Method of making iron core
By using fiber laser to cut electromagnetic steel plates, combined with high-oxygen-concentration auxiliary gas and annealing treatment, the problems of burrs and steps during electromagnetic steel plate cutting were solved, achieving high-precision cutting surface processing and magnetic property recovery, thus improving the quality of the iron core.
Patent Information
- Application Number
- CN202180079107.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-11-15
- Filing Date
- 2021-11-17
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2041-11-17
AI Technical Summary
Existing technology makes it difficult to perform curved processing when cutting electromagnetic steel plates, resulting in burrs and steps, which leads to deterioration of magnetic properties and accumulation of varnish, affecting the quality and performance of the iron core.
Fiber laser is used to cut the electromagnetic steel plate, and a high oxygen concentration auxiliary gas is used for cutting. The magnetic properties are restored by annealing, and an oxide film is formed to prevent rust and avoid the accumulation of varnish.
It achieves high-precision cutting surface processing, suppresses the deterioration of magnetic properties and the accumulation of varnish, and improves the pass rate of electromagnetic steel plates and the appearance and dimensional quality of the iron core.
Smart Images

Figure CN116547102B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for manufacturing an electromagnetic steel sheet used in the core of a current transformer or a vehicle-mounted current sensor, and more specifically, to a method for cutting an electromagnetic steel sheet using a fiber laser, a method for manufacturing an electromagnetic steel sheet that minimizes the deterioration of magnetic properties and provides rust prevention, and a method for manufacturing a core from the cut electromagnetic steel sheet. Background Technology
[0002] The cores used in current transformers, current sensors, etc., are made by winding strips of electromagnetic steel sheets obtained from cutting electromagnetic steel sheets, or by stacking stamped electromagnetic steel sheets (hereinafter, "winding" and "stacking" are collectively referred to as "stacking"). The core assembly formed by stacking electromagnetic steel sheets is annealed, and varnish (adhesive impregnation) is impregnated to fix the electromagnetic steel sheets to each other.
[0003] To cut electromagnetic steel sheets into strips, a strip-cutting device is used. For example, in Patent Document 1, a pair of upper and lower rotating blades equipped with a strip-cutting device are used to cut long strips of electromagnetic steel sheets to obtain strip-shaped electromagnetic steel sheet parts.
[0004] However, cutting with a rotary cutter is difficult to perform on curved surfaces and complex outer shapes. Additionally, the rotary cutter wears out quickly. Furthermore, during cutting, the electromagnetic steel sheet sometimes recoils relative to the rotary cutter, making it particularly difficult to obtain narrow strips of electromagnetic steel sheet. Moreover, since the rotary cutter is only a few millimeters thick, it leads to a decrease in material yield during cutting.
[0005] Furthermore, the cutting using a rotating blade is performed with the upper and lower rotating blades staggered. Therefore, as... Figure 8 And then Figure 10 As shown, burrs 22 are generated at the cut surface 21 of the electromagnetic steel sheet 20, in the biting portion formed by the cutting blade, resulting in a deviation in the width after cutting. The result is as follows: Figure 9 As shown, in the core assembly 23a formed by stacking multiple electromagnetic steel plates 20 layers, a step of about ±0.1mm is generated on the side.
[0006] In the case of electromagnetic steel sheets obtained by stamping and blanking, burrs are generated at the biting part of the die in the blanked electromagnetic steel sheet, and the width after cutting is deviated. As a result, when the electromagnetic steel sheets are stacked, steps are generated on the side of the core assembly in the same way as described above.
[0007] If a step is formed on the side of the core assembly, it will be the cause of dimensional defects or poor performance of the core in the final product.
[0008] However, for the core assembly 23a formed by stacking electromagnetic steel sheets, after annealing for manufacturing the core 23, an impregnation treatment with varnish 25 is performed to prevent the electromagnetic steel sheets from peeling off. At this time, if varnish 25 remains on the side of the core 23, it will cause problems. Figure 10 As shown, a varnish accumulation zone 24 will form and solidify. Sometimes the varnish accumulation zone 24 has a diameter of more than 0.3 mm and a height of a few tenths of a mm, resulting in poor appearance and dimensional defects in the iron core 23 of the varnish accumulation zone 24.
[0009] The inventors noticed that cores made from electromagnetic steel sheets obtained by cutting with a rotary cutter or by stamping were prone to impregnation material accumulation. Further investigation revealed that this accumulation was caused by the following reasons.
[0010] The reason is the surface structure of the cut surface of the electromagnetic steel sheet 20. After being cut by a rotary cutter or punched, the cut surface 21 of the electromagnetic steel sheet 20 becomes a flat structure with few bumps. Because the flat cut surface with few bumps has high wettability, therefore... Figure 11 As schematically shown, the varnish 26 easily adheres to the cut surface 21. Furthermore, the adhered varnish 26 cures directly, thereby partially becoming... Figure 10 The varnish accumulation section 24 is shown.
[0011] It should be noted that the steps (layer offset) formed on the side of the core by the burrs 22 generated on the electromagnetic steel sheet 20 are also a reason for varnish accumulation. This is because varnish tends to accumulate on the steps.
[0012] Therefore, the inventors studied the adoption of a cutting method for electromagnetic steel plates that uses lasers instead of rotary blades and stamping.
[0013] For example, Patent Document 2 discloses a method for laser cutting of galvanized steel sheets. A YAG laser or a CO2 laser is used as the laser. The laser is irradiated onto the steel sheet while an auxiliary gas of 2-20% by volume oxygen and the remainder nitrogen is blown in.
[0014] Prior art literature
[0015] Patent documents
[0016] Patent Document 1: Japanese Patent Application Publication No. 5-299277
[0017] Patent Document 2: Japanese Patent Application Publication No. 2001-353588 Summary of the Invention
[0018] The problem that the invention aims to solve
[0019] However, when YAG lasers or CO2 lasers are used to cut electromagnetic steel sheets, excessive heat is applied to the cut surface during the cutting process. As a result, the temperature is heated to approximately 1500°C or higher from the cut end to a depth of about 1000 μm, causing changes in the crystal structure of the electromagnetic steel sheet, affecting its magnetic properties. Furthermore, with YAG and CO2 lasers, the use of oxygen as an assist gas results in black rust on the cut surface of the electromagnetic steel sheet. Even after annealing, the reduced magnetic properties caused by the aforementioned changes in the surface crystal structure and the black rust are difficult to recover. Therefore, electromagnetic steel sheets cut by YAG or CO2 lasers can be used for cores in motors and other applications where the width of the hysteresis curve (B-H curve) is less affected, but they cannot be used for cores in current transformers, current sensors, and other products where soft magnetic properties are required across the entire B-H curve, from the micromagnetization region to the saturation magnetization region, and are affected by coercive force or remanent flux density.
[0020] The purpose of this invention is to provide a method for cutting an electromagnetic steel plate using a fiber laser, a method for manufacturing an electromagnetic steel plate that minimizes the deterioration of magnetic properties and provides rust prevention, and a method for manufacturing an iron core from the cut electromagnetic steel plate that suppresses the formation of varnish accumulation.
[0021] Solution for solving the problem
[0022] The method for cutting electromagnetic steel plates of the present invention involves blowing an auxiliary gas with an oxygen concentration of 50% or more by volume onto the electromagnetic steel plate while irradiating it with a fiber laser, thereby obtaining an electromagnetic steel plate part that imparts a rust-proof effect to the cut surface.
[0023] Alternatively, the fiber laser can irradiate the electromagnetic steel plate with a core diameter of 1μm to 25μm, a laser output of 300W to 1000W, and a cutting speed of 300mm / second to 500mm / second.
[0024] Alternatively, the oxygen concentration may be 60% by volume or more, with the remainder being nitrogen.
[0025] The method for manufacturing electromagnetic steel sheet of the present invention involves annealing the electromagnetic steel sheet after it has been cut by the above-mentioned electromagnetic steel sheet cutting method to restore its magnetic properties.
[0026] Preferably, the annealing treatment is carried out at 750°C to 850°C for more than 1 hour.
[0027] In addition, the method for manufacturing the iron core of the present invention includes the step of winding or stacking the electromagnetic steel plate after it has been cut by the above-described electromagnetic steel plate cutting method to obtain an iron core assembly.
[0028] The steps of annealing the core assembly to restore the magnetic properties of the electromagnetic steel sheet; and
[0029] The step of immersing the core assembly in varnish.
[0030] Preferably, the annealing treatment is carried out at 750°C to 850°C for more than 1 hour.
[0031] Alternatively, the varnish may be a material comprising acrylic monomers and epoxy resin.
[0032] Invention Effects
[0033] According to the method for cutting electromagnetic steel sheets of the present invention, a fiber laser is used to irradiate the electromagnetic steel sheet while blowing an auxiliary gas with a high oxygen concentration, thereby cutting the electromagnetic steel sheet to obtain an electromagnetic steel sheet component. The fiber laser can concentrate energy over a narrow area, thus allowing the electromagnetic steel sheet to be cut without excessive heating. As a result, the resulting electromagnetic steel sheet exhibits minimal changes in the crystal structure of the cut surface, thereby minimizing the deterioration of its magnetic properties. Furthermore, by using an auxiliary gas with a high oxygen concentration, the cut surface undergoes rapid oxidation to form an oxide film. This oxide film has the effect of inhibiting the formation of red rust, therefore the resulting electromagnetic steel sheet component does not require rust-proofing treatment or packaging with rust-proof paper.
[0034] Electromagnetic steel sheets cut using fiber lasers have uniformly processed cut surfaces, unlike rotary cutters or punching cuts which produce burrs due to biting. Therefore, the cut surfaces of wound or stacked core assemblies are clean, suppressing the formation of side steps.
[0035] Annealing is performed on core assemblies that are wound or stacked. The region where crystal structure changes occur in the cut surface of the electromagnetic steel sheet is extremely shallow; therefore, annealing can restore the crystal structure of the cut surface layer, thereby restoring the magnetic properties.
[0036] After restoring the magnetic properties, the core assembly is immersed in varnish and then dried. Regarding the core assembly, the slight unevenness of the cut surface of the electromagnetic steel sheet reduces wettability due to the lotus leaf effect. Furthermore, by suppressing the formation of steps on the sides, varnish buildup is reduced. Therefore, appearance and dimensional defects in the resulting core can be reduced.
[0037] The iron core produced by this invention is suitable for use as a stamped iron core for current transformers and the like, as well as an iron core for vehicle-mounted current sensors and the like. Attached Figure Description
[0038] Figure 1The images show (a) and (b) magnified photographs of the cut surfaces of an electromagnetic steel sheet cut by the cutting method of the present invention.
[0039] Figure 2 This is an enlarged schematic diagram comparing the metal microstructure before and after annealing of the cut surfaces obtained by fiber laser cutting and rotary blade cutting.
[0040] Figure 3 This is a cross-sectional view of the core assembly of the present invention.
[0041] Figure 4 These are side views of the iron core assembly after annealing, obtained by cutting with (a) fiber laser and (b) and (c) using a rotary cutter.
[0042] Figure 5 This is a graph comparing the B-H curves of electromagnetic steel sheets before and after annealing, obtained by cutting with fiber laser and rotary cutter.
[0043] Figure 6 This is an enlarged photograph showing the state of the varnish accumulation section of the iron core of the present invention.
[0044] Figure 7 This is a cross-sectional view illustrating the mechanism by which the iron core of the present invention is difficult to accumulate varnish.
[0045] Figure 8 This is an enlarged photograph of the cut surface of the electromagnetic steel sheet after it has been cut by a rotary cutter.
[0046] Figure 9 It is a cross-sectional view of the core assembly formed by stacking electromagnetic steel sheets after they have been cut by a rotary cutter.
[0047] Figure 10 It is an enlarged photograph of the varnish accumulation area on the side of the iron core, which is formed by stacking electromagnetic steel sheets after being cut by a rotary cutter.
[0048] Figure 11 This is a cross-sectional view illustrating the mechanism by which varnish accumulates in the core formed by stacking electromagnetic steel sheets after being cut by a rotary cutter. Detailed Implementation
[0049] The following describes a method for cutting an electromagnetic steel plate and a method for manufacturing an iron core according to an embodiment of the present invention.
[0050] The cut electromagnetic steel sheet can be either directional or non-directional. The thickness of the electromagnetic steel sheet is preferably 0.2 mm to 0.5 mm. However, the thickness of the electromagnetic steel sheet is not limited to this.
[0051] In this invention, the fiber laser used for cutting the electromagnetic steel sheet is supplied to the laser unit via an optical fiber from a fiber laser processing machine and irradiated from the laser head of the laser unit. The laser unit has a built-in gas nozzle that blows auxiliary gas around the laser head. During the cutting of the electromagnetic steel sheet using the fiber laser, the gas nozzle blows high-pressure auxiliary gas supplied from a gas storage cylinder toward the cutting position.
[0052] Fiber lasers can be configured with a core diameter of 1μm to 25μm and a laser output of 300W to 1000W. Of course, these values are not limited to these limits.
[0053] For example, fiber lasers can irradiate electromagnetic steel plates with a spot diameter of 10μm to 100μm.
[0054] The auxiliary gas used is a gas with a high oxygen concentration. For example, the auxiliary gas can be a gas with an oxygen concentration of 50% by volume or more, preferably 60% by volume or more. The remainder can be substantially nitrogen. The use of a high oxygen concentration auxiliary gas is to properly oxidize the cut surface of the electromagnetic steel sheet. The flow rate of the auxiliary gas is preferably set to 30 liters / minute or more and 100 liters / minute or less. Of course, it is not limited to these values.
[0055] The feed speed of the electromagnetic steel sheet is preferably adjusted to a cutting speed of 300 mm / s to 500 mm / s. It should be noted that the feed speed can be adjusted appropriately based on the thickness of the electromagnetic steel sheet, the core diameter, and the laser output.
[0056] By irradiating an electromagnetic steel sheet with a fiber laser, the sheet is cut to obtain an electromagnetic steel sheet part. Using a fiber laser to cut the electromagnetic steel sheet also enables the machining of curves or complex outer shapes that cannot be achieved with a rotary cutter. Furthermore, in stamping and blanking, dies are required for each shape of the electromagnetic steel sheet part, while fiber laser cutting eliminates the need for dies.
[0057] In this invention, when cutting using a fiber laser, a high-oxygen auxiliary gas is blown towards the cutting position of the electromagnetic steel plate, causing the cut surface to combine with oxygen and oxidize rapidly. Furthermore, slag such as molten metal generated at the cut surface by the blowing of the auxiliary gas is blown away and purified.
[0058] The resulting electromagnetic steel sheet is cut using a fiber laser while being purged with a high-oxygen auxiliary gas, thus forming an oxide film on the cut surface as described above. This oxide film has the effect of suppressing the formation of red rust that affects magnetic properties, etc. For example, in electromagnetic steel sheets that have been cut with a cutting tool or punched, red rust will form on the cut surface if no oxide film is formed, so it is necessary to wrap them with rust-proof paper, etc. However, in this invention, since an oxide film is formed on the cut surface of the electromagnetic steel sheet, it is not necessary to use rust-proof paper for wrapping, etc.
[0059] By using a fiber laser for cutting, the cut surface of the electromagnet steel sheet instantly reaches a high temperature (above 1500°C), causing changes in the crystal structure of the cut surface. However, because fiber lasers can concentrate energy over a narrow area, the depth of the surface layer where the crystal structure changes is limited to approximately 10 μm to 50 μm. In the case of YAG lasers and CO2 lasers, the depth of the surface layer where the crystal structure changes is approximately 1000 μm or more. Therefore, it can be seen that with fiber lasers, the depth of the surface layer where the crystal structure changes can be limited to an extremely shallow range, minimizing the degradation of magnetic properties. Since the depth of the crystal structure change at the cut surface of the electromagnet steel sheet cut by a fiber laser is extremely shallow, the inventors discovered that by annealing the electromagnet steel sheet after cutting, both the crystal structure and magnetic properties can be restored. It should be noted that the annealing process will be described later.
[0060] Figure 1 These are photographs (a) and (b) enlarged images of the cut surface 11 of the electromagnetic steel sheet 10 cut by the aforementioned cutting method. (Refer to...) Figure 1 It can be seen that multiple tiny bumps and depressions are formed on the cut surface 11 obtained using a fiber laser. By using a fiber laser to cut the electromagnetic steel sheet, tiny bumps and depressions, nearly dome-shaped, are formed on the cut surface of the electromagnetic steel sheet with a spacing of tens of μm, a height of tens of μm, and a diameter of tens of μm. On the other hand, no slag residue remains on the cut surface. Slag residue occurs due to insufficient fiber laser output, slow cutting speed, etc. Furthermore, if referring to… Figure 1 In (a) and (b), the cut surface 11 is glossy, so it can be seen that a colorless oxide film (a few μm thick, as described later) is formed on the surface.
[0061] Figure 2 It is a schematic diagram showing the metal structure of the cut surface of an electromagnetic steel sheet before annealing. Figure 2 (a) is the cut surface of an electromagnetic steel sheet cut using a fiber laser. Figure 2 (c) is the cut surface of the electromagnetic steel sheet cut by a rotary cutter.
[0062] If reference Figure 2 From (a), it can be seen that the cut surface of the electromagnetic steel plate obtained using fiber laser technology undergoes deterioration in a very shallow region of the surface (denoted by the reference numeral α in the attached figure) due to the heat from the fiber laser, resulting in a change in the crystal structure. On the other hand, as... Figure 2 As shown in (c), no thermally induced alteration or crystal structure changes were observed in the cut surface formed using a rotating blade. However, in the cut surface formed using a fiber laser, changes in crystal structure were observed, as will be described later. Figure 5As shown by the solid line in (a), the magnetic properties of the electromagnetic steel sheet are reduced compared to those cut by a rotary cutter (represented by the dashed line), i.e., the remanent magnetic flux density is lower. However, as described later, this reduced magnetic property can be restored by annealing.
[0063] Figure 3 This is a cross-sectional view of a core assembly 13a formed by stacking multiple electromagnetic steel plates 10 cut into identical shapes using a fiber laser. As shown, the cut surfaces 11 of each electromagnetic steel plate 10 are slightly tilted due to the conical shape of the laser beam, but the sides of the stacked electromagnetic steel plates 10 are neat and there is no stacking misalignment. It should be noted that... Figure 3 The tilt of the cut surface 11 is exaggerated in the image, but the actual tilt is less than about 1°. By using a fiber laser for cutting, the electromagnetic steel sheet 10 can control the deviation of the shape of the cut surface 11 and the deviation of the width of the cut electromagnetic steel sheet 10 with high precision (less than ±0.05 mm).
[0064] After the electromagnetic steel sheet 10 is cut, as shown in Figure 3 After being stacked as shown to form the core assembly 13a, an annealing process is performed. The annealing conditions are 750°C to 850°C for at least 1 hour. Preferably, the conditions are 780°C to 820°C for at least 2 hours. The annealing atmosphere can be an inert gas atmosphere.
[0065] It can be seen that by annealing the electromagnetic steel sheet cut using fiber laser, Figure 2 The region α on the surface of the cut surface shown in (a) where the crystal structure changes is as follows: Figure 2 As shown in (b), the crystal structure is restored; furthermore, in its deeper layers, the tiny crystal structures are enlarged due to the annealing process. Thus, as will be described later... Figure 5 As shown in (b), the residual magnetic flux density also increases, and the magnetic properties can be recovered.
[0066] Figure 4 (a) is a side view of the core assembly 13a of the present invention after annealing, which is cut using a fiber laser. Figure 4 (b) and (c) are side views of the core assembly 23a, which was formed by stacking electromagnetic steel sheets after being cut by a rotary cutter, and which underwent the same annealing treatment for comparison. If the core assemblies 13a and 23a are annealed, a thin oxide film with a thickness of several hundred nm is formed on the side of the core assembly, regardless of the cutting method. However, as... Figure 4 As shown in (a), the core assembly 13a of the present invention, cut using a fiber laser, does not exhibit tempering color (light interference color) caused by the formation of a thin oxide film, even after annealing. On the other hand, in the core assembly 23a after being cut by a rotary cutter, as... Figure 4As shown in (b) and (c), tempering color appears.
[0067] The reason is that a colorless oxide film with a thickness of several μm is initially formed at the cutting surface 11 using a fiber laser. Because this colorless oxide film is formed first, even if a thin oxide film with a thickness of several hundred nm is formed on it through annealing, tempering color will not appear. On the other hand, at the cutting surface 21 of the electromagnetic steel sheet 20 cut by the rotary cutter, a colorless oxide film with a thickness of several μm is not formed due to cutting. Instead, a thin oxide film with a thickness of several hundred nm is directly formed on the cutting surface 21 through annealing, resulting in tempering color. The iron core 23 with tempering color generally becomes an appearance defect.
[0068] After annealing, the core assembly undergoes impregnation with varnish. Varnish is a penetrating adhesive, such as a liquid containing relatively low viscosity acrylic monomers and epoxy resin that easily penetrates between laminated electromagnet steel sheets.
[0069] The core assembly is manufactured by immersing it in varnish, which penetrates between the stacked (including wound) electromagnetic steel sheets. The curing of the varnish secures the sheets together. To facilitate varnish penetration, the core assembly is preferably preheated to approximately 80°C–90°C and then immersed in a liquid varnish at room temperature and pressure. During the cooling process of the preheated electromagnetic steel sheets, capillary action allows the varnish to effectively penetrate between them. After immersion, air is blown to allow any remaining varnish to drip off the sides, and the assembly is dried in a drying oven at approximately 110°C–150°C for 2–3 hours. (Refer to...) Figure 6 Therefore, it can be seen that the manufactured iron core 13 has almost no varnish accumulation area. Although a varnish accumulation area 14 is observed in some areas, it becomes a teardrop shape that is rounded off by the cut surface 11. The diameter of this varnish accumulation area 14 is about 0.05 mm, and the height is also very low, about 0.02 mm, which is less than 1 / 10 of the thickness of the electromagnetic steel plate. Therefore, there are no problems with its appearance and size in terms of practicality.
[0070] The reason why it is difficult to form a varnish accumulation area in the iron core of the present invention is as follows. At the cut surface 11 of the electromagnetic steel sheet 10 cut using a fiber laser, as described above, a plurality of near-dome-shaped micro-protrusions with a height of tens of μm and a diameter of tens of μm are formed at intervals of tens of μm on the cut surface of the electromagnetic steel sheet 10 (see reference). Figure 1 Furthermore, the core assembly is formed by stacking electromagnetic steel sheets having this cut surface. Because multiple tiny irregularities are formed on the cut surface 11, wettability is reduced due to the lotus leaf effect, thus preventing liquid varnish from adhering to the cut surface 11. Therefore, as... Figure 7As shown, varnish remains between the electromagnetic steel plates 10, 10 as indicated by reference numeral 15, but the varnish adhering to the cut surface 11 is repelled by the cut surface 11. Therefore, on the side of the core 13, as shown... Figure 6 That way, no varnish buildup will occur. For other reasons, such as... Figure 3 As shown, because the electromagnetic steel sheets 10 are cut with high dimensional accuracy, it is difficult to create steps on the sides of the core assembly 13a formed by stacking them. As a result, it is possible to reduce the amount of varnish accumulating on the sides of the core 13, thereby reducing the formation of varnish accumulation areas.
[0071] According to the present invention, by using a fiber laser to cut electromagnetic steel sheets, it is possible to achieve curved machining that cannot be achieved with a rotary cutter, and the yield rate of electromagnetic steel sheets can also be improved. By cutting the electromagnetic steel sheet while blowing a high-oxygen auxiliary gas, an oxide film is formed on the cut surface, preventing the formation of red rust. In addition, the cut surface of the electromagnetic steel sheet cut by the fiber laser can minimize the deterioration of magnetic properties, and its magnetic properties can be restored by annealing. Moreover, multiple tiny irregularities are formed on the cut surface of the electromagnetic steel sheet, thereby making it difficult for varnish to adhere to the cut surface due to the lotus leaf effect, reducing the varnish accumulation in the core. The core of the present invention has excellent magnetic properties and fewer appearance and dimensional defects, and is therefore suitable for various cores such as power transformers, choke coils, reactors, current transformers, and automotive current sensors.
[0072] It should be noted that, as described above, the present invention can suppress the formation of red rust on the cut surface of the electromagnetic steel sheet, thus enabling the electromagnetic steel sheet to be pre-cut and stored using the cutting method of the present invention. Furthermore, the electromagnetic steel sheet can be annealed or impregnated as needed for future use in iron cores, etc.
[0073] The above description is for illustrative purposes and should not be construed as limiting or restricting the scope of the invention described in the technical solution. Furthermore, the structure of each part of the invention is not limited to the above embodiments, and various modifications can be made within the scope of the technology described in the technical solution.
[0074] It should be noted that when cutting electromagnetic steel plates, straight sections can be cut with a cutting tool, curved sections can be cut with a fiber laser, and electromagnetic steel plates can be cut in combination with other cutting methods.
[0075] Example
[0076] <Example 1>
[0077] The electromagnetic steel plate was cut using a fiber laser and a rotating blade. The cut surfaces before and after annealing were observed, and the B-H curve was measured.
[0078] The electromagnetic steel sheet is a directional electromagnetic steel sheet with a thickness of 0.23 mm. It is cut using a fiber laser under the following conditions: fiber core diameter of 14 μm, laser output of 400 W, cutting speed of 500 mm / s, oxygen concentration of 100 vol% in the auxiliary gas, and flow rate of 30 L / min (Invention Example). For comparison, a directional electromagnetic steel sheet of the same thickness is cut using a rotary cutter (Comparative Example).
[0079] exist Figure 2 of (a) Figure 2 (c) shows schematic diagrams of the metal microstructure before annealing of the cut surface (laser cutting) of the invention example and the cut surface (tool cutting) of the comparative example, respectively. Figure 2 As shown in (a), in the region indicated by reference numeral α in the figure, the cut surface of the invention is altered due to the heat from the fiber laser, resulting in a change in the crystal structure. On the other hand, as... Figure 2 As shown in (c), no alteration or crystal structure change was observed on the cut surface. For these electromagnetic steel sheets before annealing, the B-H curves were measured, as shown... Figure 5 As shown in (a), it can be seen that the saturation magnetic flux density of the inventive example (solid line) is lower and the magnetic properties are reduced compared to the comparative example (dashed line). In addition, the iron losses of the two are 2.90 W / kg and 3.00 W / kg, respectively, and the average grain size of the crystal structure is 100 μm.
[0080] Next, the electromagnetic steel sheets of the inventive example and the comparative example were subjected to annealing treatment at 800°C for 2 hours, respectively. As a result, the inventive example... Figure 2 As shown in (b), Figure 2 Region α of (a) disappears. Additionally, as... Figure 2 (b) and the comparative example Figure 2 As shown in (d), the average grain size of the crystals in the Invention Example and the Comparative Example is enlarged to 150 μm to 200 μm. The iron loss of the two is 2.37 W / kg and 2.17 W / kg, respectively, which is an improvement compared with that before annealing treatment.
[0081] In addition, the B-H curves of the inventive examples and comparative examples after annealing were measured, such as... Figure 5 As shown in (b), it can be seen that the saturation magnetic flux density of the inventive example (solid line) is approximately the same as that of the comparative example (dashed line), and the magnetic properties can be restored to the same level as those of the comparative example through annealing.
[0082] In other words, the present invention achieves cutting of the electromagnet steel sheet by simultaneously blowing a high-oxygen-concentration auxiliary gas onto the sheet and irradiating it with a fiber laser, followed by annealing. This results in magnetic properties equivalent to those obtained using a rotary cutter. Furthermore, fiber lasers facilitate both straight-line and curved cutting, allowing for the production of cores with circular cross-sections even when wound. Additionally, since the laser unit does not experience wear and tear like a rotary cutter, cutting defects caused by blade shrinkage are prevented, reducing the time required for blade tip maintenance by experienced workers. Moreover, fiber lasers do not cause the electromagnet steel sheet to recoil as with rotary cutters, thus improving the yield rate.
[0083] <Example 2>
[0084] The electromagnetic steel plate was cut by changing the irradiation conditions of the fiber laser and the oxygen concentration of the auxiliary gas, and the presence of red rust was observed in a high temperature and high humidity atmosphere.
[0085] The electromagnetic steel sheet is a directional electromagnetic steel sheet with a thickness of 0.23 mm. It was cut using a fiber laser under eight conditions (all with a flow rate of 30 L / min): a fiber core diameter of 14 μm, a laser output of 400 W, a cutting speed of 300 mm / s and 500 mm / s, and an oxygen concentration of 40 vol% (reference example), 50 vol%, 70 vol%, and 100 vol% (all invention examples) for the auxiliary gas. For comparison, directional electromagnetic steel sheets of the same thickness were cut using a rotating blade (comparative example). After cutting, all samples were annealed at 800°C for 2 hours.
[0086] Each sample was placed in a high-temperature and high-humidity environment of 85°C and 85% humidity, and the number of days until red rust was observed on the cut surface was measured. The results are shown in Table 1.
[0087] [Table 1]
[0088]
[0089] Referring to Table 1, in all the invention examples where fiber laser cutting was performed under an assist gas atmosphere with an oxygen concentration of 50% by volume or higher, no red rust was observed on the cut surface for a period of 3 weeks or more. More specifically, in the invention examples where cutting was performed under an assist gas atmosphere with an oxygen concentration of 70% by volume or higher, no red rust was observed for a period of 4 weeks. On the other hand, in the invention examples where the oxygen concentration of the assist gas was 40% by volume and the comparative examples where cutting was performed with a cutting tool, red rust appeared on the cut surface after 1 day.
[0090] As described above, by performing fiber laser cutting in an auxiliary gas atmosphere with an oxygen concentration of 50% by volume or higher, an oxide film is formed on the cut surface of the electromagnetic steel sheet, which inhibits the formation of red rust. These inventions are unlikely to produce red rust even when placed in an oxidizing atmosphere for extended periods, thus eliminating the need for rust-proofing treatments or packaging with rust-proof paper. This is particularly effective for large components stored in a ring-like manner. It should be noted that an auxiliary gas with an oxygen concentration of 60% by volume or higher is preferred for reliably forming the oxide film.
[0091] <Example 3>
[0092] A current transformer was fabricated using an E-type iron core made by cutting the entire circumference with a fiber laser and an E-type iron core of the same shape made by punching with a stamping press. The output voltage characteristics before and after annealing were measured.
[0093] The electromagnetic steel sheet is a 0.35mm thick non-directional electromagnetic steel sheet. An E-type core (laser-cut core) was fabricated by cutting it using a fiber laser under conditions of a 14μm core diameter, 300W laser output, a cutting speed of 300mm / s, an oxygen concentration of 100% by volume in the assist gas, and a flow rate of 30 liters / minute. For comparison, a non-directional electromagnetic steel sheet of the same thickness was cut using a stamping machine to produce an E-type core of the same shape (comparative example: stamped core).
[0094] Using cores assembled from E-type cores produced in the above manner, current transformers with a turns ratio of 1:3000 (before annealing in Table 2) were fabricated, and their output voltage characteristics were measured. Furthermore, after annealing the E-type cores of both the Invention Example and the Comparative Example at 800°C for 2 hours, current transformers were fabricated again (after annealing in Table 2), and their output voltage characteristics were measured. The results are shown in Table 2.
[0095] [Table 2]
[0096]
[0097] Referring to Table 2, the properties of the inventive example before annealing were reduced by 3.2% compared to the comparative example, but after annealing, the reduction was improved to 0.3%. The difference after annealing is sufficiently practical. In practical applications, when an E-type core is manufactured by laser cutting and punching only in the processing of electromagnetic steel sheets, the area affected by the heat generated by laser cutting is only one side of the back of the E-type core, thus further improving the poor properties.
[0098] Explanation of reference numerals in the attached figures
[0099] 10 Electromagnetic steel sheet
[0100] 11. Cross-section
[0101] 13 Iron Heart
[0102] 13a Iron Core Assembly
[0103] 14 Varnish Storage Department
[0104] 15. Varnish.
Claims
1. A method for manufacturing an iron core, comprising the following steps: A fiber laser is irradiated while an auxiliary gas with an oxygen concentration of more than 50% by volume is blown onto an electromagnetic steel plate with a thickness of 0.2 to 0.5 mm. The electromagnetic steel plate is cut by the fiber laser, thereby obtaining an electromagnetic steel plate part with rust-proof effect on the cut surface; The electromagnetic steel sheets are wound or stacked to obtain an iron core assembly; Annealing is performed on the core assembly to restore the magnetic properties deteriorated by the irradiation with the fiber laser; and By immersing the core assembly in varnish and fixing the electromagnetic steel sheets together, a core with reduced varnish buildup between the electromagnetic steel sheets is produced.
2. The method for manufacturing an iron core according to claim 1, wherein, When manufacturing the iron core, the maximum diameter of the varnish accumulation portion formed on the cut surface is suppressed to less than 0.05 mm.
3. The method for manufacturing an iron core according to claim 1 or 2, wherein, The fiber laser irradiates the electromagnetic steel plate with a core diameter of 1μm to 25μm, a laser output of 300W to 1000W, and a cutting speed of 300mm / second to 500mm / second.
4. The method for manufacturing an iron core according to claim 1 or 2, wherein, The oxygen concentration is above 60% by volume, with the remainder being nitrogen.
5. The method for manufacturing an iron core according to claim 1 or 2, wherein, The annealing process is carried out at 750℃~850℃ for more than 1 hour.
6. The method for manufacturing an iron core according to claim 1 or 2, wherein, The varnish is a material containing acrylic monomers and epoxy resin.
Citation Information
Patent Citations
Winding iron core band cutting device
JP1993299277A
Laser beam cutting of galvanized sheet using nitrogen / oxygen mixture as assist gas
JP2001353588A
LASER BEAM CUTTING METHOD OF Zn-BASED PLATED STEEL SHEET
JP2014237141A
Solenoid core manufacturing method
WO2010076877A1
Electromagnetic field shielding plate, method for manufacturing same, electromagnetic field shielding structure, and semiconductor manufacturing environment
WO2020148796A1