A Cr-Si coating on the surface of a nuclear zirconium alloy and a preparation method thereof

By doping Si atoms on the surface of the zirconium alloy, a Cr-Si coating is prepared to form a Cr2O3/SiO2 double oxide layer, which solves the problems of Cr coating failure and Zr and Cr diffusion in a high-temperature water vapor environment, and achieves high-temperature resistance Oxidation and improvement of mechanical properties.

CN116516291BActive Publication Date: 2024-10-08CHONGQING UNIV OF ARTS & SCI
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310520282.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-10-08
Estimated Expiration
2043-05-10

AI Technical Summary

Technical Problem

The Cr coating on the surface of the existing zirconium alloy fails in a high-temperature water vapor environment, and there is mutual diffusion between the Zr matrix and the Cr coating, causing the film-base interface to become unstable and reducing the protective performance.

Method used

Si atoms are doped into the Cr coating, and the Cr-Si coating is prepared through magnetron sputtering technology. The Si content is controlled between 7.5 and 22.0at.% to form a Cr2O3/SiO2 double oxide layer to prevent the mutual diffusion of Zr and Cr. , and improve the mechanical properties and wear resistance and friction reduction properties of the coating.

Benefits of technology

It effectively delays the failure of the Cr2O3 oxide layer and improves the high-temperature oxidation resistance and mechanical properties of the coating. The hardness reaches 14.64GPa, which enhances the wear resistance and friction reduction performance. The oxidation weight gain is as low as 1.4mg/cm2, and it is resistant to water at 1200℃. Stable in vapor environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116516291B_ABST
    Figure CN116516291B_ABST
Patent Text Reader

Abstract

A Cr-Si coating on the surface of a nuclear zirconium alloy is prepared by magnetron sputtering a Cr target and a Si target, and the Si content in the coating is controlled at 7.5-22.0 at.%, and the power drives of the Cr target and the Si target are respectively a DC power supply and a radio frequency power supply, wherein the sputtering power of the Cr target is 300W, and the power of the Si target is 100-300W. The Cr-Si coating prepared on the surface of the zirconium alloy substrate by the present invention has excellent high-temperature oxidation resistance. During the oxidation process, a Cr2O3 / SiO2 double oxide layer is formed at the interface between the substrate and the coating, which effectively delays the failure of Cr2O3. When oxidized in a 1200°C water vapor environment, the oxidation weight gain is as low as 1.4 mg / cm 2 At the same time, through the doping of Si, the mechanical properties of the coating are effectively improved, the hardness reaches 14.64GPa, and its wear resistance and friction reduction performance are enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alloy protective coating preparation, and in particular to a Cr-Si series coating on the surface of a nuclear zirconium alloy and a preparation method thereof. Background Art

[0002] Nuclear fuel cladding is the first safety barrier of nuclear power plants. Zirconium alloy has become the preferred material for nuclear fuel cladding due to its extremely low thermal neutron absorption cross section, good mechanical properties and corrosion resistance. However, in a loss of coolant accident (LOCA), zirconium alloy will react violently with high-temperature water vapor to form a zirconium-water reaction, leading to core meltdown and ultimately hydrogen explosion and nuclear leakage, posing a huge safety hazard. Therefore, the key to improving the safety of nuclear reactors is to slow down or prevent the zirconium-water reaction by developing accident-tolerant fuel (ATF).

[0003] Surface modification of zirconium alloy can not only effectively improve the high-temperature oxidation resistance of nuclear fuel cladding, but also retain the existing nuclear system and cladding tube production process, which is a relatively economical and efficient solution. The specific implementation method is to prepare a coating containing Si, Cr, and Al elements on the surface of the zirconium alloy, and to generate corresponding oxides in a high-temperature water vapor environment to hinder or slow down the diffusion of O into the matrix, so as to achieve the purpose of improving the oxidation resistance of the zirconium alloy cladding.

[0004] At present, the research on accident fault-tolerant coatings mainly revolves around ceramic coatings (MAX phase ceramic coatings, nitride coatings, carbide coatings, etc.) and metal coatings (FeCrAl coatings, Cr coatings, etc.). Among them, the metal Cr coating has a high thermal conductivity coefficient (94W / mK), excellent mechanical properties and corrosion resistance, good compatibility with the zirconium alloy cladding tube production process, and will generate Cr2O3 oxide film during use, which reduces the oxidation rate of zirconium alloy. It is considered to be the best choice for improving the accident fault tolerance of zirconium alloy cladding in the short term. However, the maximum tolerance temperature of Cr2O3 in a high-temperature water vapor environment is 1042℃. When the temperature is too high, Cr2O3 will form volatile CrO2(OH)2 or Cr(OH)3 and fail. In addition, the mutual diffusion between the Zr matrix and the Cr coating causes a eutectic reaction at the coating interface in an environment above 1330℃, resulting in instability of the film-base interface and reducing the protective performance of the Cr coating. Summary of the invention

[0005] The object of the present invention is to provide a Cr-Si coating on the surface of a zirconium alloy for nuclear use.

[0006] Another object of the present invention is to provide a method for preparing the Cr-Si coating on the surface of the above-mentioned nuclear zirconium alloy. By doping Si atoms in the Cr coating, the Cr-Si coating prepared can effectively delay the failure of the Cr2O3 oxide layer, effectively prevent the mutual diffusion of Zr and Cr at the interface, and effectively improve the mechanical properties and wear resistance and friction reduction properties of the coating.

[0007] The purpose of the present invention is achieved through the following technical solutions:

[0008] The present invention has the following technical effects:

[0009] A Cr-Si coating on the surface of a nuclear zirconium alloy, characterized in that: the Cr-Si coating is made by magnetron sputtering a Cr target and a Si target, the Si content in the coating is controlled at 7.5-22.0 at.%, the power drives of the Cr target and the Si target are a DC power supply and a radio frequency power supply respectively, wherein the sputtering power of the Cr target is 300 W, and the power of the Si target is 100-300 W.

[0010] Furthermore, during the magnetron sputtering process, the vacuum degree is 8×10 -4 Pa, the deposition temperature is 380~420℃, the substrate bias is -40~-60V, the deposition gas pressure is 0.3~0.5Pa, and the deposition time is 4~6h.

[0011] A method for preparing a Cr-Si coating on the surface of a nuclear zirconium alloy, characterized in that a Cr-Si coating with a Si content of 7.5 to 22.0 at.% is sputtered and deposited on the surface of a zirconium alloy substrate by magnetron sputtering using a Cr target and a Si target.

[0012] Furthermore, the power driving devices of the Cr target and the Si target are a DC power supply and a radio frequency power supply respectively, wherein the sputtering power of the Cr target is 300W, and the power of the Si target is 100-300W.

[0013] Furthermore, the vacuum degree of the magnetron sputtering is 8×10 -4 Pa, the deposition temperature is 380~420℃, the substrate bias is -40~-60V, the deposition gas pressure is 0.3~0.5Pa, and the deposition time is 4~6h.

[0014] Preferably, the deposition temperature is 400° C., the substrate bias voltage is −50 V, the deposition gas pressure is 0.4 Pa, and the deposition time is 5 h.

[0015] Most specifically, a method for preparing a Cr-Si coating on the surface of a nuclear zirconium alloy is characterized by the following steps:

[0016] ① Pretreatment of zirconium alloy substrate: The surface of the Zry-4 alloy substrate was polished with 100#, 400#, 1000#, and 2000# SiC sandpaper in sequence. The polished Zry-4 alloy substrate was polished with a diamond polishing liquid with a particle size of 1.5μm and a silica suspension with a particle size of 0.06μm in sequence, and then ultrasonically cleaned with acetone and anhydrous ethanol for 10 minutes and then dried for use;

[0017] ② Preparation of Cr-Si coating: The coating was prepared by magnetron sputtering. The Cr target and Si target were driven by a DC power supply and a radio frequency (RF) power supply, respectively. The vacuum was 8×10 -4 Pa, the deposition temperature is 380-420°C, the substrate bias is -40--60V, the deposition gas pressure is 0.3-0.5Pa, and the deposition time is 4-6h; among them, the sputtering power of the Cr target is fixed at 300W, the sputtering power of the Si target is 100-300W, and the Si content of the coating is controlled between 7.5 and 22.0at.%.

[0018] Beneficial effects:

[0019] The Cr-Si coating prepared on the surface of the zirconium alloy substrate has excellent high-temperature oxidation resistance. During the high-temperature steam oxidation process, a Cr2O3 / SiO2 double oxide layer is formed at the interface between the substrate and the coating, which effectively delays the failure of Cr2O3. When oxidized in a 1200°C water vapor environment, the oxidation weight gain is as low as 1.4 mg / cm 2 At the same time, through the doping of Si, the mechanical properties of the coating are effectively improved, the hardness reaches 14.64GPa, and its wear resistance and friction reduction performance are enhanced. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 : Surface morphology and element content analysis of the deposited CrSi-100W coating prepared by the present invention.

[0021] Figure 2 : Cross-sectional morphology of the deposited CrSi-100W coating prepared by the present invention.

[0022] Figure 3 : Surface morphology and element content analysis of the deposited CrSi-200W coating prepared by the present invention.

[0023] Figure 4 : Cross-sectional morphology of the deposited CrSi-200W coating prepared by the present invention.

[0024] Figure 5 : Surface morphology and element content analysis of the deposited CrSi-300W coating prepared by the present invention.

[0025] Figure 6 : Cross-sectional morphology of the deposited CrSi-300W coating prepared by the present invention.

[0026] Figure 7 : Comparison of high temperature oxidation weight gain of each coating.

[0027] Figure 8 : The structure of the double oxide layer generated after the coating is oxidized, including (a) cross-sectional view; (b) EDS surface scan; (c) local magnified image; (d) high-resolution image and SAED image of area (d); (e) high-resolution image and SAED image of area (e).

[0028] Fig. 9 : Cross-sectional morphology and element distribution of CrSi-300W coating after oxidation in water vapor at 1300℃ / 30min. DETAILED DESCRIPTION

[0029] The present invention is described in detail below through examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments to the present invention based on the above-mentioned contents of the present invention.

[0030] Example 1

[0031] A method for preparing a Cr-Si coating on the surface of a nuclear zirconium alloy is carried out according to the following steps:

[0032] ① Pretreatment of zirconium alloy substrate: The surface of the Zry-4 alloy substrate was polished with 100#, 400#, 1000#, and 2000# SiC sandpaper in sequence. The polished Zry-4 alloy substrate was polished with a diamond polishing liquid with a particle size of 1.5μm and a silica suspension with a particle size of 0.06μm in sequence, and then ultrasonically cleaned with acetone and anhydrous ethanol for 10 minutes and then dried for use;

[0033] ② Preparation of Cr-Si coating: The coating was prepared by magnetron sputtering. The Cr target and Si target were driven by a DC power supply and a radio frequency (RF) power supply, respectively. The vacuum was 8×10 -4 Pa, the deposition temperature is 400℃, the substrate bias is -50V, the deposition gas pressure is 0.4Pa, and the deposition time is 5h; among them, the sputtering power of the Cr target is fixed at 300W, the sputtering power of the Si target is 100W, and the Si content of the coating is 7.8at.%, recorded as CrSi-100W.

[0034] Figure 1The surface morphology and element content of the deposited CrSi-100W coating. It can be seen that the coating surface structure is dense without any cracks, holes and other defects. The Si content in the coating is 7.8at.%. Figure 2 This is the cross-sectional morphology of the CrSi-200W coating. The coating is well bonded to the Zry-4 alloy substrate, the coating structure is dense and uniform, and the thickness is 11.4μm.

[0035] Example 2

[0036] A method for preparing a Cr-Si coating on the surface of a nuclear zirconium alloy is carried out according to the following steps:

[0037] ① Pretreatment of zirconium alloy substrate: The surface of the Zry-4 alloy substrate was polished with 100#, 400#, 1000#, and 2000# SiC sandpaper in sequence. The polished Zry-4 alloy substrate was polished with a diamond polishing liquid with a particle size of 1.5μm and a silica suspension with a particle size of 0.06μm in sequence, and then ultrasonically cleaned with acetone and anhydrous ethanol for 10 minutes and then dried for use;

[0038] ② Preparation of Cr-Si coating: The coating was prepared by magnetron sputtering. The Cr target and Si target were driven by a DC power supply and a radio frequency (RF) power supply, respectively. The vacuum was 8×10 -4 Pa, the deposition temperature is 400℃, the substrate bias is -50V, the deposition gas pressure is 0.4Pa, and the deposition time is 5h; among them, the sputtering power of the Cr target is fixed at 300W, the sputtering power of the Si target is 200W, and the Si content of the coating is controlled at 14.3at.%, recorded as CrSi-200W.

[0039] Figure 3 The surface morphology and element content of the deposited CrSi-200W coating. It can be seen that the coating surface structure is dense without any cracks, holes and other defects. The Si content in the coating is 14.3at.%. Figure 4 This is the cross-sectional morphology of the CrSi-200W coating. It can be seen that the coating is well bonded to the Zry-4 alloy substrate, the coating structure is dense and uniform, and the thickness is 10.7μm.

[0040] Example 3

[0041] A method for preparing a Cr-Si coating on the surface of a nuclear zirconium alloy is carried out according to the following steps:

[0042] ① Pretreatment of zirconium alloy substrate: The surface of the Zry-4 alloy substrate was polished with 100#, 400#, 1000#, and 2000# SiC sandpaper in sequence. The polished Zry-4 alloy substrate was polished with a diamond polishing liquid with a particle size of 1.5μm and a silica suspension with a particle size of 0.06μm in sequence, and then ultrasonically cleaned with acetone and anhydrous ethanol for 10 minutes and then dried for use;

[0043] ② Preparation of Cr-Si coating: The coating was prepared by magnetron sputtering. The Cr target and Si target were driven by a DC power supply and a radio frequency (RF) power supply, respectively. The vacuum was 8×10 -4 Pa, the deposition temperature is 400°C, the substrate bias is -50V, the deposition gas pressure is 0.4Pa, and the deposition time is 5h; among them, the sputtering power of the Cr target is fixed at 300W, the sputtering power of the Si target is 300W, and the Si content of the coating is controlled at 21.7at.%, recorded as CrSi-300W.

[0044] Figure 5 The surface morphology and element content of the deposited CrSi-300W coating. It can be seen that the coating surface structure is dense without any cracks, holes and other defects. The Si content in the coating is 21.7at.%. Figure 6 This is the cross-sectional morphology of the CrSi-300W coating. It can be seen that the coating is well bonded to the Zry-4 alloy substrate, the coating structure is dense and uniform, and the thickness is 12.8μm.

[0045] Performance Testing:

[0046] (1) Mechanical properties

[0047] Generally speaking, the higher the hardness of the material, the better its wear resistance, which is beneficial to improving the tribological performance of the zirconium alloy cladding under normal working conditions. By doping Si atoms in the Cr coating, the hardness and elastic modulus of the coating are effectively improved. The hardness of the pure Cr coating on the surface of the zirconium alloy and the Cr-Si coating prepared in Examples 1-3 are tested, and the results are shown in Table 1.

[0048] Table 1: Microhardness of deposited coatings

[0049] coating Cr CrSi-100W CrSi-200W CrSi-300W Si content (at.%) 0 7.8 14.3 21.7 Hardness(GPa) 3.11 5.73 8.62 14.64

[0050] It can be seen from Table 1 that the Cr-Si coating improves the hardness of the pure Cr coating. At the same time, the hardness of the Cr-Si coating increases with the increase of Si content.

[0051] (2) High temperature antioxidant performance

[0052] The Zry-4 alloy substrate and the Cr-Si coatings with different Si doping amounts deposited on the surface of the Zry-4 alloy substrate by magnetron sputtering were tested for oxidation weight gain after being treated in a high-temperature water vapor environment at 1200°C for 30 minutes. The specific humidity was 90% at 50°C. The high-temperature oxidation resistance of each coating was tested. The results are as follows Figure 7 As shown in the figure, it can be seen that the weight gain of zirconium alloy without any coating protection after steam oxidation at 1200℃ for 30min reaches 29.9mg / cm 2 , while the oxidation weight gain of the Cr-Si coating (CrSi-100W) prepared in Example 1 is as low as 1.4 mg / cm 2 , and with the increase of Si content, the oxidation weight gain gradually increases, CrSi-200W and CrSi-300W are 2.2mg / cm 2 and 4.6 mg / cm 2 ,With the increase of subsequent oxidation time, the oxidation weight gain of each coating does not change significantly.

[0053] After oxidation test, the surface of CrSi-100W, CrSi-200W and CrSi-300W coatings all formed an oxide layer, specifically a Cr2O3 / SiO2 double oxide layer structure. The Cr2O3 / SiO2 double oxide layer delayed the failure of Cr2O3. The structural analysis of CrSi-200W after oxidation showed that, Figure 8 As shown, (a) is a cross-sectional view of the interface. It can be clearly seen that while Cr2O3 is oxidized, SiO2 is also generated, forming a Cr2O3 / SiO2 double oxide layer structure. (b) is the corresponding EDS surface scan. (c) is a local magnified image, (d) is a high-resolution image and SAED image of region (d) (Cr2O3), and (e) is a high-resolution image and SAED image of region (e) (SiO2). The elemental analysis corresponding to regions (d) and (e) is shown in Table 2.

[0054] Table 2: Element analysis corresponding to region (d) and region (e)

[0055] at.% O Si Cr Zr Area (d) 70.3 0.2 29.2 0.3 Area (e) 69.4 30.0 0.4 0.2

[0056] From the table above, we can see that the elements in area (d) are mainly O and Cr, while the elements in area (e) are mainly O and Si. Due to the limited accuracy of the test precision, the accuracy of the element analysis is limited. Figure 8Overall analysis shows that the main components of region (d) and region (d) are Cr2O3 and SiO2, and the trace Zr content proves that there is a slight diffusion, which is conducive to the improvement of the bonding strength between the coating and the substrate. The presence of amorphous SiO2 reduces the difference in thermal expansion coefficient between the CrSi residual layer and the Cr2O3 oxide layer, thereby reducing the generation of internal stress and enhancing the stability of the coating.

[0057] (3) Mutual diffusion performance of zirconium alloy and Cr-Si coating

[0058] After the CrSi-300W coating prepared in Example 3 was oxidized in water vapor at 1300°C / 30min (humidity 90% at 50°C), its cross-sectional morphology and element distribution were detected. Figure 5 As shown in Figure 3, a continuous Zr-Si interdiffusion layer (Diffusion layer) is formed in situ between the Cr-Si coating and the zirconium alloy interface after oxidation treatment, the surface of which is a CrSi residual layer (Residual layer), and the outermost surface is an oxide layer (Oxide layer). The thickness of each layer is shown in Table 3.

[0059] Table 3: Thickness of each layer after oxidation at 1300℃ / 30min (μm)

[0060] CrSi-100W CrSi-200W CrSi-300W Oxidelayer 1.45 3.13 3.7 Residuallayer 6.9 5.51 5.84 Cr-Si 5.6 5.8 8.3

[0061] At the same time, there is no Zr in the Cr-Si coating and no Cr in the zirconium alloy matrix, which shows that the continuous Zr-Si layer has a significant effect on hindering the mutual diffusion of Zr and Cr.

[0062] In summary, the Cr-Si coating prepared on the surface of the Zry-4 alloy substrate by the method of the present invention forms a four-layer structure during the oxidation process, which is, from the outside to the inside, a Cr2O3 oxide layer, a SiO2 oxide layer, a CrSi residual layer and a Zr-Si interdiffusion layer.

[0063] Example 4

[0064] A method for preparing a Cr-Si coating on the surface of a nuclear zirconium alloy is carried out according to the following steps:

[0065] ① Pretreatment of zirconium alloy substrate: The surface of the Zry-4 alloy substrate was polished with 100#, 400#, 1000#, and 2000# SiC sandpaper in sequence. The polished Zry-4 alloy substrate was polished with a diamond polishing liquid with a particle size of 1.5μm and a silica suspension with a particle size of 0.06μm in sequence, and then ultrasonically cleaned with acetone and anhydrous ethanol for 10 minutes and then dried for use;

[0066] ② Preparation of Cr-Si coating: The coating was prepared by magnetron sputtering. The Cr target and Si target were driven by a DC power supply and a radio frequency (RF) power supply, respectively. The vacuum was 8×10 -4 Pa, the deposition temperature is 380°C, the substrate bias is -60V, the deposition gas pressure is 0.5Pa, and the deposition time is 4h; among them, the sputtering power of the Cr target is fixed at 300W, the sputtering power of the Si target is 200W, and the Si content of the coating is 16at.%.

[0067] Example 5

[0068] A method for preparing a Cr-Si coating on the surface of a nuclear zirconium alloy is carried out according to the following steps:

[0069] ① Pretreatment of zirconium alloy substrate: The surface of the Zry-4 alloy substrate was polished with 100#, 400#, 1000#, and 2000# SiC sandpaper in sequence. The polished Zry-4 alloy substrate was polished with a diamond polishing liquid with a particle size of 1.5μm and a silica suspension with a particle size of 0.06μm in sequence, and then ultrasonically cleaned with acetone and anhydrous ethanol for 10 minutes and then dried for use;

[0070] ② Preparation of Cr-Si coating: The coating was prepared by magnetron sputtering. The Cr target and Si target were driven by a DC power supply and a radio frequency (RF) power supply, respectively. The vacuum was 8×10 -4 Pa, the deposition temperature is 420°C, the substrate bias is -40V, the deposition gas pressure is 0.3Pa, and the deposition time is 6h; among them, the sputtering power of the Cr target is fixed at 300W, the sputtering power of the Si target is 300W, and the Si content of the coating is 21.9at.%.

Claims

1. A method for preparing a Cr-Si coating on the surface of a nuclear zirconium alloy, characterized in that: By magnetron sputtering, a Cr-Si coating with a Si content of 7.5-22.0 at.% was sputtered and deposited on the surface of the zirconium alloy substrate using a Cr target and a Si target. The power drives of the Cr target and the Si target were a DC power supply and a radio frequency power supply, respectively. The sputtering power of the Cr target was 300 W, and the power of the Si target was 100-300 W. The vacuum degree of the magnetron sputtering was 8×10 -4 Pa, the deposition temperature is 380~420℃, the substrate bias is -40~-60V, the deposition gas pressure is 0.3~0.5Pa, and the deposition time is 4~6h.

2. A method for preparing a Cr-Si coating on the surface of a nuclear zirconium alloy, characterized in that: Proceed as follows: ① Pretreatment of zirconium alloy substrate: The surface of the Zry-4 alloy substrate was polished with 100#, 400#, 1000#, and 2000# SiC sandpaper in sequence. The polished Zry-4 alloy substrate was polished with a diamond polishing liquid with a particle size of 1.5 μm and a silica suspension with a particle size of 0.06 μm in sequence, and then ultrasonically cleaned with acetone and anhydrous ethanol for 10 minutes and then dried for use; ② Preparation of Cr-Si coating: The coating was prepared by magnetron sputtering. The Cr target and Si target were driven by direct current (DC) power supply and radio frequency (RF) power supply respectively. The vacuum degree was 8×10 -4 Pa, the deposition temperature is 380~420℃, the substrate bias is -40~-60V, the deposition gas pressure is 0.3~0.5Pa, and the deposition time is 4~6h; among them, the sputtering power of the Cr target is fixed at 300W, the sputtering power of the Si target is 100~300W, and the Si content of the coating is between 7.5~22.0 at.%.

Citation Information

Patent Citations

  • Protective coating with long-time high-temperature water vapor oxidation resistance and preparation method of protective coating

    CN112853287A

  • Plasma spray surface coating on Zirconium alloy for increasing the corrosion resistance at very high temperature