A method for preparing a hydrophilic ultra-thin hydrogel modified film

The ultra-thin hydrogel modification layer is constructed through interface-initiated free radical polymerization, which solves the problems of membrane fouling and high requirements on the base membrane during the modification process, and achieves membrane modification with low material requirements and no structural damage, and The ultra-thin gel layer significantly improves anti-pollution performance and water passing ability.

CN116550158BActive Publication Date: 2024-10-18HARBIN INST OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310556388.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-10-18
Estimated Expiration
2043-05-17

AI Technical Summary

Technical Problem

In existing membrane separation technology, serious membrane fouling leads to increased mass transfer resistance and weakened water passing capacity. Moreover, existing membrane modification methods have high requirements on base membrane materials and may damage the base membrane structure and affect permeability.

Method used

An ultra-thin hydrogel modified layer is constructed on the membrane surface through interface-initiated free radical polymerization. The polymer monomer and cross-linking agent are stirred in deionized water to form an aqueous polymerization liquid, and mixed with a photoinitiator in an organic solvent. Mixed, UV light initiates polymerization to form an ultrathin hydrogel modified film.

Benefits of technology

It achieves low requirements on the material of the base membrane, no structural damage during the modification process, and the formed hydrogel layer is defect-free. The ultra-thin gel layer alleviates the reduction in water passing capacity, and has good anti-pollution performance, and the flux is maintained after pollution. 97%~100%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116550158B_ABST
    Figure CN116550158B_ABST
Patent Text Reader

Abstract

A method for preparing a hydrophilic ultra-thin hydrogel modified membrane, which relates to a method for preparing a hydrophilic modified membrane. The purpose of the present invention is to construct an ultra-thin hydrogel modified layer on the membrane surface through an interface-initiated free radical polymerization reaction, so as to solve the problems of serious membrane pollution, high requirements for membrane materials during membrane modification, and serious reduction in the water-passing capacity of the membrane. Method: 1. Prepare a polymer liquid; 2. Prepare a hydrogel modified membrane; 3. Clean the hydrogel modified membrane. The present invention has low requirements for the material of the base membrane when preparing the membrane, and has a wide range of applicable membrane hydrophilic modification; the present invention does not damage the structure of the base membrane during the preparation of the membrane, and the formed hydrogel layer does not have defects; the gel layer thickness of the hydrogel modified membrane prepared by the present invention is nanometer-level, and the ultra-thin gel layer alleviates the reduction of the membrane's water-passing capacity due to the modification; the present invention has a simple process, is easy to operate, has a short process cycle, and has low requirements for the operating environment. The present invention can obtain a hydrophilic ultra-thin hydrogel modified membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a hydrophilic modified membrane. Background Art

[0002] In the field of water treatment, membrane separation technology is a new type of water treatment technology. Due to its simple process equipment, strong adaptability to water source conditions, good selectivity during the treatment process, no phase change and energy saving, and no secondary pollution after the treatment, membrane separation technology is regarded as an ideal choice to replace traditional water treatment processes. During the operation of the membrane separation system, pollutants are attached to the membrane surface or inside the membrane pores through adsorption or deposition, causing membrane fouling problems. The accumulation of pollutants causes the formation of a fouling layer, and the increase in the mass transfer resistance of the membrane weakens the membrane's water-passing capacity, thereby reducing the membrane's water production efficiency; at the same time, the damage of the membrane structure by fouling shortens the service life of the membrane, greatly hindering the application of membrane separation technology. Therefore, the control of membrane fouling is particularly critical to the application and promotion of separation membranes.

[0003] The hydrophilic modification of the membrane is considered to be an effective means to improve the anti-fouling performance of the membrane; hydrogel is formed by cross-linking of hydrophilic polymer chains in water, can absorb a large amount of water, has strong hydrophilicity, and is an ideal material for hydrophilic modification of the membrane surface. The hydrophilic modification of the membrane surface is usually achieved by surface coating and surface grafting. Surface grafting produces specific grafting sites on the membrane surface through pretreatment, and then chemically bonds the hydrogel to the grafting sites through chemical reactions to form a hydrogel layer on the membrane surface. This method has little effect on the membrane permeability and its binding is relatively strong, but it requires the base membrane to have grafting sites or can produce grafting sites. The formed hydrogel layer may have defects and may damage the base membrane structure. Surface coating usually applies the hydrogel prepolymer solution to the membrane surface, and then cross-links the prepolymer solution through physical, chemical and other methods to form a hydrogel layer. The gel-modified membrane prepared by this method is uniform and flat, and the gel layer structure can be regulated by the prepolymer solution components, but the coated gel layer increases the membrane filtration resistance and significantly reduces the membrane permeability. Summary of the invention

[0004] The purpose of the present invention is to construct an ultra-thin hydrogel modified layer on the membrane surface through an interface-initiated free radical polymerization reaction, thereby solving the problems of serious membrane pollution, high requirements for membrane materials during membrane modification, and serious reduction in the water-passing capacity of the membrane, and providing a method for preparing a hydrophilic ultra-thin hydrogel modified membrane.

[0005] A method for preparing a hydrophilic ultrathin hydrogel modified film is specifically completed by the following steps:

[0006] 1. Prepare polymer liquid:

[0007] ①, add polymer monomer and cross-linking agent into deionized water, stir magnetically to obtain aqueous polymer solution;

[0008] The polymer monomer described in step 1① is an organic substance with an ionic group and a carbon-carbon double bond;

[0009] The cross-linking agent described in step 1① is an organic substance with two carbon-carbon double bonds;

[0010] The mass fraction of water in the aqueous phase polymerization liquid described in step 1① is 80% to 99%;

[0011] ②, adding a photoinitiator to an organic solvent and stirring to obtain an organic phase polymerization liquid;

[0012] The concentration of the photoinitiator in the organic phase polymerization solution described in step 1② is 0.01 g / mL;

[0013] 2. Preparation of hydrogel modified membrane:

[0014] The membrane is cleaned and fixed on a glass plate, and then deionized water is poured on the membrane surface, and after the membrane is wetted, the water on the surface is poured off and the membrane surface is blown dry; an aqueous phase polymer solution is poured on the membrane surface, and after the membrane is wetted, the surface aqueous phase polymer solution is poured off and residual droplets on the surface are removed; then an organic phase polymer solution is poured on the membrane surface and placed under an ultraviolet lamp for reaction to obtain an ultrathin hydrogel modified membrane;

[0015] 3. Cleaning the hydrogel modified membrane:

[0016] The ultra-thin hydrogel modified membrane is washed with deionized water for 3 to 5 times, and then stored in deionized water to obtain a hydrophilic ultra-thin hydrogel modified membrane.

[0017] Advantages of the present invention:

[0018] 1. The present invention has low requirements on the material of the base film when preparing the film, and has a wide range of applicable membrane hydrophilic modification;

[0019] Second, the structure of the base film is not damaged during the process of preparing the film of the present invention, and the formed hydrogel layer has no defects;

[0020] 3. The gel layer thickness of the hydrogel modified membrane prepared by the present invention is nanometer-level, and the ultra-thin gel layer alleviates the reduction of the membrane's water permeability caused by the modification;

[0021] Fourth, the process equipment for preparing the modified membrane of the present invention is simple, the operation is simple, the process cycle is short, and the requirements for the operating environment are low;

[0022] 5. The hydrogel modified membrane prepared by the present invention has good anti-pollution performance. In the pollution experiment, the presence of the ultra-thin hydrogel layer enables the membrane to maintain 97% to 100% of its initial flux after being polluted. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The scanning electron microscope cross-sectional images of the hydrophilic ultrathin hydrogel modified membranes prepared in Examples 1, 2 and 3;

[0024] Figure 2 The XPS full spectrum of the hydrophilic ultra-thin hydrogel modified membrane prepared in Examples 1, 2, and 3;

[0025] Figure 3 This is a graph showing the changing trend of membrane specific flux during the fouling-cleaning cycle test. DETAILED DESCRIPTION

[0026] Specific implementation method 1: This implementation method is a method for preparing a hydrophilic ultra-thin hydrogel modified film, which is specifically completed according to the following steps:

[0027] 1. Prepare polymer liquid:

[0028] ①, add polymer monomer and cross-linking agent into deionized water, stir magnetically to obtain aqueous polymer solution;

[0029] The polymer monomer described in step 1① is an organic substance with an ionic group and a carbon-carbon double bond;

[0030] The cross-linking agent described in step 1① is an organic substance with two carbon-carbon double bonds;

[0031] The mass fraction of water in the aqueous phase polymerization liquid described in step 1① is 80% to 99%;

[0032] ②, adding a photoinitiator to an organic solvent and stirring to obtain an organic phase polymerization liquid;

[0033] The concentration of the photoinitiator in the organic phase polymerization solution described in step 1② is 0.01 g / mL;

[0034] 2. Preparation of hydrogel modified membrane:

[0035] The membrane is cleaned and fixed on a glass plate, and then deionized water is poured on the membrane surface, and after the membrane is wetted, the water on the surface is poured off and the membrane surface is blown dry; an aqueous phase polymer solution is poured on the membrane surface, and after the membrane is wetted, the surface aqueous phase polymer solution is poured off and residual droplets on the surface are removed; then an organic phase polymer solution is poured on the membrane surface and placed under an ultraviolet lamp for reaction to obtain an ultrathin hydrogel modified membrane;

[0036] 3. Cleaning the hydrogel modified membrane:

[0037] The ultra-thin hydrogel modified membrane is washed with deionized water for 3 to 5 times, and then stored in deionized water to obtain a hydrophilic ultra-thin hydrogel modified membrane.

[0038] The fixing in step 2 of this embodiment is as follows: the membrane is clamped on the glass plate along the four sides by a 1 cm thick hollow polytetrafluoroethylene plate through a binder clip, and a hollow rubber pad is added between the membrane and the plate to prevent the polymer solution from leaking; the middle hollow area is the membrane modification area, and the thickness of the plate can be used to accommodate the aqueous phase polymer solution and the organic phase polymer solution;

[0039] The step 2 of this embodiment of blowing the membrane surface dry is: using an air gun to spray nitrogen to blow dry the water on the membrane surface, leaving only a portion of deionized water inside the membrane pores to prevent the aqueous polymer solution from penetrating deeply into the membrane pores.

[0040] The removal of residual droplets on the surface in step 2 of this embodiment is: using an air gun to spray nitrogen to gently blow off the residual droplets on the surface, leaving only the ultra-thin liquid layer adsorbed on the membrane surface.

[0041] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that: the mass ratio of the polymer monomer to the crosslinking agent in step 1① is 1:(0.1-5); the speed of the magnetic stirring in step 1① is 300r / min-500r / min, and the magnetic stirring time is 5h-7h. The other steps are the same as those in specific embodiment 1.

[0042] Specific embodiment 3: This embodiment differs from specific embodiment 1 or 2 in that: the polymer monomer in step 1① is any one of [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide, 2-methacryloyloxyethyl phosphorylcholine, carboxybetaine methacrylate and carboxybetaine acrylamide, or a combination of several of them in any ratio. The other steps are the same as those in specific embodiment 1 or 2.

[0043] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that: the cross-linking agent in step 1 is any one of polyethylene glycol diacrylate, N,N-methylenebis(acrylamide) and N,N-dimethylacryloylcystine or a combination of several of them in any ratio. The other steps are the same as those of specific embodiments 1 to 3.

[0044] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that the organic solvent in step 1② is any one of Isopar-G, benzene, xylene, n-hexane and cyclohexane or a combination of several of them in any ratio. The other steps are the same as those of specific embodiments 1 to 4.

[0045] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that the photoinitiator described in step 1 ② is any one of 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone and diphenylacetone. The other steps are the same as those of specific embodiments 1 to 5.

[0046] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that: the process for cleaning the membrane in step 2 is: soak the membrane in isopropyl alcohol for 5 hours to 7 hours, then wash it with deionized water for 3 to 5 times, and then store it in deionized water. The other steps are the same as those of specific embodiments 1 to 6.

[0047] Specific embodiment 8: This embodiment differs from specific embodiments 1 to 7 in that the wetting described in step 2 is to pour the liquid on the membrane surface and let it stand for 5 to 7 minutes, and then the liquid enters the membrane pores through capillary action. The other steps are the same as specific embodiments 1 to 7.

[0048] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that the membrane described in step 2 is any one of polysulfone membrane, polyethersulfone membrane, polyvinyl chloride membrane and polyvinylidene fluoride membrane. The other steps are the same as those of specific embodiments 1 to 8.

[0049] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that: the reaction under ultraviolet light in step 2 is to induce the photoinitiator in the organic phase to generate free radicals under the ultraviolet light that runs stably for 10 minutes, and the free radicals induce the polymer monomers and the crosslinking agent to undergo polymerization reaction at the interface between the organic phase and the aqueous phase to form a hydrogel layer; the reaction time under ultraviolet light is 5 minutes to 60 minutes. The other steps are the same as those of specific embodiments 1 to 9.

[0050] The following examples are used to verify the beneficial effects of the present invention:

[0051] Embodiment 1: A method for preparing a hydrophilic ultra-thin hydrogel modified film is specifically completed by the following steps:

[0052] 1. Prepare polymer liquid:

[0053] ①, add polymer monomer and cross-linking agent to deionized water, and stir magnetically at 300r / min for 6h to obtain aqueous polymer solution;

[0054] The polymer monomer described in step 1① is [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide;

[0055] The cross-linking agent described in step 1① is polyethylene glycol diacrylate;

[0056] The mass ratio of the polymer monomer to the cross-linking agent described in step 1① is 1:1;

[0057] The mass fraction of water in the aqueous phase polymerization liquid described in step 1① is 99%;

[0058] ②, adding a photoinitiator to an organic solvent and stirring to obtain an organic phase polymerization liquid;

[0059] The photoinitiator described in step 1② is 1-hydroxycyclohexyl phenyl ketone;

[0060] The organic solvent described in step 1② is Isopar-G;

[0061] The concentration of the photoinitiator in the organic phase polymerization solution described in step 1② is 0.01 g / mL;

[0062] 2. Preparation of hydrogel modified membrane:

[0063] The membrane is cleaned and fixed on a glass plate, and then deionized water is poured on the membrane surface, and after the membrane is wetted, the water on the surface is poured off and the membrane surface is blown dry; an aqueous phase polymer solution is poured on the membrane surface, and after the membrane is wetted, the surface aqueous phase polymer solution is poured off and residual droplets on the surface are removed; then an organic phase polymer solution is poured on the membrane surface and placed under an ultraviolet lamp for reaction to obtain an ultrathin hydrogel modified membrane;

[0064] The process for cleaning the membrane in step 2 is as follows: soak the membrane in isopropanol for 6 hours, then wash it three times with deionized water, and then store it in deionized water;

[0065] The wetting described in step 2 is to pour the liquid on the membrane surface and let it stand, waiting for the liquid to contact for 5 minutes to 7 minutes, and the liquid enters the membrane pores through capillary action;

[0066] The membrane described in step 2 is a polysulfone ultrafiltration membrane with a molecular weight cutoff of 100k Daltons;

[0067] The fixing in step 2 is as follows: the membrane is clamped on the glass plate along the four sides by a 1 cm thick hollow polytetrafluoroethylene plate through a binder clip, and a hollow rubber pad is added between the membrane and the plate to prevent the polymer solution from leaking; the middle hollow area is the membrane modification area, and the thickness of the plate can be used to accommodate the aqueous phase polymer solution and the organic phase polymer solution;

[0068] The step 2 of drying the membrane surface is as follows: using an air gun to spray nitrogen to dry the water on the membrane surface, leaving only a portion of deionized water inside the membrane pores to prevent the aqueous polymer solution from penetrating deeply into the membrane pores;

[0069] The step 2 of removing the residual droplets on the surface is as follows: using an air gun to spray nitrogen to gently blow off the residual droplets on the surface, leaving only the ultra-thin liquid layer adsorbed on the membrane surface;

[0070] 3. Cleaning the hydrogel modified membrane:

[0071] The ultra-thin hydrogel modified membrane was washed three times with deionized water and then stored in deionized water to obtain a hydrophilic ultra-thin hydrogel modified polysulfone membrane.

[0072] Embodiment 2: The difference between this embodiment and embodiment 2 is that the mass fraction of water in the aqueous phase polymerization liquid described in step 1① is 90%. The other steps and parameters are the same as those in embodiment 2.

[0073] Embodiment 3: The difference between this embodiment and embodiment 2 is that the mass fraction of water in the aqueous phase polymerization liquid described in step 1① is 80%. The other steps and parameters are the same as those in embodiment 2.

[0074] Figure 1 The scanning electron microscope cross-sectional images of the hydrophilic ultrathin hydrogel modified membranes prepared in Examples 1, 2 and 3;

[0075] from Figure 1 It can be seen that a hydrophilic hydrogel layer with nanometer-scale thickness is continuously coated on the surface of the polysulfone membrane. The thicknesses of the gel layers corresponding to Examples 1, 2 and 3 are 40 nm, 60 nm and 110 nm, respectively, indicating that as the hydrogel content increases, the thickness of the hydrogel on the membrane surface increases; and there is no obvious boundary between the hydrogel layer and the membrane surface, and the close combination of the two ensures the stability of the gel membrane.

[0076] Figure 2 The XPS full spectrum of the hydrophilic ultra-thin hydrogel modified membrane prepared in Examples 1, 2, and 3;

[0077] from Figure 2 It can be seen that the hydrophilic hydrogel layer is continuously coated on the surface of the polysulfone membrane because the N element representing the hydrogel component appears on its surface, and as the hydrogel content increases, the proportion of the N element increases, indicating that the gel membrane generated by the high concentration hydrogel content has a large degree of cross-linking.

[0078] The membrane anti-fouling performance was evaluated using a membrane filtration device built with a Millipore 8200 ultrafiltration cup produced by the American company MILLIPORE. Escherichia coli suspension was used as the membrane fouling test liquid (the concentration of Escherichia coli in the bacterial suspension was 1.7×10 6 CFUmL -1 ), the pollution-cleaning cycle test is used to characterize the membrane anti-fouling performance and its stability through the change trend of membrane specific flux, such as Figure 3 shown.

[0079] Figure 3This is the trend diagram of membrane specific flux change during the fouling-cleaning cycle test;

[0080] Depend on Figure 3 It can be seen that after 3 hours of Escherichia coli suspension filtration contamination, the flux of the commercial polysulfone ultrafiltration membrane and the hydrophilic ultrathin hydrogel modified membrane prepared in Examples 1, 2 and 3 dropped to 46%, 88%, 90% and 91% of the initial membrane flux, respectively; after a simple rinse with deionized water, the flux of the commercial polysulfone ultrafiltration membrane and the hydrophilic ultrathin hydrogel modified membrane prepared in Examples 1, 2 and 3 recovered to 56%, 97%, 98% and 100% of the initial membrane flux, respectively; compared with the purchased commercial polysulfone ultrafiltration membrane and hydrophilic modified membrane, the anti-pollution performance of the hydrophilic ultrathin hydrogel modified membrane was significantly improved; by repeating the Escherichia coli suspension filtration and contaminated membrane cleaning process, the anti-pollution stability of the hydrophilic ultrathin hydrogel modified membrane was verified.

Claims

1. A method for preparing a hydrophilic ultra-thin hydrogel modified film, characterized in that The preparation method is specifically completed according to the following steps:

1. Prepare polymer liquid: ①, add polymer monomer and cross-linking agent into deionized water, stir magnetically, and obtain aqueous polymer solution; The polymer monomer in step 1① is any one of [2-(methacryloyloxy)ethyl]dimethyl-(3-sulfopropyl)ammonium hydroxide, 2-methacryloyloxyethyl phosphorylcholine, carboxybetaine methacrylate and carboxybetaine acrylamide, or a combination of several of them in any ratio; The cross-linking agent in step 1 is any one of polyethylene glycol diacrylate, N,N-methylenebis(acrylamide) and N,N-dimethylacryloylcystine or a combination of several of them in any ratio; The mass fraction of water in the aqueous phase polymerization liquid described in step 1① is 80% to 99%; ②, adding a photoinitiator to an organic solvent and stirring to obtain an organic phase polymerization liquid; The concentration of the photoinitiator in the organic phase polymerization solution described in step 1② is 0.01 g / mL; 2. Preparation of hydrogel modified membrane: The membrane is cleaned and fixed on a glass plate, and then deionized water is poured on the membrane surface, and after the membrane is wetted, the water on the surface is poured off and the membrane surface is blown dry; an aqueous phase polymer solution is poured on the membrane surface, and after the membrane is wetted, the surface aqueous phase polymer solution is poured off and residual droplets on the surface are removed; then an organic phase polymer solution is poured on the membrane surface and placed under an ultraviolet lamp for reaction to obtain an ultrathin hydrogel modified membrane; 3. Cleaning the hydrogel modified membrane: The ultra-thin hydrogel modified membrane is washed with deionized water for 3 to 5 times, and then stored in deionized water to obtain a hydrophilic ultra-thin hydrogel modified membrane.

2. The method for preparing a hydrophilic ultra-thin hydrogel modified membrane according to claim 1, characterized in that The mass ratio of the polymer monomer to the cross-linking agent described in step 1① is 1:(0.1~5); the speed of the magnetic stirring described in step 1① is 300r / min~500r / min, and the time of magnetic stirring is 5h~7h.

3. The method for preparing a hydrophilic ultra-thin hydrogel modified membrane according to claim 1, characterized in that The organic solvent described in step 1② is any one of Isopar-G, benzene, xylene, n-hexane and cyclohexane, or a combination of several of them in any ratio.

4. The method for preparing a hydrophilic ultra-thin hydrogel modified membrane according to claim 1, characterized in that The photoinitiator described in step 1② is any one of 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone and diphenylacetone.

5. The method for preparing a hydrophilic ultra-thin hydrogel modified membrane according to claim 1, characterized in that The process for cleaning the membrane in step 2 is: soak the membrane in isopropanol for 5 hours to 7 hours, then wash it with deionized water for 3 to 5 times, and then store it in deionized water.

6. The method for preparing a hydrophilic ultra-thin hydrogel modified membrane according to claim 1, characterized in that The wetting described in step 2 is to pour the liquid on the membrane surface and let it stand, waiting for the liquid to contact for 5 minutes to 7 minutes, and the liquid enters the membrane pores through capillary action.

7. The method for preparing a hydrophilic ultra-thin hydrogel modified membrane according to claim 1, characterized in that The membrane described in step 2 is any one of a polysulfone membrane, a polyethersulfone membrane, a polyvinyl chloride membrane and a polyvinylidene fluoride membrane.

8. The method for preparing a hydrophilic ultra-thin hydrogel modified membrane according to claim 1, characterized in that The reaction under ultraviolet light in step 2 is to induce the photoinitiator in the organic phase to produce free radicals under ultraviolet light that runs stably for 10 minutes. The free radicals induce the polymer monomers and the crosslinking agent to undergo polymerization reaction at the interface between the organic phase and the aqueous phase to form a hydrogel layer; the reaction time under ultraviolet light is 5 minutes to 60 minutes.

Citation Information

Patent Citations

  • Heparinoid-modified polyvinyl alcohol hydrogel thin nano-compound hematodialysis film and preparation method thereof

    CN105727771A

  • Separation membrane modified by hydrophilic antifouling gel coating and preparation method thereof

    CN105833732A