent N,N-dimethylformamide was extracted completely. After the extract was concentrated, it was dried with anhydrous sodium sulfate to remove water. After mixing the sample with coarse silica gel, it was purified by column chromatography with fine silica gel as the stationary phase and dichloromethane and petroleum ether as the mobile phase. The eluent containing the target compound was collected, the solvent was removed by rotary evaporation and dried to obtain the pure product CB-3Br with a yield of 82%.

[0065] Example 3 Preparation of CB-3Br

[0066] 9-(4-bromophenyl)-carbazole (500 mg, 1.55 mmol) and NBS (1.65 g, 9.30 mmol) were added to a single-mouth round-bottom flask in sequence, and anhydrous N,N-dimethylformamide (20 mL) was added as the reaction solvent. The mixture was stirred and stirred in a 10°C ice-water mixed bath for 8 hours. After the reaction was completed, the reaction solution was poured into 200 mL of deionized water and extracted with 400 mL of dichloromethane for 5 times until the solvent N,N-dimethylformamide was extracted completely. After the extract was concentrated, it was dried with anhydrous sodium sulfate to remove water. After mixing the sample with coarse silica gel, it was purified by column chromatography with fine silica gel as the stationary phase and dichloromethane and petroleum ether as the mobile phase. The eluent containing the target compound was collected, the solvent was removed by rotary evaporation and dried to obtain the pure product CB-3Br with a yield of 81%.

[0067] Example 4 Preparation of 3CBCB

[0068] CB-3Br (533 mg, 1.12 mmol), 4-(9-carbazolyl)phenylboronic acid (1.12 g, 3.92 mmol), tetrabutylammonium bromide (1% W), K2CO3 (3 qe) and tetrakis(triphenylphosphine)palladium (0.1% W) were added sequentially into a 100 mL two-necked round-bottom flask. Under N2 protection, toluene (15 mL) and tetrahydrofuran (10 mL) were added as reaction solvents. Then 3 ml of deionized water was added into the reaction flask, stirred, and heated under reflux at 90°C for 48 hours. After the reaction was completed, the mixture was extracted with dichloromethane three times. The extract was concentrated and dried over anhydrous sodium sulfate to remove water. The sample was mixed with coarse silica gel and purified by column chromatography using fine silica gel as the stationary phase and dichloromethane and petroleum ether as the mobile phases (dichloromethane: petroleum ether=1:5). The eluent containing the target compound was collected, the solvent was removed by rotary evaporation, and the product was dried to obtain the pure product 3CBCB with a yield of 82%.

[0069] Example 5 Preparation of 3CBCB

[0070] CB-3Br (533 mg, 1.12 mmol), 4-(9-carbazolyl)phenylboronic acid (1.06 g, 3.70 mmol), tetrabutylammonium bromide (1% W), K2CO3 (3 qe) and tetrakis(triphenylphosphine)palladium (0.1% W) were added into a 100 mL two-necked round-bottom flask in sequence. Under N2 protection, toluene (15 mL) and tetrahydrofuran (10 mL) were added as reaction solvents. Then 3 ml of deionized water was added into the reaction flask, stirred, and heated under reflux at 90°C for 48 hours. After the reaction was completed, it was extracted with dichloromethane three times. The extract was concentrated and dried over anhydrous sodium sulfate to remove water. The sample was mixed with coarse silica gel and purified by column chromatography using fine silica gel as the stationary phase and dichloromethane and petroleum ether as the mobile phases (dichloromethane: petroleum ether=1:5). The eluent containing the target compound was collected, the solvent was removed by rotary evaporation and dried to obtain the pure product 3CBCB with a yield of 70%.

[0071] Example 6 Preparation of 3CBCB

[0072] CB-3Br (533 mg, 1.12 mmol), 4-(9-carbazolyl)phenylboronic acid (964 mg, 3.36 mmol), tetrabutylammonium bromide (1% W), K2CO3 (3 qe) and tetrakis(triphenylphosphine)palladium (0.1% W) prepared in Example 1 were added. W) were added into a 100 mL two-necked round-bottom flask in sequence. Under N2 protection, toluene (15 mL) and tetrahydrofuran (10 mL) were added as reaction solvents. Then 3 ml of deionized water was added into the reaction flask, stirred, and heated under reflux at 90°C for 48 hours. After the reaction was completed, it was extracted with dichloromethane three times. The extract was concentrated and dried over anhydrous sodium sulfate to remove water. The sample was mixed with coarse silica gel and purified by column chromatography using fine silica gel as the stationary phase and dichloromethane and petroleum ether as the mobile phases (dichloromethane: petroleum ether=1:5). The eluent containing the target compound was collected, the solvent was removed by rotary evaporation and dried to obtain the pure product 3CBCB with a yield of 65%.

[0073] Example 7 Preparation of polymer p3CBCB

[0074] 10.93 mg (1 mmol / L) of the dendritic carbazole derivative 3CBCB monomer was added to a 10 mL volumetric flask, 0.387 g (0.1 mol / L) of tetrabutylammonium hexafluorophosphate was added as a supporting electrolyte, and the volume was fixed with chromatographic grade dichloromethane. Ultrasonication was performed for 3 min. After the solid was completely dissolved, cyclic voltammetry electrochemical polymerization was performed. The specific process was as follows: ITO glass (0.9×4 cm) was used as the working electrode, platinum wire was used as the counter electrode, and Ag / AgCl was used as the reference electrode. The polymerization voltage window was 0-1.5 V, and the number of polymerization cycles was 20 cycles. After the polymerization was completed, the polymer was dedoped in a blank electrolyte solution (0.1 mol / L tetrabutylammonium hexafluorophosphate / dichloromethane) for 60 s (voltage -0.5 V), and then the polymer film was washed with a chromatographic grade mixed solution of dichloromethane: acetonitrile = 2:3, and dried at 50°C for two hours.

[0075] The cyclic voltammetry polymerization curve of the preparation process is as follows Figure 1 As shown. Figure 1 It can be seen that with the increase in the number of polymerization cycles, the peak current intensity of the polymer gradually increases, indicating that the polymer is successfully deposited on the ITO conductive glass.

[0076] Example 8 Preparation of polymer p3CBCB

[0077] 10.93 mg (1 mmol / L) of the dendritic carbazole derivative 3CBCB monomer was added to a 10 mL volumetric flask, 0.387 g (0.1 mol / L) of tetrabutylammonium hexafluorophosphate was added as a supporting electrolyte, and the volume was fixed with chromatographic grade dichloromethane. Ultrasonication was performed for 3 min. After the solid was completely dissolved, cyclic voltammetry electrochemical polymerization was performed. The specific process was as follows: ITO glass (0.9×4 cm) was used as the working electrode, platinum wire was used as the counter electrode, and Ag / AgCl was used as the reference electrode. The polymerization voltage window was 0-1.5 V, and the number of polymerization cycles was 18 cycles. After the polymerization was completed, the polymer was dedoped in a blank electrolyte solution (0.1 mol / L tetrabutylammonium hexafluorophosphate / dichloromethane) for 60 s (voltage -0.5 V), and then the polymer film was washed with a chromatographic grade mixed solution of dichloromethane: acetonitrile = 2:3, and dried at 50°C for two hours.

[0078] The cyclic voltammetry polymerization curve of the preparation process is as follows Figure 2 As shown. Figure 2 It can be seen that with the increase in the number of polymerization cycles, the peak current intensity of the polymer gradually increases, indicating that the polymer is successfully deposited on the ITO conductive glass.

[0079] Example 9 Preparation of polymer p3CBCB

[0080] 10.93 mg (1 mmol / L) of the dendritic carbazole derivative 3CBCB monomer was added to a 10 mL volumetric flask, 0.387 g (0.1 mol / L) of tetrabutylammonium hexafluorophosphate was added as a supporting electrolyte, and the volume was fixed with chromatographic grade dichloromethane. Ultrasonication was performed for 3 min. After the solid was completely dissolved, cyclic voltammetry electrochemical polymerization was performed. The specific process was as follows: ITO glass (0.9×4 cm) was used as the working electrode, platinum wire was used as the counter electrode, and Ag / AgCl was used as the reference electrode. The polymerization voltage window was 0-1.5 V, and the number of polymerization cycles was 15 cycles. After the polymerization was completed, the polymer was dedoped in a blank electrolyte solution (0.1 mol / L tetrabutylammonium hexafluorophosphate / dichloromethane) for 60 s (voltage -0.5 V), and then the polymer film was washed with a chromatographic grade mixed solution of dichloromethane: acetonitrile = 2:3, and dried at 50°C for two hours.

[0081] The cyclic voltammetry polymerization curve of the preparation process is as follows Figure 3 As shown. Figure 3 It can be seen that with the increase in the number of polymerization cycles, the peak current intensity of the polymer gradually increases, indicating that the polymer is successfully deposited on the ITO conductive glass.

[0082] Example 10 UV-Visible Absorption Spectrum Test of Polymer p3CBCB Film

[0083] 0.387 g (0.1 mol / L) of tetrabutylammonium hexafluorophosphate was added to a 10 mL volumetric flask and fixed to volume with chromatographic grade dichloromethane to serve as a blank supporting electrolyte solution. The dendritic carbazole derivative 3CBCB polymer film prepared in Example 7 was used as a working electrode, Ag / AgCl as a reference electrode, and platinum wire as a counter electrode to test the UV-visible absorption spectrum of the polymer film at different voltages. The test results are shown in FIG. Figure 4 shown.

[0084] Depend on Figure 4 It can be seen from the UV-visible absorption spectrum that the polymer film is colorless and transparent in the neutral state, yellow in the semi-oxidized state, and green in the fully oxidized state, and has good electrochromic properties.

[0085] Example 11 Electrochromic performance test of polymer p3CBCB film

[0086] 0.387 g (0.1 mol / L) of tetrabutylammonium hexafluorophosphate was added to a 10 mL volumetric flask and fixed to volume with chromatographic grade dichloromethane to serve as a blank supporting electrolyte solution. The dendritic carbazole derivative 3CBCB polymer film prepared in Example 7 was used as a working electrode, Ag / AgCl as a reference electrode, and platinum wire as a counter electrode to test the optical contrast of the polymer film. The test results are shown in FIG. Figure 5 shown.

[0087] Depend on Figure 5 From the optical contrast diagram, it can be seen that the coloring time of the film at 425nm, 794nm and 1100nm are 2.39s, 2.66s and 1.50s respectively, and the fading time is 2.43s, 3.56s and 2.01s respectively. The optical contrast can reach 35.73%, 63.47% and 78.51% respectively, showing relatively good electrochromic performance.

[0088] Example 12 Test of the charge and discharge performance of the polymer p3CBCB film as a supercapacitor material The charge and discharge performance of the dendritic carbazole derivative 3CBCB polymer film prepared in Example 7 was tested using an electrochemical workstation. The specific test process is as follows:

[0089] 0.387g of tetrabutylammonium hexafluorophosphate was added to a 10mL volumetric flask and fixed to volume with chromatographic grade dichloromethane to serve as a blank supporting electrolyte solution. The blank electrolyte solution was used as the test solution, the prepared polymer film was used as the working electrode, the platinum wire was used as the counter electrode, and Ag / AgCl was used as the reference electrode to form a three-electrode system. The test voltage window was 0.4V to 1.4V, and the current density was 5mA / cm 3 , 10mA / cm 3 , 20mA / cm3 、30mA / cm 3 and 50mA / cm 3 The charge and discharge performance of the film was tested under constant current conditions. The test results are as follows Figure 6 shown.

[0090] Depend on Figure 6 It can be seen that the constant current charge and discharge curves of the polymer show obvious supercapacitive properties. 3 , 10A / cm 3 , 20A / cm 3 , 30A / cm 3 and 50A / cm 3 At a current density of 280.9 F / cm 3 , 277.8F / cm 3 , 244.7F / cm 3 , 211.7F / cm 3 , 179.6F / cm 3 and 143.9F / cm 3 , it can be seen that the polymer has a higher volumetric capacity and better charge and discharge rate performance.

[0091] Comparative Example 1

[0092] Compound To prepare a single polymer pCBCB film, the preparation method is the same as in Example 7.

[0093] The obtained pCBCB film and the p3CBCB film obtained in Example 7 were tested for charge and discharge performance. The test method was as follows: 0.387 g of tetrabutylammonium hexafluorophosphate was added to a 10 mL volumetric flask, and the volume was fixed with chromatographic grade dichloromethane, which was used as a blank supporting electrolyte solution. The blank electrolyte solution was used as the test solution, the pCBCB film or the p3CBCB film was used as the working electrode, the platinum wire was used as the counter electrode, and Ag / AgCl was used as the reference electrode to form a three-electrode system. The test voltage window was 0.8 V to 1.7 V, and the current density was 5 A / cm 3 The results are as follows Figure 7 shown.

[0094] Figure 7 The figure is a comparison of the charge and discharge performance test curves of the polymer films p3CBCB and pCBCB. Figure 7 It can be seen that at a current density of 5A / cm 3 When p3CBCB and pCBCB have a volume specific capacitance of 280.9 F / cm 3 and 266.2F / cm 3, p3CBCB shows a higher specific capacity than pCBCB. The conductive polymer prepared based on the dendritic carbazole derivatives provided by the present invention as monomer molecules has excellent energy storage properties, which is of great significance for the preparation of high-performance energy storage materials and their application in electronic device materials.

[0095] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0096] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A dendritic carbazole derivative, Features: The chemical structure is: 。 2. A method for preparing the dendritic carbazole derivatives as claimed in claim 1, Features: The following steps are involved: (1) 9-phenylcarbazole reacts with N-bromosuccinimide to obtain an intermediate; (2) reacting the intermediate obtained in step (1) with 4-(9-carbazolyl)phenylboronic acid to obtain the dendritic carbazole derivative; Wherein, the chemical structural formula of the intermediate is: .

3. The method for preparing the dendritic carbazole derivative according to claim 2, Features: In step (1), the reaction temperature is -5~10°C.

4. The method for preparing the dendritic carbazole derivative according to claim 2, Features: In step (2), the reaction is a Suzuki coupling reaction.

5. A carbazole conductive polymer using the dendritic carbazole derivative according to claim 1 or the dendritic carbazole derivative prepared by the preparation method according to any one of claims 2 to 4 as a monomer, Features: The average degree of polymerization is 10~2000.

6. A method for preparing the carbazole conductive polymer according to claim 5, Features: The following steps are involved: S1: dissolving the dendritic carbazole derivative according to claim 1 and a supporting electrolyte in a solvent; S2: using a cyclic voltammetry electrochemical method to polymerize into a film to obtain the carbazole conductive polymer; Wherein, in step S1, the supporting electrolyte is selected from tetrabutylammonium hexafluorophosphate, tetrabutylammonium perchlorate, lithium tetrafluoroborate, and lithium perchlorate; and the solvent is selected from dichloromethane, chromatographic grade acetonitrile, and propylene carbonate.

7. The method for preparing the carbazole conductive polymer according to claim 6, Features: In step S2, the parameters of the cyclic voltammetry electrochemical method include: voltage of 0-1.5 V, and number of polymerization cycles of 15-20 cycles.

8. Use of the carbazole conductive polymer according to claim 5 or the carbazole conductive polymer prepared by the preparation method according to any one of claims 6 to 7 in an electrochromic supercapacitor.