Method for producing zirconia sintered body
Through the multi-stage heating process and the use of stabilizers, the problem of poor hue and light transmittance of sintered zirconia sintered bodies in a short time is solved, and the aesthetic and strength requirements of reproducing the ideal zirconia sintered bodies in a short time are achieved. , suitable for dental patches.
Patent Information
- Application Number
- CN202310495309.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-07-31
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-07-31
AI Technical Summary
The prior art is difficult to reproduce the ideal zirconia sintered body with the same hue and light transmittance in a short period of time, and cannot meet the aesthetic requirements and strength requirements of dental patches.
The sintering method of a multi-stage heating process is adopted, including the first heating process, the second heating process and the third heating process, to control the heating rate and temperature, to ensure that the zirconia molded body or pre-sintered body is sintered in a short time, and includes a stabilizer Such as yttrium oxide, it can optimize the hue and light transmittance of the sintered body.
The same zirconia sintered body as sintered for a long time is manufactured in a short time, which meets the aesthetic requirements and strength requirements of dental patches. It has excellent hue and light transmittance, and is suitable for use in dental products.
Smart Images

Figure CN116553925B_ABST
Abstract
Description
Technical Field
[0001] This application is a divisional application of the PCT application entering the national phase with application number 202080054914.X (international filing date is July 31, 2020) and invention name "Method for producing a zirconia sintered body". The present invention relates to a method for producing a zirconia sintered body. Background Art
[0002] In the past, metals were widely used as dental products (e.g., representative crowns, tooth crowns, prostheses such as dentures, orthodontic products, and dental implant products). However, the color of metal is significantly different from that of natural teeth, which has the disadvantage of lacking aesthetic appeal, and sometimes causes allergies due to metal dissolution. Therefore, in order to solve the problems associated with the use of metals, ceramic materials such as alumina (aluminum oxide) or zirconium oxide (zirconia) are gradually being used in dental products as alternative materials to metals. In particular, zirconium oxide has excellent strength and aesthetic appeal, and therefore, demand has increased, especially in conjunction with the recent low prices.
[0003] On the other hand, for the production of dental prostheses using zirconia, since a predetermined shape of the dental prostheses (unsintered zirconia processed body) is cut out from a block or disc-shaped cutting workpiece (cut workpiece) pre-fired at a temperature about 400°C to 700°C lower than the temperature at which an ideal sintered body can be obtained using a CAD / CAM device, and the cut unsintered zirconia processed body is sintered by being kept at a maximum temperature of 1400°C to 1650°C, it usually takes 6 hours to 12 hours to calculate the total time from heating, staying, to cooling. Regarding this time, the demand for short-time firing in dental hospitals has increased in recent years, and a firing furnace capable of firing in a short time as described in Patent Document 1 has also been manufactured. However, short-time firing has problems such as increased brightness, and it is difficult to obtain the same hue or light transmittance as in normal firing in short-time firing.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2015-531048. Summary of the invention
[0007] Problems to be solved by the invention
[0008] Patent Document 1 describes a firing furnace and scheduling conditions for a ceramic containing zirconium oxide in a short period of time, but the scheduling cannot be used to obtain specific ideal physical properties of a dental zirconium oxide sintered body. It is aimed at a theoretically achievable firing furnace, and does not describe the necessary physical properties, color, etc. for a dental prosthesis obtained from a specific fired body, and does not meet the firing conditions for satisfying aesthetic requirements.
[0009] Therefore, an object of the present invention is to provide a method for producing a zirconia sintered body by sintering a zirconia formed body or a zirconia calcined body in a short time and capable of reproducing the aesthetic requirements and strength of an ideal dental prosthesis to the same extent as in the case of conventional sintering.
[0010] Means for solving problems
[0011] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found that by applying a specific short-time firing schedule to a zirconia formed body or a zirconia calcined body, a dental prosthesis having excellent reproducibility of hue (brightness and chroma) and light transmittance can be manufactured. Based on this finding, further studies were conducted to complete the present invention.
[0012] That is, the present invention includes the following technical solutions.
[0013] [1] A method for producing a zirconia sintered body, comprising a firing step of firing a zirconia formed body or a zirconia calcined body,
[0014] The sintering step includes at least three steps of heating steps, namely, a first heating step (H1), a second heating step (H2) and a third heating step (H3).
[0015] The temperature increase rate in the first temperature increase step (H1) is denoted as HR1.
[0016] The temperature increase rate in the second temperature increase step (H2) is denoted as HR2.
[0017] When the temperature increase rate in the third temperature increase step (H3) is denoted as HR3,
[0018] HR1=50~500℃ / min,
[0019] HR2=11~300℃ / min,
[0020] HR3=10~299℃ / min,
[0021] HR1>HR2,
[0022] HR2 / HR3>1,
[0023] Regarding the starting temperature in each heating step,
[0024] In H1, the temperature is from room temperature to 500℃.
[0025] 900~1250℃ in H2
[0026] In H3, it is 1300~1550℃,
[0027] Regarding the reaching temperature in each heating step,
[0028] In H1, it is 900~1250℃,
[0029] 1300~1550℃ in H2
[0030] In H3, it is 1400~1650℃.
[0031] [2] The method for producing a zirconia sintered body according to [1], wherein HR2 is 13 to 280°C / min.
[0032] [3] The method for producing a zirconia sintered body according to [1] or [2], wherein HR3 is 13 to 250°C / min.
[0033] [4] The method for producing a zirconia sintered body according to any one of [1] to [3], wherein HR2 / HR3>1.5.
[0034] [5] The method for producing a zirconia sintered body according to any one of [1] to [4], wherein the maximum sintering temperature in the temperature raising step is 1400 to 1650° C., and the residence time at the maximum sintering temperature is within 15 minutes.
[0035] [6] The method for producing a zirconia sintered body according to any one of [1] to [5], comprising: a cooling step of cooling from the highest sintering temperature in the heating step to 1100°C at a cooling rate of 10°C / min or more.
[0036] [7] A method for producing a zirconia sintered body according to any one of [1] to [6], wherein the total sintering time from the start of the temperature increase in the first temperature increase step (H1) in the sintering step to the end of the residence time at the maximum sintering temperature is within 50 minutes.
[0037] [8] The method for producing a zirconia sintered body according to any one of [1] to [7], wherein 55% or more of the zirconia calcined body is monoclinic.
[0038] [9] The method for producing a zirconia sintered body according to any one of [1] to [8], wherein the zirconia formed body or the zirconia calcined body contains 2 to 8 mol % of a stabilizer.
[0039]
[10] The method for producing a zirconia sintered body according to [9], wherein in the zirconia formed body or the zirconia calcined body, at least a portion of the stabilizer is not dissolved in zirconia.
[0040]
[11] The method for producing a zirconia sintered body according to [9] or
[10] , wherein the stabilizer is yttrium oxide.
[0041]
[12] The method for producing a zirconia sintered body according to any one of [1] to
[11] , wherein the zirconia formed body or the zirconia calcined body has a predetermined shape of a dental product.
[0042]
[13] The method for producing a zirconia sintered body according to
[12] , wherein the dental product is a dental prosthesis.
[0043] Effects of the Invention
[0044] According to the method for producing a zirconia sintered body of the present invention, a zirconia formed body or a zirconia calcined body can be sintered in a short time, and a zirconia sintered body that can reproduce the aesthetic requirements and strength of an ideal dental prosthesis to the same extent as in the case of conventional sintering (sintering for 6 to 12 hours) can be produced. In addition, by using the method for producing a zirconia sintered body of the present invention, the obtained zirconia sintered body has excellent color reproducibility. According to the method for producing a zirconia sintered body of the present invention, the color development of the composite oxide contained in the zirconia formed body or the zirconia calcined body can be promoted, and appropriate brightness can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 This is a graph showing the temperature increase rate in the temperature increase step described in Example 1.
[0046] Figure 2 This is a diagram showing the temperature increase rate in the temperature increase step described in Example 2.
[0047] Figure 3 This is a diagram showing the temperature increase rate in the temperature increase step described in Example 3.
[0048] Figure 4 This is a graph showing the temperature increase rate in the temperature increase step described in Comparative Example 1.
[0049] Figure 5 This is a graph showing the temperature increase rate in the temperature increase step described in Comparative Example 2. DETAILED DESCRIPTION
[0050] Hereinafter, the present invention will be described in detail.
[0051] The firing furnace used in the firing of the present invention is an atmospheric furnace, which can be a box-type furnace, a crucible furnace, a tubular furnace, a furnace bottom lifting furnace, a continuous furnace, a rotary furnace, a resistance heating furnace, an induction heating furnace, a straight-through electric furnace, an IH furnace, a high-frequency furnace, a microwave oven, and the heat release body can use a metal heat release body, silicon carbide, molybdenum disilicide, lanthanum chromium wire, molybdenum, carbon, tungsten, etc., and SiC can also be used as a heat release body base. It can also be a firing furnace obtained by combining any two or more of these. In addition, the firing furnace has a small internal volume of the firing furnace with a base for placing the zirconia formed body or zirconia pre-calcined body having a specified shape such as a crown, and the thermal efficiency is good, which can easily maintain the heat in the furnace during firing.
[0052] In addition, in this specification, the upper limit and lower limit of the numerical range (heating rate, cooling rate, sintering time, temperature, rate ratio, content of each component (for example, stabilizer) etc.) can be combined appropriately.
[0053] The method for producing a zirconia sintered body of the present invention includes at least three stages of heating processes. The first heating process is denoted as H1, the second heating process is denoted as H2, and the third heating process is denoted as H3, and each heating process has a different heating rate. In addition, the heating process may be only three stages, or may include other heating processes.
[0054] [First temperature rising step (H1)]
[0055] In the first heating step (H1) in the method for producing a zirconia sintered body of the present invention, a zirconia formed body or a zirconia pre-calcined body is heated in a firing furnace heated to room temperature or above room temperature and below 500°C, and the temperature is raised to the reaching temperature of the first heating step (H1) at one time. The zirconia formed body or the zirconia pre-calcined body before firing in the first heating step (H1) preferably has a prescribed shape of a dental product. Dental products include, for example, representative dental prostheses such as crowns, tooth crowns, and attached dentures; products for orthodontic treatment; products for dental implants, etc. The zirconia formed body or the zirconia pre-calcined body before heating can be processed using a dental CAD / CAM device, or can be produced by a dental technician through cutting or the like.
[0056] The zirconia formed body or zirconia calcined body before heating may be directly placed on the muffle member of the firing furnace during firing, or may be placed in the furnace using a tray, base, or pin formed of ceramic or high melting point metal, or may be placed using ceramic beads.
[0057] The starting temperature of the first temperature rising step (H1) is room temperature to 500°C, preferably room temperature to 400°C, more preferably room temperature to 300°C, and even more preferably room temperature to 200°C. The reaching temperature of the first temperature rising step (H1) is 900°C to 1250°C. From the viewpoint of further shortening the operation time, it is preferably 950°C or higher, more preferably 1000°C or higher, and even more preferably 1050°C or higher. In addition, from the viewpoint of obtaining a zirconia sintered body with better brightness and light transmittance, it is preferably 1230°C or lower, more preferably 1220°C or lower, and even more preferably 1200°C or lower.
[0058] In addition, when the heating rate of the first heating step (H1) is recorded as HR1, HR1 is 50°C / min or more, preferably 60°C / min or more, more preferably 70°C / min or more, and more preferably 80°C / min or more from the viewpoint of further shortening the working time. In addition, HR1 is 500°C / min or less, preferably 450°C / min or less, more preferably 400°C / min or less, and more preferably 350°C / min or less. When HR1 exceeds 500°C / min, there is a possibility of inducing the generation of cracks or cracks during firing. In the case where the zirconia formed body or zirconia calcined body provided for the first heating step (H1) contains water used in processing and a coloring pigment liquid, the first heating step (H1) can be started after a drying step of 300°C or less and 1 minute or more and 20 minutes or less, preferably 5 minutes or more and 15 minutes or less.
[0059] [Second temperature rising step (H2)]
[0060] In the method for producing a zirconia sintered body of the present invention, when the heating rate of the second heating step (H2) is recorded as HR2, HR1>HR2. By setting HR1>HR2, when combined with other structures, the color difference △E*ab of the zirconia sintered body can be suppressed from becoming too large, and a dental product with excellent hue can be obtained. In a suitable embodiment, HR1 / HR2>1.5, and HR1 / HR2>2 can be obtained. In addition, HR2 is 11°C / min or more, and from the viewpoint of further shortening the working time, it is preferably 13°C / min or more, more preferably 15°C / min or more, and further preferably 20°C / min or more. In addition, HR2 is 300°C / min or less, and from the viewpoint of better brightness and light transmittance of the obtained zirconia sintered body, it is preferably 280°C / min or less, more preferably 260°C / min or less, and further preferably 250°C / min or less.
[0061] The starting temperature of the second temperature raising step (H2) is 900-1250°C, and is preferably 950°C or higher, more preferably 1000°C or higher, and more preferably 1050°C or higher, from the viewpoint of further shortening the working time. In addition, from the viewpoint of better brightness and light transmittance of the obtained zirconia sintered body, the starting temperature is preferably 1230°C or lower, more preferably 1220°C or lower, and more preferably 1200°C or lower. The reaching temperature of the second temperature raising step (H2) is 1300-1550°C, and is preferably 1310°C or higher, more preferably 1320°C or higher, and more preferably 1350°C or higher, from the viewpoint of further shortening the working time. In addition, from the viewpoint of better brightness, light transmittance and chroma of the obtained zirconia sintered body, and better color development of the composite oxide contained in the zirconia formed body or the zirconia calcined body, the reaching temperature of H2 is preferably 1540°C or lower, more preferably 1530°C or lower, and more preferably 1520°C or lower.
[0062] [Third Temperature Heating Step (H3)]
[0063] When the heating rate in the third heating step (H3) is denoted as HR3, HR2 / HR3>1. From the viewpoint of the brightness, light transmittance and chroma of the obtained zirconia sintered body being more excellent and the color development of the composite oxide contained in the zirconia formed body or the zirconia calcined body being excellent, HR2 / HR3>1.2 is preferred, HR2 / HR3>1.5 is more preferred, and HR2 / HR3>2 is further preferred. In addition, HR3 is 10°C / min or more. From the viewpoint of further shortening the working time, HR3 is preferably 11°C / min or more, more preferably 12°C / min or more, and further preferably 13°C / min or more. In addition, from the viewpoint of the chroma of the obtained zirconia sintered body being more excellent and the color development of the composite oxide contained in the zirconia formed body or the zirconia calcined body being excellent, HR3 is 299°C / min or less, preferably 270°C / min or less, more preferably 250°C / min or less, and further preferably 200°C / min or less.
[0064] The starting temperature of the third temperature raising step (H3) is 1300-1550°C, and is preferably 1310°C or higher, more preferably 1320°C or higher, and further preferably 1350°C or higher from the viewpoint of further shortening the operation time. In addition, from the viewpoint of better brightness, light transmittance and chroma of the obtained zirconia sintered body and better color rendering of the composite oxide contained in the zirconia formed body or the zirconia calcined body, the starting temperature of H3 is preferably 1540°C or lower, more preferably 1530°C or lower, and further preferably 1520°C or lower.
[0065] The reaching temperature of the third temperature raising step (H3) is 1400-1650°C, and is preferably 1450°C or higher, more preferably 1500°C or higher, and further preferably 1520°C or higher, from the viewpoint of further improving the brightness, light transmittance, and chroma of the obtained zirconia sintered body and improving the color development of the composite oxide contained in the zirconia formed body or the zirconia calcined body. In addition, from the viewpoint of further shortening the working time, improving the brightness, light transmittance, and chroma of the obtained zirconia sintered body and improving the color development of the composite oxide contained in the zirconia formed body or the zirconia calcined body, the reaching temperature of H3 is preferably 1630°C or lower, more preferably 1620°C or lower, and further preferably 1610°C or lower. The difference between the starting temperature and the reaching temperature of the third temperature raising step (H3) (reaching temperature-starting temperature) is preferably 30°C or higher, more preferably 40°C or higher, and further preferably 50°C or higher. In addition, in a certain embodiment, the treatment time of the third temperature rising step (H3) is preferably shorter than the treatment time of the first temperature rising step (H1) from the viewpoint that the brightness, light transmittance and chroma of the obtained zirconia sintered body are more excellent, and the color rendering of the composite oxide contained in the zirconia formed body or the zirconia calcined body is excellent. Furthermore, in another embodiment, the treatment time of the third temperature rising step (H3) is preferably shorter than the treatment time of the second temperature rising step (H2) from the viewpoint that the brightness, light transmittance and chroma of the obtained zirconia sintered body are more excellent, and the color rendering of the composite oxide contained in the zirconia formed body or the zirconia calcined body is excellent.
[0066] The zirconia formed body or zirconia calcined body used in the method for producing a zirconia sintered body of the present invention preferably contains a stabilizer capable of suppressing the phase transformation of zirconia in addition to zirconia. The zirconia formed body or zirconia calcined body is preferably a zirconia formed body or zirconia calcined body in which at least a part of the stabilizer is not solid-dissolved in zirconia. The stabilizer is preferably capable of forming partially stabilized zirconia.
[0067] Examples of the stabilizer include calcium oxide (CaO), magnesium oxide (MgO), yttrium oxide, cerium oxide (CeO2), scandium oxide (Sc2O3), niobium oxide (Nb2O5), lanthanum oxide (La2O3), erbium oxide (Er2O3), praseodymium oxide (Pr6O 11), samarium oxide (Sm2O3), europium oxide (Eu2O3) and thulium oxide (Tm2O3) and other oxides. The stabilizer can be used alone or in combination of two or more. The content of the stabilizer in the zirconium oxide calcined body and its sintered body of the present invention can be measured by, for example, inductively coupled plasma (ICP; Inductively Coupled Plasma) emission spectrometry, fluorescent X-ray analysis, etc. In the zirconium oxide calcined body and its sintered body of the present invention, the content of the stabilizer is preferably 0.1~18mol%, more preferably 1~15mol%, and further preferably 2~8mol% relative to the total mol of zirconium oxide and stabilizer. From the viewpoint of the strength and light transmittance of the obtained zirconium oxide sintered body, the zirconium oxide formed body or the zirconium oxide calcined body preferably contains yttrium oxide as a stabilizer. The content of yttrium oxide is preferably 3mol% or more, more preferably 3.5mol% or more, further preferably 3.8mol% or more, and particularly preferably 4.0mol% or more relative to the total mol of zirconium oxide and yttrium oxide. When the content of yttrium oxide is 3 mol% or more, the light transmittance of the zirconium oxide sintered body can be improved. In addition, the content of yttrium oxide is preferably 7.5 mol% or less, more preferably 7.0 mol% or less, further preferably 6.5 mol% or less, and particularly preferably 6.0 mol% or less relative to the total mol of zirconium oxide and yttrium oxide. When the content of yttrium oxide is 7.5 mol% or less, the strength reduction of the obtained zirconium oxide sintered body can be suppressed.
[0068] In the zirconia formed body or zirconia calcined body of the present invention, it is preferred that at least a portion of the aforementioned stabilizer is not solid-dissolved in zirconia. That a portion of the stabilizer is not solid-dissolved in zirconia can be confirmed, for example, by an XRD diagram. When a peak derived from the stabilizer is confirmed in the XRD diagram of the zirconia calcined body, it indicates that there is a stabilizer that is not solid-dissolved in zirconia in the zirconia formed body or the zirconia calcined body. When all stabilizers are solid-dissolved, basically no peak derived from the stabilizer is confirmed in the XRD diagram. Among them, depending on conditions such as the crystal state of the stabilizer, even if there is no peak of the stabilizer in the XRD diagram, the stabilizer is sometimes not solid-dissolved in zirconia. The main crystal system of zirconia is a tetragonal system and / or a cubic system. When there is no peak of the stabilizer in the XRD diagram, it can be considered that most of the stabilizer, or substantially all of it, is solid-dissolved in zirconia. In the zirconia formed body or zirconia calcined body of the present invention, it may be that all of the stabilizer is not solid-dissolved in zirconia. It should be noted that in the present invention, solid-dissolved stabilizer means, for example, that the element (atom) contained in the stabilizer is solid-dissolved in zirconia.
[0069] In the zirconia formed body or zirconia calcined body of the present invention, the existence ratio of yttrium oxide not dissolved in zirconia (hereinafter sometimes referred to as "undissolved yttrium oxide") is yIt can be calculated according to the following mathematical formula (1): The existence rate of undissolved yttrium oxide f y It is preferably greater than 0%, more preferably 1% or more, further preferably 2% or more, and particularly preferably 3% or more. y The upper limit of f may be, for example, 15% or less, depending on the content of yttria in the zirconia formed body or the zirconia calcined body. When the content of yttria is 3 mol% or more and less than 4.5 mol%, f y When the content of yttrium oxide is 4.5 mol% or more and less than 5.8 mol%, f y When the content of yttrium oxide is 5.8 mol% or more and 7.5 mol% or less, f y It may be less than 15%.
[0070] In the zirconia formed body or the zirconia calcined body of the present invention, when the content of yttria is 3 mol% or more and less than 4.5 mol%, f y It is preferably 0.5% or more, more preferably 1.0% or more, and even more preferably 2.0% or more. When the content of yttrium oxide is 4.5 mol% or more and less than 5.8 mol%, the existence rate of undissolved yttrium oxide is y When the content of yttrium oxide is 5.8 mol % or more and 7.5 mol % or less, f y Preferably it is 2% or more, more preferably 3% or more, and further preferably 4% or more. In the zirconia calcined body of the present invention, when the content of yttrium oxide is 3 mol% or more and less than 4.5 mol%, f m / f y It is preferably 20 to 200, more preferably 25 to 100, and even more preferably 30 to 60. When the content of yttrium oxide is 4.5 mol% or more and less than 5.8 mol%, f m / f y Preferably, it is 5 to 45, more preferably, it is 10 to 40, and further preferably, it is 15 to 35. When the content of yttrium oxide is 5.8 mol% or more and 7.5 mol% or less, f m / f y It is preferably 2 to 40, more preferably 5 to 35, and even more preferably 10 to 30. m As described later, it refers to the ratio of monoclinic crystals in zirconium oxide calculated by mathematical formula (2).
[0071] [Mathematical formula 1]
[0072]
[0073] In mathematical formula (1), Iy (111) represents the peak intensity of the (111) plane of yttrium oxide at around 2θ=29° in the XRD pattern based on CuKα radiation. m (111) and I m (11-1) represents the peak intensity of the (111) plane and the (11-1) plane of the monoclinic system of zirconium oxide. t (111) represents the peak intensity of the (111) plane of the tetragonal system of zirconium oxide. c (111) represents the peak intensity of the (111) plane of the cubic crystal system of zirconium oxide.
[0074] For the above mathematical formula (1), by substituting other peaks in place of I y (111) can also be applied to the calculation of the undissolved fraction of stabilizers other than yttrium oxide.
[0075] The main crystal system of zirconium oxide in the zirconium oxide calcined body of the present invention is preferably monoclinic. In the present invention, "the main crystal system is monoclinic" means that the proportion of monoclinic in zirconium oxide calculated by the following mathematical formula (2) relative to the total amount of all crystal systems (monoclinic, tetragonal and cubic) in zirconium oxide is: m In the calcined zirconium oxide of the present invention, the ratio of the monoclinic system in the zirconium oxide calculated by the following mathematical formula (2) is: m The proportion of the monoclinic system is preferably 55% or more, more preferably 60% or more, further preferably 70% or more, further preferably 75% or more, particularly preferably 80% or more, more particularly preferably 85% or more, and most preferably 90% or more relative to the total amount of the monoclinic system, tetragonal system, and cubic system. m It can be calculated from the peak of the X-ray diffraction (XRD) chart using CuKα rays by the following mathematical formula (2): It should be noted that the main crystal system in the calcined zirconium oxide body may contribute to the increase in the shrinkage temperature and the shortening of the sintering time.
[0076] In the calcined zirconium oxide of the present invention, the peaks of the tetragonal system and the cubic system can be substantially undetectable. That is, the ratio of the monoclinic system is m It can be 100%.
[0077] [Mathematical formula 2]
[0078]
[0079] In mathematical formula (2), I m (111) and I m (11-1) represent the peak intensities of the (111) plane and (11-1) plane of the monoclinic system of zirconium oxide, respectively.t (111) represents the peak intensity of the (111) plane of the tetragonal system of zirconium oxide. c (111) represents the peak intensity of the (111) plane of the cubic crystal system of zirconium oxide.
[0080] The zirconia formed body or zirconia calcined body may contain additives as needed. Examples of additives include binders, colorants (including pigments, composite pigments, and fluorescent agents), aluminum oxide (Al2O3), titanium oxide (TiO2), silicon dioxide (SiO2), etc. The additives may be used alone or in combination of two or more.
[0081] Examples of the binder include polyvinyl alcohol, methyl cellulose, carboxymethyl cellulose, acrylic binders, wax binders (paraffin, etc.), polyvinyl butyral, polymethyl methacrylate, ethyl cellulose, polyethylene, polypropylene, ethylene vinyl acetate copolymer, polystyrene, atactic polypropylene, methacrylic resins, and stearic acid.
[0082] Examples of the pigment include oxides of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Pr, Sm, Eu, Gd, Tb, and Er (specifically, NiO, Cr2O3, etc.), preferably oxides of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Pr, Sm, Eu, Gd, and Tb, and more preferably oxides of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Sm, Eu, Gd, and Tb. In addition, the zirconium oxide formed body or zirconium oxide calcined body of the present invention may not contain Er2O3. Examples of the composite pigments include composite oxides such as (Zr, V) O2, Fe(Fe, Cr) 2 O4, (Ni, Co, Fe)(Fe, Cr) 2 O4・ZrSiO4, and (Co, Zn) Al2 O4. Examples of fluorescent agents include Y2 SiO5: Ce, Y2 SiO5: Tb, (Y, Gd, Eu) BO3, Y2 O3: Eu, YAG: Ce, ZnGa2 O4: Zn, BaMgAl 10 O 17 :Eu et al.
[0083] The method for producing the zirconia formed body used in the present invention is not particularly limited, and examples thereof include the following production method, which includes: a step of press-forming a mixed powder containing zirconia and the aforementioned stabilizer at a pressure of 175 MPa or more to obtain a zirconia formed body. By press-forming at the aforementioned pressure, the volume density of the zirconia formed body (and thus the obtained zirconia sintered body) can be increased regardless of the thickness. It should be noted that in this specification, the aforementioned pressure of 175 MPa or more refers to the maximum pressure during press-forming.
[0084] The method for producing the zirconia calcined body used in the present invention is not particularly limited, and examples thereof include a method for producing a zirconia formed body formed by a raw material powder containing zirconia particles and a stabilizer at a temperature at which the zirconia particles do not reach sintering (i.e., calcining). The zirconia formed body is as described above. An example of the method for producing the zirconia calcined body of the present invention is described. First, a raw material powder for a zirconia formed body is produced. A mixture is prepared using a monoclinic zirconia powder and a stabilizer powder (e.g., yttrium oxide powder) to achieve a desired content of the stabilizer (e.g., yttrium oxide). Next, the mixture is added to water to produce a slurry, and wet pulverized and mixed using a ball mill until the desired particle size is reached. The pulverized slurry is dried and granulated using a spray dryer. The obtained powder is calcined at a temperature at which the zirconia particles do not reach sintering (e.g., 800 to 1200°C) to produce a powder (primary powder). Pigments may be added to the primary powder. Afterwards, the primary powder is added to water to prepare a slurry, and wet crushing and mixing is performed using a ball mill until the desired particle size is reached. After adding additives such as a binder to the crushed slurry as needed, it is dried using a spray dryer to prepare a mixed powder (secondary powder). The secondary powder is filled into a specified mold, the upper surface is smoothed to make it flat, an upper mold is set, and the secondary powder is press-formed using a uniaxial press molding machine to obtain a zirconia molded body. As described above, the pressure when the mixed powder is press-formed is preferably above 175 MPa. It should be noted that the obtained zirconia molded body may or may not be further CIP (Cold Isostatic Press) formed.
[0085] The zirconia calcined body may have a multilayer structure. When manufacturing a zirconia calcined body having a multilayer structure, the primary powder may be divided into at least 2 parts (preferably 4 parts) in the above-mentioned manufacturing method in order to make the zirconia formed body into a multilayer structure.
[0086] Next, the zirconia formed body obtained as above is pre-sintered to obtain a zirconia formed body. The pre-sintering temperature is, for example, preferably 800°C or higher, more preferably 900°C or higher, and further preferably 950°C or higher. In order to improve dimensional accuracy, the pre-sintering temperature is, for example, preferably 1200°C or lower, more preferably 1150°C or lower, and further preferably 1100°C or lower. This is because it is considered that at such a pre-sintering temperature, the stabilizer will not be dissolved.
[0087] As the zirconia calcined body used in the present invention, a commercial product can be used. As a commercial product, a zirconia calcined body containing yttria as a stabilizer, such as "Norita Kekatana (registered trademark) zirconia" (model: Desque UTML, Desque STML, Desque ML, Desque HT, Desque LT) (the above are manufactured by Kuraray Norita Kedental Co., Ltd.) can be cited. In the method for producing a zirconia sintered body of the present invention, it is preferred to use the above-mentioned commercially available zirconia calcined body after cutting into a predetermined shape of a dental product.
[0088] In the method for manufacturing a zirconia sintered body of the present invention, as long as the starting temperature, the reaching temperature, the range of the heating rate, the relationship of HR1>HR2, and HR2 / HR3>1 of each heating process described above are satisfied, the heating rate of each heating process described above may be a constant rate, or may be changed in the middle and set to multiple stages. For example, in a certain embodiment, for the second heating process, the temperature may be increased at 150°C / min for 30 seconds from the starting temperature, and after 30 seconds, the temperature may be increased at 80°C / min. In other embodiments, for the third heating process, the temperature may be increased at 60°C / min for 30 seconds from the starting temperature, and after 30 seconds, the temperature may be increased at 20°C / min.
[0089] [Stop process]
[0090] In the method for producing a zirconia sintered body of the present invention, the residence time at the maximum sintering temperature is preferably within 15 minutes, and from the viewpoint that the working time can be further shortened and the strength of the obtained zirconia sintered body is excellent, it is more preferably 1 to 15 minutes, and more preferably 5 to 15 minutes. In addition, as a suitable embodiment, the maximum sintering temperature is 1400 to 1650°C, and from the viewpoint that the brightness, light transmittance and chroma of the obtained zirconia sintered body are more excellent, and the color rendering of the composite oxide contained in the zirconia formed body or the zirconia calcined body is excellent, it is preferably 1450°C or more, more preferably 1500°C or more, and more preferably 1520°C or more. In addition, from the viewpoint that the working time can be further shortened, the brightness, light transmittance and chroma of the obtained zirconia sintered body are more excellent, and the color rendering of the composite oxide contained in the zirconia formed body or the zirconia calcined body is excellent, the maximum sintering temperature is preferably 1630°C or less, more preferably 1620°C or less, and more preferably 1610°C or less. The dwelling step is preferably performed immediately after the third temperature rising step, but as long as the effect of the present invention is exerted, another temperature rising step may be further provided between the third temperature rising step and the dwelling step. In an embodiment not including temperature rising steps other than the above, the reaching temperature of H3 becomes the highest firing temperature.
[0091] From the viewpoint of further shortening the working time, the total calcination time from the start of the temperature increase in the first temperature increase step in the calcination step to the end of the residence time at the maximum calcination temperature is preferably within 50 minutes, more preferably within 45 minutes, and even more preferably within 40 minutes.
[0092] [Cooling process]
[0093] The method for manufacturing a zirconia sintered body of the present invention preferably includes a step of cooling after maintaining the above-mentioned maximum sintering temperature for a specified time. In the cooling step, the cooling rate from the maximum sintering temperature for obtaining the zirconia sintered body to 1100°C is preferably 10°C / min or more, more preferably 30°C / min or more, and further preferably 50°C / min or more. The cooling method may use any one of external air introduction cooling, water cooling, air cooling, slow cooling, and natural cooling, or a combination thereof. The reaching temperature of the cooling step varies depending on the type and performance of the sintering furnace, and may be 1300°C, 1050°C, or 1000°C.
[0094] From the perspective of suitability as a dental product, the color difference ΔE*ab of the zirconium oxide sintered body obtained by the manufacturing method of the present invention is preferably 2.7 or less, more preferably 2.0 or less, further preferably 1.6 or less, and particularly preferably 0.8 or less. The comparative measurement object of the color difference ΔE*ab is the hue of the zirconium oxide sintered body during normal firing (total firing time: 6 to 12 hours). The evaluation method of the hue is described in the examples described below.
[0095] From the aspect of suitability as a dental product, the difference between the lightness index L* of the zirconia sintered body obtained by the manufacturing method of the present invention and the lightness index L* of the zirconia sintered body during normal firing (total firing time: 6 to 12 hours) is preferably 2.0 or less, more preferably 1.5 or less, and further preferably 1.0 or less. L*, a* and b* of the zirconia sintered body obtained by the manufacturing method of the present invention can be selected and set according to the target part such as the cervical part (tooth neck part) and the incisal part (incisal part).
[0096] The present invention includes various embodiments in which the above-described configurations are combined within the technical concept of the present invention within the scope in which the effects of the present invention are exhibited. Example
[0097] Next, the present invention will be described in more detail with reference to examples. However, the present invention is not limited to these examples at all, and a person having common knowledge in the art can make various modifications within the scope of the technical idea of the present invention.
[0098] [Example 1]
[0099] Ten rectangular samples of 1.7 mm × 5.2 mm × 20.2 mm cut from a "Nori Ta Kekatana (registered trademark) Zirconia" STML A1 color zirconia disc workpiece (manufactured by Kura Norita Kedentar Co., Ltd.) were prepared using DWX51D (manufactured by Roland DG Co., Ltd.). As a firing furnace, Programat (registered trademark) CS4 (manufactured by Ibo Cura Biparton Co., Ltd.) was used to fire the samples under the firing schedule conditions shown in Table 1. The samples were fired under the conditions that the total firing time from the start of the first heating step to the end of the residence time at the maximum firing temperature was within 50 minutes to obtain a zirconia sintered body.
[0100] [Measurement of three-point bending strength]
[0101] For the zirconia sintered body obtained by firing, a rotating grinding disc and #1000 grinding paper were used to grind it to make a sintered body sample in the shape of a rectangular parallelepiped of 1.2 mm × 4 mm × 16 mm. Using this sintered body sample, the three-point bending strength was measured under the conditions of a crosshead speed of 0.5 mm / min and a distance (span) between fulcrums of 14 mm in accordance with ISO6872:2015. In addition, in order to confirm the three-point bending strength of the sintered body sample when fired under the previous firing schedule, Norita Kekatana (registered trademark) F1-N (manufactured by Kuraray Norita Kedentar Co., Ltd.) was used as a firing furnace, and under the firing schedule shown in Table 6, the three-point bending strength of the sintered body sample was measured in the same manner as the above method. As shown in Table 7, the three-point bending strength of the sintered body sample of Example 1 showed a value equivalent to that of the case where the sintering was performed under the conventional sintering schedule, and it was confirmed that the strength was sufficient for dental use.
[0102]
[0103] [Measurement of lightness, chroma and color difference]
[0104] Next, a dental crown shape was cut out from the same zirconia disk workpiece as that used in the three-point bending strength measurement using DWX51D, and samples of the same shape were fired under the conventional firing schedule (Table 6) using the Norita Kekatana (registered trademark) F1-N as the firing furnace and the firing schedule described in Table 1 using the Programat (registered trademark) CS4 as the firing furnace. The fired sintered body samples were colorimetrically measured using a dental colorimetric device (manufactured by Orinpass, 7-band LED light source, "Crystal Ai" (manufactured by Orinpass)) to evaluate the lightness, chroma, and color difference ΔE*ab (n=5) in the L*a*b* colorimetric system (JIS Z8781-4:2013 Colorimetry-Part 4: CIE 1976 L*a*b* color space). The average value of n=5 is shown as the evaluation result in Table 8. The color difference ΔE*ab refers to the color difference ΔE* (ΔE*ab) obtained by using the lightness index L* in the CIE 1976 L*a*b* color space, the color coordinates a*, b*, and the sintered body sample obtained under the firing schedule described in Table 6 (L1*, a1*, b1*) and the sintered body sample obtained under the firing schedule described in Table 1 (L2*, a2*, b2*) using the following formula (3).
[0105] [Mathematical formula 3]
[0106]
[0107] As shown in Table 8, it was confirmed that the color difference ΔE*ab between the sintered body sample sintered under the sintering schedule in Table 1 and the sintered body sample sintered under the conventional sintering schedule described in Table 6 was 2.7 or less.
[0108] [Example 2]
[0109] The three-point bending strength and color difference ΔE*ab were measured by the same method as in Example 1 except that the firing schedule was set to the schedule described in Table 2. As shown in Table 7, the three-point bending strength of Example 2 showed the same value as when fired under the conventional firing schedule described in Table 6, and it was confirmed that it was a strength that was not a problem for dental products. In addition, as shown in Table 8, it was confirmed that the color difference ΔE*ab of the sintered body sample fired under the firing schedule described in Table 2 was 2.7 or less compared with the sintered body sample fired under the conventional firing schedule described in Table 6.
[0110]
[0111] [Example 3]
[0112] The three-point bending strength and color difference ΔE*ab were measured by the same method as in Example 1 except that SINTERMAT1600 (manufactured by The Dental Solution, Inc.) was used as a firing furnace and the firing schedule was set to the firing schedule described in Table 3. As shown in Table 7, the three-point bending strength of Example 3 showed the same value as that when fired under the conventional firing schedule shown in Table 6, and it was confirmed that it was a strength that was not a problem for dental products. In addition, as shown in Table 8, it was confirmed that the color difference ΔE*ab of the sintered body sample fired under the firing schedule of Table 3 was 2.7 or less compared with the sintered body sample fired under the conventional firing schedule.
[0113]
[0114] [Comparative Examples 1 and 2]
[0115] SINTERMAT1600 (manufactured by The Dental Solution, Inc.) was used as a firing furnace, and the firing schedule was set to the firing schedule described in Tables 4 and 5. In addition, the three-point bending strength and color difference △E*ab were measured using the same method as in Example 1. As shown in Table 7, the three-point bending strength of the comparative example showed the same value as when fired under the previous firing schedule shown in Table 6, and it can be confirmed that it is a strength that is not a problem for dental products. However, as shown in Table 8, the color difference △E*ab of the sintered body samples fired under the firing schedules of Table 4 (Comparative Example 1) and Table 5 (Comparative Example 2) compared with the sintered body samples fired under the previous firing schedule described in Table 6 exceeded 2.7, and the hue equivalent to the previous firing schedule could not be obtained. In addition, an increase in brightness was observed in the zirconia sintered bodies of Comparative Examples 1 and 2.
[0116]
[0117]
[0118]
[0119]
[0120]
[0121] Furthermore, it can be confirmed by visual observation that the zirconia sintered bodies of Examples 1 to 3 have the same appropriate light transmittance as the case of normal sintering (total sintering time: 6 to 12 hours) despite the short total sintering time of less than 50 minutes. From the above results, it can be confirmed that the zirconia sintered bodies obtained by the production method of the present invention have excellent strength, can suppress the increase of lightness, show appropriate light transmittance, and have excellent hue, and are suitable as dental products (such as dental prostheses).
[0122] Industrial Applicability
[0123] The method for producing a zirconia sintered body of the present invention can sinter a zirconia formed body or a zirconia calcined body in a short time, and the obtained zirconia sintered body can reproduce the aesthetic requirements (color and light transmittance) and strength of an ideal dental prosthesis to the same extent as in the case of conventional sintering (total sintering time: 6 to 12 hours), and is therefore useful in the production of dental products (dental prostheses, etc.). In particular, the zirconia sintered body is excellent in color and has light transmittance like the incisal edge of a natural tooth, and is therefore useful in the production of dental prostheses such as attached dentures.
Claims
1. A method for producing a zirconia sintered body, comprising a firing step of firing a zirconia formed body or a zirconia calcined body, The sintering process includes at least three stages of heating processes, namely, a first heating process H1, a second heating process H2 and a third heating process H3. The temperature increase rate in the first temperature increase step H1 is denoted as HR1. The temperature increase rate in the second temperature increase step H2 is denoted as HR2. When the temperature increase rate of the third temperature increase step H3 is denoted as HR3, HR1=70~500℃ / min、 HR2 = 20 ~ 300 ° C / min, HR3 = 10 ~ 299 ° C / min, HR1>HR2, HR2 / HR3>1, Regarding the starting temperature in each heating step, In H1, the temperature is from room temperature to 500°C. 900~1250℃ in H2 In H3, it is 1300~1550℃, Regarding the reaching temperature in each heating step, In H1, 900~1250℃, 1300~1550℃ in H2 In H3, it is 1400~1650℃, The zirconia formed body or zirconia calcined body contains 2 to 8 mol% of a stabilizer, The stabilizer is yttrium oxide.
2. The method for producing a zirconia sintered body according to claim 1, wherein: HR2 is 20~280℃ / min.
3. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: HR3 is 13~250℃ / min.
4. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: HR2 / HR3>1.
2.
5. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: HR2 / HR3>1.
5.
6. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: The maximum calcination temperature in the temperature raising step is 1400 to 1650° C., and the residence time at the maximum calcination temperature is within 15 minutes.
7. The method for producing a zirconia sintered body according to claim 1 or 2, comprising: A temperature reduction step in which the temperature is reduced from the highest sintering temperature in the temperature increase step to 1100°C at a temperature reduction rate of 10°C / min or more.
8. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: The total calcination time from the start of the temperature increase in the first temperature increase step H1 in the calcination step to the end of the residence time at the maximum calcination temperature is within 50 minutes.
9. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: More than 55% of the calcined zirconium oxide is monoclinic.
10. The method for producing a zirconia sintered body according to claim 1, wherein: In the zirconia formed body or the zirconia calcined body, at least a part of the stabilizer is not solid-dissolved in the zirconia.
11. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: The zirconia formed body or zirconia calcined body has a predetermined shape of a dental product.
12. The method for producing a zirconia sintered body according to claim 11, wherein: Dental products are dental prostheses.
13. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: HR1 / HR2>1.
5.
14. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: It further includes a stay process, and the first temperature rising process H1, the second temperature rising process H2, the third temperature rising process H3 and the stay process are all performed continuously.