Modified ABS rubber powder and preparation method thereof, ABS resin and vehicle interior decoration parts
By introducing residual monomer adsorbent and titanium dioxide modified with transition metal elements into ABS powder, the problem of high residual monomer content in ABS powder is solved, resulting in modified ABS powder with low odor and low emission, which is suitable for vehicle interior parts.
Patent Information
- Application Number
- CN202310527469.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-10
AI Technical Summary
The high residual content in existing ABS adhesive powder leads to excessive odor and VOC levels, making it difficult to meet the requirements for low odor and low emission in vehicle interior parts.
Modified ABS powder was prepared by using residual monomer adsorbent and titanium dioxide modified with transition metal elements, through a combination of physical adsorption and chemical decomposition to reduce the residual monomer content.
Significantly reduces the residual content of modified ABS powder, achieving low odor and low emission, meeting the odor and VOC requirements of vehicle interior parts, and broadening application performance.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of engineering plastics, and in particular to modified ABS rubber powder and a preparation method thereof, ABS resin and vehicle interior decoration parts. Background Art
[0002] As the automotive industry continues to improve its requirements for vehicle interior air quality, more and more automakers are paying special attention to the impact of in-vehicle odor and VOC (volatile organic compounds, the main components of which are benzene, alkanes, aldehydes, ketones, and mercaptans) on the comfort of drivers and passengers. For example, some automakers require that vehicle interior parts must meet the requirements of odor test less than or equal to level 3.5 and VOC less than 50g / L. Therefore, materials with low odor and low emission will inevitably become the key materials for vehicle interior parts.
[0003] ABS resin refers to acrylonitrile-butadiene-styrene copolymer, which is an important thermoplastic polymer material with wide application prospects in vehicle interior parts. ABS resin can be flexibly adjusted by blending ABS rubber powder with SAN resin to expand the application space and breadth of ABS resin. However, ABS rubber powder generally contains more residual monomers, odor and VOC are higher. Summary of the invention
[0004] Based on this, the present invention provides a modified ABS rubber powder and a preparation method thereof, ABS resin and a vehicle interior decoration part.
[0005] The first aspect of the present invention provides a modified ABS rubber powder, and the technical solution thereof is as follows:
[0006] A modified ABS rubber powder, wherein the modified ABS rubber powder contains a residual single adsorbent and titanium dioxide doped with a transition metal element;
[0007] The residual monomer adsorbent includes diatomaceous earth, molecular sieve, porous silicate or a combination thereof.
[0008] In some embodiments, the transition metal element is palladium, platinum or a combination thereof.
[0009] In some of the embodiments, in the transition metal element doped modified titanium dioxide, the molar ratio of the transition metal element to the titanium element is 1:(1-5).
[0010] In some embodiments, one or more of the following conditions are met:
[0011] 1) The residual adsorbent accounts for 0.2wt% to 1.5wt% of the modified ABS rubber powder;
[0012] 2) The transition metal element doped modified titanium dioxide accounts for 0.2wt% to 1.5wt% of the modified ABS rubber powder; and
[0013] 3) The content of polybutadiene in the modified ABS rubber powder is 50wt% to 70wt%;
[0014] 4) The content of acrylonitrile-styrene copolymer in the modified ABS rubber powder is 27wt% to 49.6wt%; the polymerization monomers of the acrylonitrile-styrene copolymer include acrylonitrile monomer and styrene monomer in a weight ratio of (50-150):(250-350).
[0015] The second aspect of the present invention provides a method for preparing modified ABS rubber powder, and its technical scheme is as follows:
[0016] Mixing butadiene latex, acrylonitrile monomer and styrene monomer, performing emulsion graft copolymerization reaction to obtain grafted latex, and flocculating the grafted latex to prepare flocculated slurry;
[0017] Mixing the washing liquid and the flocculated slurry, collecting the solid and drying it to prepare modified ABS rubber powder;
[0018] The washing liquid comprises a residual single adsorbent and titanium dioxide doped and modified by transition metal elements;
[0019] The residual monomer adsorbent includes diatomaceous earth, molecular sieve, porous silicate or a combination thereof.
[0020] In some embodiments, the method for preparing the washing solution comprises the following steps:
[0021] Using tetrabutyl titanate as a precursor and transition metal salt as a doping source, a transition metal element-doped titanium dioxide gel was prepared by a sol-gel method.
[0022] The transition metal element doped modified titanium dioxide gel, residual adsorbent and washing solvent are mixed to prepare a washing liquid.
[0023] In some embodiments, the method for preparing the washing solution satisfies one or more of the following conditions:
[0024] 1) The transition metal salt is a palladium salt, a platinum salt or a combination thereof;
[0025] 2) The molar ratio of the transition metal salt to the tetrabutyl titanate is 1:(1-5).
[0026] In some embodiments, the concentration of the residual adsorbent in the washing liquid is 0.5wt% to 1wt%; and / or
[0027] The concentration of the titanium dioxide doped with transition metal elements in the washing liquid is 0.5 wt % to 1 wt %.
[0028] In some embodiments, the volume ratio of the washing liquid to the flocculation slurry is 1:(1.5-2.5).
[0029] In some embodiments, one or more of the following conditions are met:
[0030] 1) The butadiene latex is prepared by emulsion polymerization of butadiene monomer;
[0031] 2) controlling the weight of the butadiene latex so that the content of polybutadiene in the modified ABS rubber powder is 50wt% to 70wt%;
[0032] 3) controlling the weight of the acrylonitrile monomer and the styrene monomer so that the content of the acrylonitrile-styrene copolymer in the modified ABS rubber powder is 27wt% to 49.6wt%, and the weight ratio of the acrylonitrile monomer to the styrene monomer is (50 to 150):(250 to 350);
[0033] 4) The chain transfer agent used in the emulsion graft copolymerization reaction is α-methylstyrene dimer
[0034] 5) The initiator used in the emulsion graft copolymerization reaction is selected from one or more of cumene hydroperoxide, sodium persulfate, potassium persulfate, ammonium persulfate and azobisisobutylnitrile;
[0035] 6) the emulsifier used in the emulsion graft copolymerization reaction is selected from one or more of sodium salt of pernaphthalenesulfonic acid formaldehyde condensate, potassium salt of naphthalenesulfonic acid formaldehyde condensate, potassium oleate, potassium stearate, potassium disproportionated rosin acid, sodium dodecylbenzene sulfonate and sodium dodecyl sulfonate;
[0036] 7) The reducing agent used in the emulsion graft copolymerization reaction is selected from one or more of sodium ethylenediaminetetraacetate, ferrous sulfate, glucose, sodium pyrophosphate and sodium sulfite;
[0037] 8) The solvent used in the emulsion graft copolymerization reaction is water; and
[0038] 9) The flocculant used in the flocculation treatment is one or more selected from magnesium sulfate, sulfuric acid and calcium chloride.
[0039] The third aspect of the present invention provides an ABS resin, and its technical solution is as follows:
[0040] An ABS resin, whose components include the modified ABS rubber powder or the modified ABS rubber powder prepared by the above preparation method, and SAN resin.
[0041] A fourth aspect of the present invention provides a vehicle interior decoration component, and its technical solution is as follows:
[0042] A vehicle interior trim part, the components of which include the modified ABS rubber powder, the modified ABS rubber powder prepared by the preparation method or the ABS resin.
[0043] Compared with the traditional solution, the present invention has the following beneficial effects:
[0044] The modified ABS rubber powder of the present invention comprises a residual monophenyl adsorbent and titanium dioxide modified by doping with transition metal elements, wherein the residual monophenyl adsorbent comprises diatomaceous earth, molecular sieve, porous silicate or a combination thereof, and the residual monophenyl in the modified ABS rubber powder can be physically adsorbed by the residual monophenyl adsorbent, and at the same time, the titanium dioxide modified by doping with transition elements can continuously decompose the residual monophenyl adsorbed by the residual monophenyl adsorbent, so that the residual monophenyl content of the modified ABS rubber powder of the present invention is reduced, and the modified ABS rubber powder has the properties of low odor and low emission. After being mixed with SAN resin, it is conducive to achieving the low odor, low emission and wider application performance of ABS resin. DETAILED DESCRIPTION
[0045] The present invention will be further described in detail below in conjunction with specific embodiments. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.
[0046] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0047] the term
[0048] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0049] In the present invention, "plurality", "multiple", "multiple times", "multiple" and the like, unless otherwise specified, refer to a number greater than or equal to 2. For example, "one or more" means one or greater than or equal to two.
[0050] In the present invention, “preferred”, “better”, “more preferred” and “suitable” are only used to describe implementation methods or examples with better effects, and it should be understood that they do not constitute limitations on the scope of protection of the present invention.
[0051] In the present invention, the words “further”, “furthermore”, “particularly”, etc. are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present invention.
[0052] In the present invention, "optionally", "optional" and "optional" refer to optional, that is, to any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.
[0053] In the present invention, in the "first aspect", "second aspect", "third aspect", "fourth aspect", etc., the terms "first", "second", "third", "fourth", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0054] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0055] In the present invention, when it comes to numerical intervals (i.e., numerical ranges), unless otherwise specified, the optional numerical distribution is considered continuous within the above numerical interval, and includes the two numerical endpoints (i.e., the minimum value and the maximum value) of the numerical range, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to the integers within the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints. In this article, it is equivalent to directly listing each integer, such as t is an integer selected from 1 to 10, indicating that t is any integer selected from the group of integers consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9 and 10. In addition, when multiple ranges are provided to describe features or characteristics, these ranges can be combined. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all sub-ranges included therein.
[0056] The temperature parameters in the present invention, if not specifically limited, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.
[0057] In the present invention, when it comes to percentage concentration, unless otherwise specified, it refers to the final concentration. The final concentration refers to the proportion of the added component in the system after the addition of the component.
[0058] In the present invention, wt% means weight percentage, and wt‰ means weight thousandth.
[0059] In the present invention, the proportion of the residual single adsorbent and the transition metal element doped modified titanium dioxide in the modified ABS rubber powder is measured by the following method:
[0060] Take 5g of ABS rubber powder and test the ash content of ABS rubber powder according to GB / T 9345-2008 standard. Specifically, calcine in a muffle furnace at 850℃ for 30min. Measure the total ash content, and then calculate the ash content w.
[0061] The content of Ti and transition metal elements in the ash was tested by inductively coupled plasma optical emission spectrometry (ICP-OES) according to the GB / T 30902-2014 method. Combined with the molecular weight of TiO2, the content w1 of TiO2 doped with transition metal elements was calculated.
[0062] The content of residual adsorbent w2 = w-w1.
[0063] One embodiment of the present invention provides a modified ABS rubber powder, wherein the modified ABS rubber powder contains a residual adsorbent and titanium dioxide modified by doping with transition metal elements, wherein the residual adsorbent includes diatomaceous earth, molecular sieve, porous silicate or a combination thereof.
[0064] The modified ABS rubber powder of this embodiment includes a residual monolactic adsorbent and titanium dioxide modified by doping with transition metal elements, wherein the residual monolactic adsorbent includes diatomaceous earth, molecular sieve, porous silicate or a combination thereof. The residual monolactic adsorbent can physically adsorb the residual monolactic in the modified ABS rubber powder. At the same time, the titanium dioxide modified by doping with transition elements can continuously decompose the residual monolactic adsorbent adsorbed by the residual monolactic adsorbent. Since the decomposition of the residual monolactic by titanium dioxide takes time, after the residual monolactic is physically adsorbed by the residual monolactic adsorbent, more time is provided for the decomposition of titanium dioxide, thereby promoting more residual monolactic decomposition by titanium dioxide. The residual monolactic content of the modified ABS rubber powder of this embodiment is reduced, and it has the properties of low odor and low emission. After being mixed with SAN resin, it is conducive to achieving the low odor, low emission and wider application performance of ABS resin.
[0065] Optionally, the modified ABS rubber powder includes polybutadiene and acrylonitrile-styrene copolymer.
[0066] Optionally, the modified ABS rubber powder can be a modified ABS high-rubber powder or a modified ABS low-rubber powder. Preferably, the modified ABS rubber powder is a modified ABS high-rubber powder, and the polybutadiene content is 50wt% to 70wt%.
[0067] In this embodiment, the modified ABS rubber powder can be prepared by an emulsion method, and the polybutadiene content of the modified ABS rubber powder can reach 50wt% to 70wt% by the emulsion method. By dispersing the above-mentioned residual monobutylene adsorbent and the titanium dioxide modified by doping with transition metal elements, the residual monobutylene in the modified ABS high rubber powder can be reduced, thereby reducing the odor and VOC emission of the product.
[0068] Optionally, the content of acrylonitrile-styrene copolymer in the modified ABS rubber powder is 27wt% to 49.6wt%; the polymerization monomers of the acrylonitrile-styrene copolymer include acrylonitrile monomer and styrene monomer in a weight ratio of (50-150):(250-350).
[0069] In this embodiment, the residual monol adsorbent can effectively adsorb small molecules of residual monol by physical adsorption, thereby reducing residual monol, odor and VOC.
[0070] Optionally, the residual adsorbent accounts for 0.2wt% to 1.5wt% of the modified ABS rubber powder.
[0071] The diatomaceous earth in this embodiment has a porous structure and can effectively adsorb residual small molecules through physical adsorption.
[0072] Different from merely adding a residual monocarbonate adsorbent for adsorption, this embodiment adds titanium dioxide doped with transition metal elements to continuously decompose the residual monocarbonate adsorbed by the residual monocarbonate adsorbent, thereby preventing the adsorbed residual monocarbonate from being released and diffused during subsequent injection molding, extrusion or melt processing, causing odor or VOC to exceed the standard in subsequent steps.
[0073] In this embodiment, the titanium dioxide doped and modified by transition metal elements has the function of decomposing residues. It can not only play the role of decomposing residues under the action of light, but also play the role of decomposing residues under the action of heat separated from light by doping and modifying the titanium dioxide with transition metal elements.
[0074] Optionally, the transition metal element is palladium, platinum or a combination thereof.
[0075] Optionally, in the transition metal element-doped modified titanium dioxide, the molar ratio of the transition metal element to the titanium element is 1:(1-5).
[0076] Optionally, the transition metal element-doped modified titanium dioxide accounts for 0.2 wt% to 1.5 wt% of the modified ABS rubber powder.
[0077] Generally speaking, ABS resin can be prepared by emulsion method or bulk method. The emulsion method adds more additives during the synthesis process. Therefore, compared with the ABS resin obtained by the bulk method, the amount of residual singlet obtained by the emulsion method is relatively more, and the odor and VOC are larger. Therefore, the ABS resin produced by the bulk method is more commonly used. However, due to the limitations of the bulk method itself, the glue content in the ABS resin product obtained is limited and relatively fixed. It is difficult to obtain ABS resin with a high glue content. It performs poorly in coating performance, and the flexibility of ingredients and modification space are relatively small. Therefore, in the production of ABS resin materials for some vehicle interior parts, the emulsion method is still used. As a result, how to reduce the residual singlet of the emulsion method has become an important research topic.
[0078] By blending ABS rubber powder with SAN resin, the content of acrylonitrile, butadiene and styrene can be flexibly adjusted, and there is a large room for modification. Among them, ABS rubber powder can be prepared by emulsion method to obtain ABS rubber powder with flexible polybutadiene content.
[0079] In one embodiment of the present invention, a method for preparing a modified ABS rubber powder is provided, comprising the following steps:
[0080] Mixing butadiene latex, acrylonitrile monomer and styrene monomer, performing emulsion graft copolymerization reaction to obtain grafted latex, and flocculating the grafted latex to prepare flocculated slurry;
[0081] Mixing the washing liquid and the flocculated slurry, collecting the solid and drying it to prepare modified ABS rubber powder;
[0082] The washing liquid comprises a residual single adsorbent and titanium dioxide doped and modified by transition metal elements;
[0083] The residual monomer adsorbent includes diatomaceous earth, molecular sieve, porous silicate or a combination thereof.
[0084] In this embodiment, the modified ABS rubber powder is prepared by an emulsion method, wherein butadiene latex, acrylonitrile monomer and styrene monomer are subjected to an emulsion graft copolymerization reaction in the presence of a reducing agent, an emulsifier, an initiator, a chain transfer agent and a solvent to obtain a grafted latex.
[0085] Optionally, the butadiene latex is prepared by emulsion polymerization of butadiene monomer.
[0086] Optionally, butadiene monomer is subjected to emulsion polymerization in the presence of an electrolyte, an initiator, an emulsifier and a chain transfer agent to obtain butadiene latex.
[0087] Optionally, the reaction time of the emulsion polymerization reaction is 20 h to 40 h, and the reaction temperature is 51° C. to 93° C.
[0088] In some examples, the method for preparing the butadiene latex comprises the following steps:
[0089] The butadiene monomer, electrolyte, initiator, emulsifier and chain transfer agent are mixed, and the temperature of the obtained mixed system is raised from 51° C. to 61° C. to 83° C. to 93° C. within 20 h to 40 h.
[0090] Optionally, the initiator used in the emulsion polymerization is selected from one or more of cumene hydroperoxide, sodium persulfate, potassium persulfate, ammonium persulfate and azobisisobutylnitrile.
[0091] Optionally, the initiator accounts for 0.2 wt% to 1.5 wt% of the butadiene monomer.
[0092] Optionally, the electrolyte used in the emulsion polymerization is selected from one or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, potassium carbonate and potassium hydroxide.
[0093] Optionally, the electrolyte accounts for 2 wt% to 15 wt% of the butadiene monomer.
[0094] Optionally, the emulsifier used in the emulsion polymerization is selected from one or more of naphthalenesulfonic acid formaldehyde condensate sodium salt, naphthalenesulfonic acid formaldehyde condensate potassium salt, potassium oleate, potassium stearate, potassium disproportionated rosin acid, sodium dodecylbenzene sulfonate and sodium dodecyl sulfonate.
[0095] Optionally, the emulsifier accounts for 2 wt% to 15 wt% of the butadiene monomer.
[0096] Optionally, the chain transfer agent used in the emulsion polymerization is one or more selected from tert-dodecyl mercaptan, n-dodecyl mercaptan, tetradecyl mercaptan, tridecyl mercaptan, undecyl mercaptan and decanyl mercaptan.
[0097] Optionally, the chain transfer agent accounts for 0.5 wt% to 5 wt% of the butadiene monomer.
[0098] Optionally, the reaction time of the emulsion graft copolymerization reaction is 5 h to 9 h, and the reaction temperature is 10° C. to 72° C.
[0099] In some examples, the method for preparing the grafted latex comprises the following steps:
[0100] Mix butadiene latex and reducing agent, heat the obtained mixed system to 62°C to 72°C, add acrylonitrile monomer, styrene monomer, emulsifier, initiator, chain transfer agent and solvent, keep warm for 1 to 3 hours, and naturally cool and react for 4 hours to 6 hours.
[0101] Optionally, the weight of butadiene latex is controlled so that the content of polybutadiene in the modified ABS rubber powder is 50wt% to 70wt%.
[0102] Optionally, the solid content of the butadiene latex is 50 wt% to 65 wt%.
[0103] Optionally, the weight of acrylonitrile monomer and styrene monomer is controlled so that the content of acrylonitrile-styrene copolymer in the modified ABS rubber powder is 27wt% to 49.6wt%, and the weight ratio of acrylonitrile monomer to styrene monomer is (50-150):(250-350).
[0104] Optionally, the chain transfer agent used in the emulsion graft copolymerization reaction is α-methylstyrene dimer, which is sulfur-free, odorless, safe and environmentally friendly, and can meet FDA requirements. Compared with the use of tert-dodecyl mercaptan, the odor is much lower.
[0105] Optionally, the chain transfer agent accounts for 0.2 wt‰ to 10 wt‰ of the total amount of the polybutadiene, acrylonitrile monomer and styrene monomer.
[0106] Optionally, the initiator used in the emulsion graft copolymerization reaction is selected from one or more of cumene hydroperoxide, sodium persulfate, potassium persulfate, ammonium persulfate and azobisisobutylnitrile;
[0107] Optionally, the initiator accounts for 1 wt‰ to 10 wt‰ of the total amount of the polybutadiene, acrylonitrile monomer and styrene monomer.
[0108] Optionally, the emulsifier used in the emulsion graft copolymerization reaction is selected from one or more of sodium salt of pernaphthalenesulfonic acid formaldehyde condensate, potassium salt of naphthalenesulfonic acid formaldehyde condensate, potassium oleate, potassium stearate, potassium disproportionated rosin acid, sodium dodecylbenzene sulfonate and sodium dodecyl sulfonate.
[0109] Optionally, the emulsifier accounts for 2 wt‰ to 20 wt‰ of the total amount of the polybutadiene, acrylonitrile monomer and styrene monomer.
[0110] Optionally, the reducing agent used in the emulsion graft copolymerization reaction is selected from one or more of sodium ethylenediaminetetraacetate, ferrous sulfate, glucose, sodium pyrophosphate and sodium sulfite.
[0111] Optionally, the reducing agent accounts for 0.01 wt‰ to 0.05 wt‰ of the total amount of the polybutadiene, acrylonitrile monomer and styrene monomer.
[0112] Optionally, the solvent used in the emulsion graft copolymerization reaction may be water.
[0113] In this embodiment, a flocculant is added to the obtained graft latex to perform a flocculation treatment to prepare a flocculated slurry.
[0114] Optionally, the flocculation treatment time is 2h to 6h, and the reaction temperature is 70°C to 100°C.
[0115] Optionally, the flocculant used in the flocculation treatment is selected from one or more of magnesium sulfate, sulfuric acid and calcium chloride.
[0116] Optionally, the weight ratio of the grafted latex to the flocculant is 1000:(40-50).
[0117] It can be understood that the flocculant is added to the graft latex in the form of an aqueous solution of the flocculant.
[0118] In some examples, the method for preparing the flocculated slurry comprises the following steps:
[0119] The grafted latex is heated to 70°C to 80°C, and a flocculant aqueous solution is added, wherein the flocculant aqueous solution is added within 1 hour to 3 hours, and then the temperature is raised to 90°C to 100°C and kept warm for 1 hour to 3 hours.
[0120] Optionally, in the aqueous flocculant solution, the concentration of the flocculant is 0.5 wt% to 5 wt%.
[0121] In this embodiment, the flocculation slurry is washed with a washing liquid containing residual single adsorbent and titanium dioxide doped with transition metal elements. Through this washing treatment, the residual single adsorbent and the titanium dioxide doped with transition metal elements can be fully dispersed in the modified ABS rubber powder. In the inventor's experiment, many methods of mixing residual single adsorbent and titanium dioxide doped with transition metal elements into ABS rubber powder were studied. Through experimental verification, it was found that adding the two to the washing liquid and mixing the washing liquid into the flocculation slurry is beneficial to the dispersion of the two in the modified ABS rubber powder. The better the dispersion effect of the residual single adsorbent and the titanium dioxide doped with transition metal elements in the modified ABS rubber powder, the better the effect of reducing odor and VOC. Through the method of this embodiment, a modified ABS rubber powder with low odor and low emission can be prepared.
[0122] Optionally, the method for preparing the washing liquid comprises the following steps:
[0123] Using tetrabutyl titanate as a precursor and transition metal salt as a doping source, a transition metal element-doped titanium dioxide gel was prepared by a sol-gel method.
[0124] The transition metal element doped modified titanium dioxide gel, residual adsorbent and washing solvent are mixed to prepare a washing liquid.
[0125] In this embodiment, the transition metal element doped and modified titanium dioxide gel prepared by the sol-gel method contains transition metal element doped and modified titanium dioxide. After mixing it with the residual monosorbent adsorbent and the washing solvent, the gel is diluted and can be used as a washing liquid. The washing liquid contains the residual monosorbent adsorbent, the transition metal element doped and modified titanium dioxide and the washing solvent.
[0126] Further optionally, using tetrabutyl titanate as a precursor and a transition metal salt as a doping source, preparing a transition metal element-doped titanium dioxide gel by a sol-gel method comprises the following steps:
[0127] Mix hydrochloric acid, transition metal salt and ethanol, add tetrabutyl titanate, and then add water to adjust the pH value to 3-4.
[0128] Further optionally, the transition metal salt is a palladium salt, a platinum salt or a combination thereof, such as palladium chloride PdCl2, H2PtCl6.
[0129] Further optionally, the molar ratio of the transition metal salt to the tetrabutyl titanate is 1:(1-5).
[0130] In this embodiment, the transition metal element doped modified titanium dioxide gel, the residual mono adsorbent and the washing solvent are mixed. Optionally, the concentration of the residual mono adsorbent in the washing liquid is 0.5wt% to 1wt%. Optionally, the concentration of the transition metal element doped modified titanium dioxide in the washing liquid is 0.5wt% to 1wt%. Optionally, the washing solvent can be water.
[0131] In this embodiment, the residual single adsorbent is as described above and will not be described again here.
[0132] In this embodiment, the flocculation slurry is washed by mixing a washing liquid with the flocculation slurry. Optionally, the flow ratio of the washing liquid to the flocculation slurry is 1:(1.5-2.5). Optionally, the washing time is 20 min-40 min. After washing, the solid can be collected by centrifugation, filtration, etc., and the solid can be dried to obtain modified ABS rubber powder.
[0133] In this embodiment, the content of the titanium dioxide doped with transition metal elements and the residual adsorbent in the modified ABS rubber powder can be controlled by controlling the concentration of the titanium dioxide doped with transition metal elements and the residual adsorbent in the washing liquid, controlling the flow rate of the washing liquid and the flocculation slurry, and controlling the washing time. However, it is not limited to the above methods.
[0134] Through the preparation method of this embodiment, the proportion of the residual adsorbent in the modified ABS rubber powder is 0.2wt% to 1.5wt%; the proportion of the titanium dioxide doped with transition metal elements in the modified ABS rubber powder is 0.2wt% to 1.5wt%.
[0135] The preparation method of this embodiment requires less modification to the original emulsion production line, has less impact on the production cycle and energy consumption, and is conducive to continuous large-scale production.
[0136] In one embodiment of the present invention, an ABS resin is provided, which includes the modified ABS rubber powder or the modified ABS rubber powder prepared by the above preparation method, and SAN resin.
[0137] Optionally, the amount of modified ABS rubber powder and SAN resin added can be adjusted according to actual use requirements. In some embodiments, the weight ratio of modified ABS rubber powder to SAN resin can be (15-35): (65-85).
[0138] It can be understood that the above ABS resin can be prepared by extruding and pelletizing a powder containing modified ABS rubber powder and SAN resin. Optionally, the extrusion temperature is 180°C to 210°C, the screw speed is 200r / min to 300r / min, and the screw aspect ratio is (35 to 45):1.
[0139] In one embodiment of the present invention, a vehicle interior trim is provided, which comprises the modified ABS rubber powder, the modified ABS rubber powder obtained by the preparation method, or the ABS resin.
[0140] The vehicle interior decoration part of this embodiment has low odor and low emission and is widely used.
[0141] The following is further described in conjunction with specific examples and comparative examples. The raw materials involved in the following specific examples and comparative examples, unless otherwise specified, can all be commercially available, the instruments used, unless otherwise specified, can all be commercially available, the processes involved, unless otherwise specified, are routinely selected by those skilled in the art, and the parts involved in the following examples and comparative examples, unless otherwise specified, are all parts by weight.
[0142] Among them, butadiene monomer is industrial grade butadiene with a purity greater than 96%, which comes from Huarui Chemical; styrene monomer has a purity greater than or equal to 99% and comes from Aladdin Reagent Company; acrylonitrile monomer has a purity greater than or equal to 99% and comes from Aladdin Reagent Company; tert-dodecyl mercaptan TDM is a chain transfer agent; α-methylstyrene dimer AMSD is a chain transfer agent; SAN resin is a styrene-acrylonitrile copolymer, brand PN-128, from Chi Mei in Taiwan, China.
[0143] Example 1
[0144] This embodiment provides a modified ABS rubber powder and a preparation method thereof, an ABS resin and a preparation method thereof, and the steps are as follows:
[0145] Step 1: Preparation of butadiene latex
[0146] 100 parts of butadiene monomer, 0.5 parts of sodium persulfate (initiator), 5 parts of sodium carbonate (electrolyte), 5 parts of potassium disproportionate rosin acid (emulsifier) and 2 parts of tert-dodecyl mercaptan (chain transfer agent) were mixed, the temperature was raised to 56°C to start emulsion polymerization, the temperature was continuously raised to 88°C within 30 hours, the reaction was terminated after 30 hours, and a butadiene latex with a particle size of 310 nm and a solid content of 58wt% was obtained.
[0147] Step 2: Preparation of flocculation slurry
[0148] Add butadiene latex containing 600 parts of polybutadiene into a reactor, add 0.015 parts of ferrous sulfate into the reactor and stir evenly, heat the reactor to 67°C, add 2.51 parts of cumene hydroperoxide, 100 parts of acrylonitrile monomer, 300 parts of styrene monomer, 1.5 parts of AMSD, 5 parts of potassium disproportionate rosin acid and 175 parts of deionized water, and continue to add dropwise for 2 hours. After heating is completed, continue to react for 5 hours to obtain a grafted latex.
[0149] Take 1000 parts of grafted latex and add it to the flocculation reactor, start stirring and heat to 75°C, gradually add 450 parts of 10wt% magnesium sulfate aqueous solution, add it within 2 hours, and raise the temperature to 95°C and maintain the temperature for 2 hours. Filter the product with a 325-mesh filter to obtain a flocculation slurry.
[0150] Step 3: Prepare washing solution
[0151] At room temperature, 3 g of PdCl2 was dissolved in 20 ml of 10% hydrochloric acid, and 80 ml of anhydrous ethanol was added and mixed thoroughly. Under vigorous stirring, 20 ml of tetrabutyl titanate was slowly added dropwise to the above solution to form a homogeneous solution. Deionized water was added to adjust the pH of the system to about 4, and stirring was continued until Pd-doped TiO2 gel was formed.
[0152] Diatomaceous earth and deionized water were added to the above Pd-doped modified TiO2 gel to prepare a washing liquid, and the concentration of the Pd-doped modified TiO2 in the washing liquid was 0.5wt%, and the concentration of the diatomaceous earth in the washing liquid was 0.5wt%.
[0153] Step 4: Preparation of modified ABS rubber powder
[0154] The washing liquid and the flocculation slurry were mixed, and the flocculation slurry was washed, wherein the flow rate of the flocculation slurry was 2 tons / h, the flow rate of the washing liquid was 1 ton / h, and the washing time was 30 minutes. The mixed liquid was washed by vacuum transfer and then dehydrated in a centrifuge. After dehydration, it was dried in a fluidized bed and dried at 60°C for 6 hours to obtain a modified ABS rubber powder 1 with a moisture content of <1wt%. The proportions of Pd-doped modified TiO2 and diatomaceous earth in the modified ABS rubber powder 1 were measured, and the results are shown in Table 1.
[0155] Step 5: Preparation of ABS resin
[0156] 25 parts of the modified ABS rubber powder 1 and 75 parts of SAN resin were mixed, extruded through a twin-screw extruder, cooled, and pelletized to obtain ABS resin 1, wherein the extrusion temperature was 200°C, the screw speed was 250 r / min, and the screw aspect ratio was 40:1.
[0157] Example 2
[0158] This embodiment provides a modified ABS rubber powder and a preparation method thereof, an ABS resin and a preparation method thereof, which are basically the same as Example 1, except that: in step 3, the concentration of Pd-doped modified TiO2 in the washing liquid is 1wt%, and the concentration of diatomaceous earth in the washing liquid is 1wt%. This embodiment prepares modified ABS rubber powder 2 and ABS resin 2, and measures the proportions of Pd-doped modified TiO2 and diatomaceous earth in the modified ABS rubber powder 2, and the results are shown in Table 1.
[0159] Example 3
[0160] This embodiment provides a modified ABS rubber powder and a preparation method thereof, an ABS resin and a preparation method thereof, which are basically the same as Example 1, except that: in step 3, the concentration of Pd-doped modified TiO2 in the washing liquid is 0.8wt%, and the concentration of diatomaceous earth in the washing liquid is 0.8wt%. This embodiment obtains modified ABS rubber powder 3 and ABS resin 3, and measures the proportions of Pd-doped modified TiO2 and diatomaceous earth in the modified ABS rubber powder 3, and the results are shown in Table 1.
[0161] Example 4
[0162] This embodiment provides a modified ABS rubber powder and a preparation method thereof, an ABS resin and a preparation method thereof, which are basically the same as those in Example 1, except that in step 3, 3g of PdCl2 is replaced by 7g of H2PtCl6. This embodiment produces a modified ABS rubber powder 4 and an ABS resin 4, and the proportions of Pt-doped TiO2 and diatomaceous earth in the modified ABS rubber powder 4 are measured, and the results are shown in Table 1.
[0163] Example 5
[0164] This embodiment provides a modified ABS rubber powder and a preparation method thereof, an ABS resin and a preparation method thereof, which are basically the same as those in Embodiment 1, except that in step 3, porous silicate and deionized water are added to the Pd-doped modified TiO2 gel to prepare a washing liquid, and the concentration of the Pd-doped modified TiO2 in the washing liquid is 0.5wt%, and the concentration of the porous silicate in the washing liquid is 0.5wt%. This embodiment obtains modified ABS rubber powder 5 and ABS resin 5, and the proportions of Pd-doped modified TiO2 and porous silicate in the modified ABS rubber powder 5 are measured, and the results are shown in Table 1.
[0165] Example 6
[0166] This embodiment provides a modified ABS rubber powder and a preparation method thereof, an ABS resin and a preparation method thereof, which are basically the same as those in Example 1, except that Pd-doped modified TiO2 and diatomaceous earth are added in step 2. Steps 2 and 3 of this embodiment are as follows:
[0167] Step 2: Preparation of flocculation slurry
[0168] Add butadiene latex containing 600 parts of polybutadiene into a reactor, add 0.015 parts of ferrous sulfate into the reactor and stir evenly, heat the reactor to 67°C, add 2.51 parts of cumene hydroperoxide, 100 parts of acrylonitrile monomer, 300 parts of styrene monomer, 1.5 parts of AMSD, 5 parts of potassium disproportionate rosin acid and 175 parts of deionized water, and continue to add dropwise for 2 hours. After heating is completed, continue to react for 5 hours to obtain a grafted latex.
[0169] 1000 parts of grafted latex were added to a flocculation reaction kettle, stirred and heated to 75°C, 450 parts of 10wt% magnesium sulfate aqueous solution, 0.5 parts of Pd-doped modified TiO2 and 0.5 parts of diatomaceous earth were gradually added thereto, and the addition was completed within 2 hours, and the temperature was raised to 95°C and maintained for 2 hours. The product was filtered with a 325-mesh filter to obtain a flocculation slurry. The preparation method of Pd-doped modified TiO2 is as follows:
[0170] Under room temperature, 3g PdCl2 was dissolved in 20ml 10% hydrochloric acid, and then added into 80ml anhydrous ethanol and mixed thoroughly. Under vigorous stirring, 20ml tetrabutyl titanate was slowly dropped into the above solution to form a homogeneous solution. Deionized water was added to adjust the pH of the system to about 4. Stirring was continued until a Pd-doped TiO2 gel was formed. After dilution with water, the solution was dehydrated and dried to obtain Pd-doped TiO2.
[0171] Step 3: Preparation of modified ABS rubber powder
[0172] The flocculated slurry was washed with deionized water, wherein the flow rate of the flocculated slurry was 2 tons / h and the flow rate of water was 1 ton / h. After washing, the mixed liquid was dehydrated in a centrifuge, and then dried in a fluidized bed at 60°C for 6 hours to obtain a modified ABS rubber powder 6 with a moisture content of <1wt%. The proportions of Pd-doped modified TiO2 and diatomaceous earth in the modified ABS rubber powder 6 were measured, and the results are shown in Table 1.
[0173] Referring to step 5 of Example 1, ABS resin 6 of this example was prepared.
[0174] Example 7
[0175] This embodiment provides a modified ABS rubber powder and a preparation method thereof, an ABS resin and a preparation method thereof, which are basically the same as those in Example 1, except that Pd-doped modified TiO2 and diatomaceous earth are added after washing in step 4. Step 3 of this embodiment is as follows:
[0176] Step 3: Preparation of modified ABS rubber powder
[0177] The flocculation slurry of step 2 was washed with deionized water, wherein the flow rate of the flocculation slurry was 2 tons / h and the flow rate of water was 1 ton / h. After washing, the mixed solution was dehydrated in a centrifuge, and then dried in a fluidized bed at 60°C for 6 hours to obtain a rubber powder with a moisture content of <1wt%. Pd-doped TiO2 and diatomaceous earth were added to the rubber powder, so that the content of Pd-doped TiO2 in the powder was 0.51wt%, and the content of diatomaceous earth in the powder was 0.48wt%. The modified ABS rubber powder 7 was obtained by mechanical stirring, wherein the Pd-doped TiO2 was referred to Example 6.
[0178] Referring to step 5 of Example 1, ABS resin 7 of this example was prepared.
[0179] Example 8
[0180] This embodiment provides a modified ABS rubber powder and a preparation method thereof, an ABS resin and a preparation method thereof, which are basically the same as those in Example 1, except that in step 2, AMSD is replaced with TDM. This embodiment obtains modified ABS rubber powder 8 and ABS resin 8, and measures the proportions of Pd-doped TiO2 and diatomaceous earth in the modified ABS rubber powder 8, and the results are shown in Table 1.
[0181] Comparative Example 1
[0182] This comparative example provides an ABS rubber powder and a preparation method thereof, and an ABS resin and a preparation method thereof, which are basically the same as Example 1, except that the washing liquid is deionized water, and Pd-doped modified TiO2 and diatomaceous earth are not added. This comparative example produces ABS rubber powder 9 and ABS resin 9.
[0183] Comparative Example 2
[0184] This comparative example provides an ABS rubber powder and a preparation method thereof, an ABS resin and a preparation method thereof, which are basically the same as Example 1, except that the preparation of the washing liquid in step 3 is different. Step 3 of this comparative example is as follows:
[0185] Step 3: Prepare washing solution
[0186] At room temperature, add 80 ml of anhydrous ethanol to 20 ml of 10% hydrochloric acid and mix thoroughly. Under vigorous stirring, slowly add 20 ml of tetrabutyl titanate to the above solution to form a homogeneous solution. Add deionized water to adjust the pH of the system to about 4, and continue stirring until TiO2 gel is formed.
[0187] Diatomaceous earth and deionized water were added to the above TiO2 gel to prepare a washing liquid, and the concentration of TiO2 in the washing liquid was 0.5wt%, and the concentration of diatomaceous earth in the washing liquid was 0.5wt%.
[0188] Referring to step 4 and step 5 of Example 1, ABS rubber powder 10 and ABS resin 10 of this comparative example were prepared, and the proportions of TiO2 and diatomaceous earth in the modified ABS rubber powder 10 were measured. The results are shown in Table 2.
[0189] Comparative Example 3
[0190] This comparative example provides an ABS rubber powder and a preparation method thereof, an ABS resin and a preparation method thereof, which are basically the same as Example 1, except that the preparation of the washing liquid in step 3 is different. Step 3 of this comparative example is as follows:
[0191] Step 3: Prepare washing solution
[0192] At room temperature, 3 g of PdCl2 was dissolved in 20 ml of 10% hydrochloric acid, and 80 ml of anhydrous ethanol was added and mixed thoroughly. Under vigorous stirring, 20 ml of tetrabutyl titanate was slowly added dropwise to the above solution to form a homogeneous solution. Deionized water was added to adjust the pH of the system to about 4, and stirring was continued until Pd-doped TiO2 gel was formed.
[0193] Deionized water was added to the Pd-doped modified TiO2 gel to prepare a washing solution, and the concentration of the Pd-doped modified TiO2 in the washing solution was 1 wt %.
[0194] Referring to step 4 and step 5 of Example 1, ABS rubber powder 11 and ABS resin 11 of this comparative example were prepared, and the proportion of Pd-doped modified TiO2 in the modified ABS rubber powder 11 was measured. The results are shown in Table 2.
[0195] The ABS resins of the above embodiments and comparative examples were subjected to performance tests. The test items and methods are as follows. The test results are shown in Tables 1 and 2.
[0196] Odor: Tested according to PV3900-2000;
[0197] Total carbon (TVOC): tested according to PV3341;
[0198] Residual order test conditions:
[0199] Headspace injection: HS-10 constant temperature oven 80℃, sample flow path 210℃, transfer line 215℃, injection port: temperature 230℃, split ratio 100:1, injection time 1min, septum purge flow rate, 3ml / min. Column box: initial temperature 60℃, retention time 1min, first-order heating rate 5℃ / min, final temperature 80℃, holding time 0min, second-order heating rate 1℃ / min, final temperature 85℃, holding time: 0min. Third-order heating rate 5℃ / min, final temperature 100℃, holding time 0min, fourth-order heating rate 40℃ / min, final temperature 225℃, holding time 5min. Front detector FID: temperature 320℃, tail gas N2: 24ml / min. Gas pressure and flow rate: APC1 pressure 260.0kPa.
[0200] Quantitative method: internal standard method
[0201] Weigh 0.5 g of the sample, accurate to 0.1 mg, into a headspace bottle, add 10 ml of o-dichlorobenzene (containing 5 mg / L n-butanol), seal the bottle, place it in an oscillator at 60°C for 2 hours, and take it out for analysis.
[0202] Table 1
[0203]
[0204]
[0205] Table 2
[0206]
[0207] It can be seen from Table 1 and Table 2 that the odor of the ABS resin prepared by the modified ABS rubber powder of Examples 1-8 is between 3 and 3.7, the TVOC is between 13 and 38 μg / g, the residual styrene is between 280 and 390 ppm, the residual ethylbenzene is between 32 and 56 ppm, and the residual acrylonitrile is between 20 and 29 ppm. It shows a lower residual amount, low odor and less TVOC. The chain transfer agent used in Example 8 is different from that in Example 1, and has relatively more TVOC and odor. In Examples 6 and 7, the residual adsorbent and the titanium dioxide doped with transition metal elements are added before and after washing, respectively, but the effect is not as good as that added in the washing liquid. Adding the residual adsorbent and the titanium dioxide doped with transition metal elements in the washing liquid has a better dispersion effect on the two in the rubber powder, and a better effect on reducing the residual amount, odor and VOC.
[0208] In Comparative Example 1, no residual monophenyl adsorbent and transition metal element doped modified titanium dioxide were added, in Comparative Example 2, titanium dioxide was not modified, and in Comparative Example 3, only Pd doped modified TiO2 gel was added without adding residual monophenyl adsorbent. The ABS resins prepared from the ABS rubber powders of Comparative Examples 1, 2 and 3 had poor effects on reducing the residual monophenyl content, odor and VOC.
[0209] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0210] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A modified ABS rubber powder, characterized in that: The modified ABS rubber powder contains residual single adsorbent and titanium dioxide doped with transition metal elements, and the transition metal element is palladium, platinum or a combination thereof; The residual single adsorbent includes diatomaceous earth, molecular sieve, porous silicate or a combination thereof; The residual adsorbent accounts for 0.2wt% to 1.5wt% of the modified ABS rubber powder; The transition metal element doped modified titanium dioxide accounts for 0.2wt% to 1.5wt% of the modified ABS rubber powder.
2. The modified ABS rubber powder according to claim 1, characterized in that: In the transition metal element doped modified titanium dioxide, the molar ratio of the transition metal element to the titanium element is 1:(1-5).
3. The modified ABS rubber powder according to any one of claims 1-2, characterized in that: One or more of the following conditions are met: 1) The residual adsorbent accounts for 0.46wt% to 0.98wt% of the modified ABS rubber powder; 2) The transition metal element doped modified titanium dioxide accounts for 0.48wt% to 0.96wt% of the modified ABS rubber powder.
4. The modified ABS rubber powder according to any one of claims 1-2, characterized in that: One or more of the following conditions are met: 1) The content of polybutadiene in the modified ABS rubber powder is 50wt% to 70wt%; 2) The content of acrylonitrile-styrene copolymer in the modified ABS rubber powder is 27wt% to 49.6wt%; the polymerization monomers of the acrylonitrile-styrene copolymer include acrylonitrile monomer and styrene monomer in a weight ratio of (50-150):(250-350).
5. A method for preparing modified ABS rubber powder, characterized in that: The following steps are involved: Mixing butadiene latex, acrylonitrile monomer and styrene monomer, performing emulsion graft copolymerization reaction to obtain grafted latex, and flocculating the grafted latex to prepare flocculated slurry; Mixing the washing liquid and the flocculated slurry, collecting the solid and drying it to prepare modified ABS rubber powder; The washing liquid comprises a residual single adsorbent and titanium dioxide doped and modified by a transition metal element, wherein the transition metal element is palladium, platinum or a combination thereof; The residual single adsorbent includes diatomaceous earth, molecular sieve, porous silicate or a combination thereof; The concentration of the residual adsorbent in the washing liquid is 0.5wt% to 1wt%; The concentration of the titanium dioxide doped with transition metal elements in the washing liquid is 0.5 wt % to 1 wt %.
6. The method for preparing the modified ABS rubber powder according to claim 5, characterized in that: The preparation method of the washing liquid comprises the following steps: Using tetrabutyl titanate as a precursor and a transition metal salt as a doping source, a transition metal element-doped titanium dioxide gel is prepared by a sol-gel method, wherein the transition metal salt is a palladium salt, a platinum salt or a combination thereof; The transition metal element doped modified titanium dioxide gel, residual adsorbent and washing solvent are mixed to prepare a washing liquid.
7. The method for preparing the modified ABS rubber powder according to claim 6, characterized in that: The molar ratio of the transition metal salt to the tetrabutyl titanate is 1:(1-5).
8. The method for preparing the modified ABS rubber powder according to any one of claims 5 to 7, characterized in that: The concentration of the residual adsorbent in the washing liquid is 0.8wt% to 1wt%; and / or The concentration of the titanium dioxide doped with transition metal elements in the washing liquid is 0.8 wt % to 1 wt %.
9. The method for preparing modified ABS rubber powder according to claim 8, characterized in that: The volume ratio of the washing liquid to the flocculation slurry is 1:(1.5-2.5).
10. The method for preparing the modified ABS rubber powder according to any one of claims 5 to 7 and 9, characterized in that: One or more of the following conditions are met: 1) The butadiene latex is prepared by emulsion polymerization of butadiene monomer; 2) controlling the weight of the butadiene latex so that the content of polybutadiene in the modified ABS rubber powder is 50wt% to 70wt%; 3) controlling the weight of the acrylonitrile monomer and the styrene monomer so that the content of the acrylonitrile-styrene copolymer in the modified ABS rubber powder is 27wt% to 49.6wt%, and the weight ratio of the acrylonitrile monomer to the styrene monomer is (50 to 150):(250 to 350); 4) The chain transfer agent used in the emulsion graft copolymerization reaction is α-methylstyrene dimer 5) The initiator used in the emulsion graft copolymerization reaction is selected from one or more of cumene hydroperoxide, sodium persulfate, potassium persulfate, ammonium persulfate and azobisisobutylnitrile; 6) the emulsifier used in the emulsion graft copolymerization reaction is selected from one or more of sodium salt of pernaphthalenesulfonic acid formaldehyde condensate, potassium salt of naphthalenesulfonic acid formaldehyde condensate, potassium oleate, potassium stearate, potassium disproportionated rosin acid, sodium dodecylbenzene sulfonate and sodium dodecyl sulfonate; 7) The reducing agent used in the emulsion graft copolymerization reaction is selected from one or more of sodium ethylenediaminetetraacetate, ferrous sulfate, glucose, sodium pyrophosphate and sodium sulfite; 8) The solvent used in the emulsion graft copolymerization reaction is water; and 9) The flocculant used in the flocculation treatment is one or more selected from magnesium sulfate, sulfuric acid and calcium chloride.
11. An ABS resin, characterized in that: The composition comprises the modified ABS rubber powder described in any one of claims 1 to 4 or the modified ABS rubber powder prepared by the preparation method described in any one of claims 5 to 10, and SAN resin.
12. A vehicle interior component, characterized in that: The composition comprises the modified ABS rubber powder according to any one of claims 1 to 4, the modified ABS rubber powder prepared by the preparation method according to any one of claims 5 to 10, or the ABS resin according to claim 11.