A plant fiber toughened mortar and its preparation method and application

Through the coordinated combination of dendritic epoxy resin modified silicate cement, gradient particle size filler and kneaded fiber, the shrinkage and cracking problem of mortar during construction solidification is solved, and the shrinkage resistance and mechanical strength are significantly improved, achieving good results. engineering quality.

CN116553896BActive Publication Date: 2024-11-12FOSHAN ZHUOSHIGAO NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310541127.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-12
Estimated Expiration
2043-05-15

AI Technical Summary

Technical Problem

Due to the high moisture content during construction solidification, the surface of the existing mortar will crack later, affecting the quality of the project. The existing high-strength fast solid epoxy mortar cannot effectively solve this problem.

Method used

Using dendritic epoxy resin to modify silicate cement, fillers and kneaded fibers with gradient particle size design, and epoxy resin to modify silicate cement, gradient particle size fillers and plant fibers with specific epoxy equivalent and viscosity. Coordinated combination significantly improves the shrinkage resistance of the mortar.

Benefits of technology

The late cracking of the surface of the batch swing layer is significantly reduced, the mechanical strength and shrinkage resistance of the mortar are improved, the shrinkage rate is only 0.20%, and the problems of uneven distribution and uneven strength are avoided by improving compatibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004227963570000061
    Figure BDA0004227963570000061
  • Figure BDA0004227963570000071
    Figure BDA0004227963570000071
Patent Text Reader

Abstract

The present invention relates to the technical field of building materials, and in particular to a plant fiber toughened mortar and a preparation method and application thereof, wherein the raw materials for preparing the toughened mortar include: modified cement, filler, pre-seeded material, quicklime, and infiltration crystallization masterbatch. The present invention significantly enhances the anti-shrinkage effect of cement by using dendritic epoxy resin to modify silicate cement, and can reduce the late cracking of the surface of the plastering layer. The filler can be designed with a gradient particle size to effectively improve the compatibility of the filler in the system, especially the compatibility with modified cement and kneaded fiber, thereby avoiding the problems of uneven distribution, uneven strength, and partial cracking.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a plant fiber toughened mortar and a preparation method and application thereof. Background Art

[0002] Mortar has become an indispensable and important building material product in the national economic construction due to its wide source of raw materials, long corrosion resistance, low maintenance cost, energy saving and environmental protection. In recent years, with the continuous development of urbanization and large-scale urban construction, the mortar products industry has brought opportunities for development and is widely used in construction, water conservancy, transportation, landscaping and other engineering construction. However, when the mortar is solidified during construction, it will shrink due to the high moisture content, resulting in later cracking of the surface of the plastering layer, affecting further construction and engineering quality.

[0003] Chinese patent CN102875057B discloses a high-strength fast-setting epoxy mortar and its preparation method. The high-strength fast-setting epoxy mortar has high strength, fast strength development, good toughness, high adhesion with the substrate, good durability, and is environmentally friendly, but it still cannot effectively solve the problem of late shrinkage cracking. Therefore, a mortar with good anti-shrinkage performance and a wide range of applications is urgently needed. Summary of the invention

[0004] The first aspect of the present invention provides a plant fiber toughened mortar, wherein the raw materials for preparing the toughened mortar include: modified cement, filler, pre-mixed material, quicklime, and infiltration crystallization masterbatch.

[0005] In some embodiments, the prepared raw materials include, by weight: 15-20 parts of modified cement, 45-75 parts of filler, 15-25 parts of pre-mixed material, 0-10 parts of quicklime, and 0-3 parts of infiltration crystallization masterbatch.

[0006] Furthermore, the raw materials prepared include, by weight: 20 parts of modified cement, 55 parts of filler, 20 parts of pre-mixed material, 5 parts of quicklime, and 2 parts of infiltration crystallization masterbatch.

[0007] In some embodiments, the modified cement is high molecular polymer modified silicate cement.

[0008] Furthermore, the high molecular polymer includes at least one of polyurethane, polyethylene, polycarbonate, polylactic acid, and epoxy resin.

[0009] Furthermore, the modified cement is epoxy resin modified silicate cement.

[0010] Furthermore, the modified cement is dendritic epoxy resin modified silicate cement, and the preparation method is: adding the dendritic epoxy resin to the silicate cement while stirring, and stirring for 20-30 minutes, so that the mass ratio of the dendritic epoxy resin to the silicate cement is 1: (20-30).

[0011] Furthermore, the dendritic epoxy resin has an epoxy equivalent of 205-220 g / mol and a rotational viscosity of 14500-16000 cp, and is purchased from Weihai Chenyuan Molecular New Materials Co., Ltd. with a model number of CYE-002.

[0012] The applicant has found that modifying silicate cement with epoxy resin of specific epoxy equivalent and viscosity can significantly improve the shrinkage resistance of the modified cement and reduce the late cracking of the surface of the plastering layer. Too high viscosity makes it difficult to disperse silicate cement, while too low viscosity weakens the modification effect.

[0013] In some embodiments, the filler includes at least one of river sand, quartz sand, kaolin, quartz stone, feldspar, and mica.

[0014] In some embodiments, the filler has a particle size of 0.1-400 μm.

[0015] In some embodiments, the filler includes river sand, quartz sand, and kaolin in a mass ratio of (1-5):(1-5):(1-3).

[0016] Furthermore, the particle size of the river sand is 10-30 mesh.

[0017] Furthermore, the particle size of the quartz sand is 40-70 mesh.

[0018] Furthermore, the kaolin has a particle size of 0.8-1.0 μm and a specific surface area of ​​8-10 g / ㎡, and is purchased from Xinzhou City Xinfu District Xinze Kaolin Building Materials Co., Ltd.

[0019] The applicant also found that the gradient particle size design of the filler can effectively improve the compatibility of the filler in the system, especially the compatibility with modified cement and kneaded fiber, and avoid the problems of uneven distribution, uneven strength, and partial cracking. The speculated reason is that kaolin with a specific particle size and specific surface area can be better compatible with river sand and quartz sand, and the three gradient particle size fillers can form a relatively uniform spatial position with each other, providing a basis for improving the compatibility of the system.

[0020] In some embodiments, the raw materials for preparing the pre-mixed material include, by weight: 40-60 parts of kneaded fiber and 40-60 parts of cement.

[0021] In some embodiments, the raw materials for preparing the kneaded fiber include: plant fiber, low-viscosity sodium hydroxycellulose, HPMC cellulose ether, and additives.

[0022] Furthermore, the raw materials for preparing the kneaded fiber include, by weight: 85-100 parts of plant fiber, 0-3 parts of low-viscosity sodium hydroxycellulose, 0-2 parts of HPMC cellulose ether, and 0-9 parts of additives.

[0023] Furthermore, the plant fibers include coconut shell fibers, rice straw fibers, wheat straw fibers, and wood waste pulp fibers, with a weight ratio of (1-3): (1-3): (1-3): (1-3).

[0024] Furthermore, the plant fiber includes 1 mm coconut shell fiber, 0.5 mm rice straw fiber, 0.2 mm wheat straw fiber, and 0.05 mm wood waste pulp fiber, with a weight ratio of (1-3): (1-3): (1-3): (1-3).

[0025] Furthermore, the method for preparing the kneaded fiber comprises:

[0026] (1) dissolving low viscosity sodium hydroxycellulose, HPMC cellulose ether, and an additive in water to obtain a solution 1;

[0027] (2) The plant fibers are mixed evenly, and solution 1 is added thereto. The mixture is kneaded in a double-row spiral kneading and mixing device for 30 minutes, and then dried to obtain the product.

[0028] The applicant discovered during the research that after adding the kneaded fibers prepared by the present invention, the overall volume shrinkage problem of the mortar was significantly improved, which was further transformed into "nuclear shrinkage" when the mortar solidified. Therefore, the stress between the plastering layer and the masonry layer can be effectively eliminated, avoiding the later cracking of the surface of the plastering layer.

[0029] In some embodiments, the cement is silicate cement.

[0030] In some embodiments, the auxiliary agent is OPTIBENT 602 thixotropic agent and 5% sodium bicarbonate aqueous solution.

[0031] In some embodiments, the quicklime may be commercially available.

[0032] In some embodiments, the source of the infiltration crystallization masterbatch can be commercially available, such as the cement-based infiltration crystallization active masterbatch produced by Langfang Zuotu Anti-corrosion Equipment Co., Ltd.

[0033] The second aspect of the present invention provides a method for preparing a plant fiber toughened mortar, which is obtained by uniformly mixing the raw materials for preparing the toughened mortar.

[0034] The third aspect of the present invention provides an application of plant fiber toughened mortar in building exterior walls.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] 1. The present invention significantly enhances the anti-shrinkage effect of cement by modifying silicate cement with dendritic epoxy resin, and can reduce the late cracking of the surface of the plastering layer.

[0037] 2. The present invention can effectively improve the compatibility of the filler in the system, especially the compatibility with modified cement and kneaded fiber, by designing the filler with gradient particle size, so as to avoid the problems of uneven distribution, uneven strength and partial cracking.

[0038] 3. The present invention adds kneading fibers to form "nuclear shrinkage" when the mortar solidifies, thereby reducing later cracking.

[0039] 4. The present invention can improve the internal strength of the mortar through the synergistic combination of epoxy resin modified silicate cement with specific epoxy equivalent and viscosity, gradient particle size filler and plant fiber. Experiments have proved that the prepared mortar has excellent mechanical strength, a shrinkage rate of only 0.20%, and a good anti-shrinkage effect.

[0040] 5. The raw materials for the preparation of the present invention are simple and easy to obtain, the process is streamlined, and it is suitable for industrial production. DETAILED DESCRIPTION

[0041] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] Example 1

[0043] A plant fiber toughened mortar, the preparation raw materials of which include, by weight: 20 parts of modified cement, 55 parts of filler, 20 parts of pre-mixed material, 5 parts of quicklime, and 2 parts of infiltration crystallization masterbatch.

[0044] The modified cement is dendritic epoxy resin modified silicate cement, and the preparation method is: adding the dendritic epoxy resin to the silicate cement while stirring, stirring for 30 minutes, and the mass ratio of the dendritic epoxy resin to the silicate cement is 1:25. The epoxy equivalent of the dendritic epoxy resin is 205-220g / mol, and the rotational viscosity is 14500-16000cp.

[0045] The filler is river sand (particle size is 10-30 meshes), quartz sand (particle size is 40-70 meshes), and kaolin (particle size is 0.8-1.0 μm, specific surface area is 8-10 g / ㎡), and the mass ratio is 4:2:3.

[0046] By weight, the raw materials for preparing the pre-mixed seed material include: 50 parts of kneaded fiber and 50 parts of silicate cement.

[0047] By weight, the raw materials for preparing the kneaded fiber include: 90 parts of plant fiber, 2 parts of low-viscosity sodium hydroxycellulose, 1 part of HPMC cellulose ether, 1 part of OPTIBENT 602 thixotropic agent, and 5 parts of 5% sodium bicarbonate aqueous solution.

[0048] The plant fibers are 1 mm coconut shell fibers, 0.5 mm rice straw fibers, 0.2 mm wheat straw fibers, and 0.05 mm wood waste paper pulp fibers, with a weight ratio of 1:1:1:1. The preparation method comprises: 1. dissolving low-viscosity sodium hydroxycellulose, HPMC cellulose ether, and an additive in 500 mL of water to obtain a solution 1; 2. mixing the plant fibers evenly, adding the solution 1 at a mass ratio of 20:1, kneading in a double-row spiral kneading and mixing device for 30 minutes, and drying to obtain the obtained solution.

[0049] Example 2

[0050] A plant fiber toughened mortar, the preparation raw materials of which include, by weight: 15 parts of modified cement, 45 parts of fillers, 15 parts of pre-mixed materials, 1 part of quicklime, and 1 part of infiltration crystallization masterbatch.

[0051] The modified cement is dendritic epoxy resin modified silicate cement, and the preparation method is: adding the dendritic epoxy resin to the silicate cement while stirring, stirring for 30 minutes, and the mass ratio of the dendritic epoxy resin to the silicate cement is 1:20. The epoxy equivalent of the dendritic epoxy resin is 205-220g / mol, and the rotational viscosity is 14500-16000cp.

[0052] The filler is river sand (particle size is 10-30 meshes), quartz sand (particle size is 40-70 meshes), and kaolin (particle size is 0.8-1.0 μm, specific surface area is 8-10 g / ㎡), and the mass ratio is 1:1:1.

[0053] In parts by weight, the raw materials for preparing the pre-mixed seed material include: 40 parts of kneaded fiber and 40 parts of silicate cement.

[0054] By weight, the raw materials for preparing the kneaded fiber include: 85 parts of plant fiber, 1 part of low-viscosity sodium hydroxycellulose, 1 part of HPMC cellulose ether, 1 part of OPTIBENT 602 thixotropic agent, and 5 parts of 5% sodium bicarbonate aqueous solution.

[0055] The plant fibers are 1 mm coconut shell fibers, 0.5 mm rice straw fibers, 0.2 mm wheat straw fibers, and 0.05 mm wood waste paper pulp fibers, with a weight ratio of 1:2:3:1. The preparation method comprises: 1. dissolving low-viscosity sodium hydroxycellulose, HPMC cellulose ether, and an additive in 500 mL of water to obtain a solution 1; 2. mixing the plant fibers evenly, adding the solution 1 at a mass ratio of 20:1, kneading in a double-row spiral kneading and mixing device for 30 minutes, and drying to obtain the obtained solution.

[0056] Example 3

[0057] A plant fiber toughened mortar, the preparation raw materials of which include, by weight: 20 parts of modified cement, 75 parts of filler, 25 parts of pre-mixed material, 10 parts of quicklime, and 3 parts of infiltration crystallization masterbatch.

[0058] The modified cement is dendritic epoxy resin modified silicate cement, and the preparation method is: adding the dendritic epoxy resin to the silicate cement while stirring, stirring for 30 minutes, and the mass ratio of the dendritic epoxy resin to the silicate cement is 1:30. The epoxy equivalent of the dendritic epoxy resin is 205-220g / mol, and the rotational viscosity is 14500-16000cp.

[0059] The filler is river sand (particle size is 10-30 meshes), quartz sand (particle size is 40-70 meshes), and kaolin (particle size is 0.8-1.0 μm, specific surface area is 8-10 g / ㎡), and the mass ratio is 5:5:3.

[0060] By weight, the raw materials for preparing the pre-seeding material include: 60 parts of kneaded fiber and 60 parts of silicate cement.

[0061] By weight, the raw materials for preparing the kneaded fiber include: 100 parts of plant fiber, 3 parts of low-viscosity sodium hydroxycellulose, 2 parts of HPMC cellulose ether, 1 part of OPTIBENT 602 thixotropic agent, and 5 parts of 5% sodium bicarbonate aqueous solution.

[0062] The plant fibers are 1 mm coconut shell fibers, 0.5 mm rice straw fibers, 0.2 mm wheat straw fibers, and 0.05 mm wood waste paper pulp fibers, with a weight ratio of 2:2:3:3. The preparation method comprises: 1. dissolving low-viscosity sodium hydroxycellulose, HPMC cellulose ether, and an additive in 500 mL of water to obtain a solution 1; 2. mixing the plant fibers evenly, adding the solution 1 at a mass ratio of 20:1, kneading in a double-row spiral kneading and mixing device for 30 minutes, and drying to obtain the obtained solution.

[0063] Comparative Example 1

[0064] A plant fiber toughened mortar, the specific implementation method is the same as Example 1, except that the epoxy equivalent of the dendritic epoxy resin is 240-260 g / mol, the rotational viscosity is 15000-16500 cp, and it is purchased from Weihai Chenyuan Molecular New Materials Co., Ltd., model CYE-003.

[0065] Comparative Example 2

[0066] A plant fiber toughened mortar, the specific implementation manner is the same as that of Example 1, except that the filler is river sand (particle size is 10-30 mesh) and quartz sand (particle size is 40-70 mesh), and the mass ratio is 4:2.

[0067] Comparative Example 3

[0068] A plant fiber toughened mortar, the specific implementation method is the same as that of Example 1, except that 0 parts of pre-mixed seed material is used.

[0069] Comparative Example 4

[0070] A plant fiber toughened mortar, the specific implementation method is the same as that of Example 1, except that 20 parts of kneaded fibers are used.

[0071] Comparative Example 5

[0072] A plant fiber toughened mortar, the specific implementation method is the same as that of Example 1, except that acrylic resin is used to replace the dendritic epoxy resin, and the acrylic resin is purchased from DSM.

[0073] Comparative Example 6

[0074] A plant fiber toughened mortar, the specific implementation manner is the same as that of Example 1, except that the mass ratio of the dendritic epoxy resin to silicate cement is 1:10.

[0075] Comparative Example 7

[0076] A plant fiber toughened mortar, the specific implementation method is the same as Example 1, except that it contains 20 parts of modified cement, 30 parts of filler, 30 parts of pre-mixed material, 15 parts of quicklime, and 2 parts of infiltration crystallization masterbatch.

[0077] Performance Testing

[0078] The plant fiber toughened mortar prepared in the above examples and comparative examples was subjected to the following tests after curing for 3 days. The results are shown in Table 1.

[0079] The strength related tests were carried out with reference to the standard JC-T 1024-2007 on wall facing mortar.

[0080] Refer to GBT20473-2021 for shrinkage test.

[0081] Table 1

[0082]

[0083]

[0084] It can be seen from Examples 1-3 that the mortar prepared by the present invention has good flexural and compressive strength and low shrinkage. It can be seen from the comparative example that after changing the limiting parameters, gradient particle size ratio and formula addition amount of the epoxy resin, the mechanical properties and anti-shrinkage effect are significantly deteriorated, indicating that the compatibility of the formula is unstable within the system, which further affects the use effect of the mortar.

[0085] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A plant fiber toughened mortar, characterized in that: In parts by weight, the raw materials for preparing the toughened mortar include: 20 parts of modified cement, 55 parts of filler, 20 parts of pre-mixed material, 5 parts of quicklime, and 2 parts of infiltration crystallization masterbatch; The modified cement is dendritic epoxy resin modified silicate cement, and the preparation method is: adding the dendritic epoxy resin to silicate cement while stirring, stirring for 30 minutes, and the mass ratio of the dendritic epoxy resin to the silicate cement is 1:25; the epoxy equivalent of the dendritic epoxy resin is 205-220g / mol, and the rotational viscosity is 14500-16000cp; The filler is river sand, quartz sand and kaolin, with a mass ratio of 4:2:3; The particle size of river sand is 10-30 mesh; the particle size of quartz sand is 40-70 mesh; the particle size of kaolin is 0.8-1.0μm, and the specific surface area is 8-10 g / ㎡; In parts by weight, the raw materials for preparing the pre-seeded material include: 50 parts of kneaded fiber and 50 parts of silicate cement; The raw materials for preparing the kneaded fiber include, by weight: 90 parts of plant fiber, 2 parts of low-viscosity sodium hydroxycellulose, 1 part of HPMC cellulose ether, 1 part of OPTIBENT 602 thixotropic agent, and 5 parts of 5% sodium bicarbonate aqueous solution; The plant fibers are 1 mm coconut shell fibers, 0.5 mm rice straw fibers, 0.2 mm wheat straw fibers, and 0.05 mm wood waste paper pulp fibers, with a weight ratio of 1:1:1:

1. The preparation method comprises:

1. dissolving low-viscosity sodium hydroxycellulose, HPMC cellulose ether, OPTIBENT602 thixotropic agent, and sodium bicarbonate aqueous solution in 500 mL of water to obtain solution 1; 2. mixing the plant fibers evenly, adding solution 1 at a mass ratio of 20:1, kneading in a double-row spiral kneading mixing device for 30 minutes, and drying to obtain the obtained product.

2. A method for preparing the plant fiber toughened mortar according to claim 1, characterized in that: The raw materials for preparing the toughening mortar are mixed evenly to obtain the mortar.