ABS rubber powder and preparation method thereof, ABS material and vehicle interior parts
By using emulsion graft copolymerization and flocculation treatment technology in ABS glue powder, ABS glue powder with high loss modulus is prepared, which solves the noise problem in the vehicle and achieves a lasting anti-noise effect.
Patent Information
- Application Number
- CN202310531191.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-10
AI Technical Summary
The noise in the vehicle mainly comes from the extrusion of the combined components in the vehicle and the friction between the components. The existing methods cannot achieve a lasting anti-noise effect.
A ABS rubber powder is used, which includes a continuous phase and a dispersed phase, the continuous phase is an acrylonitrile-styrene copolymer, and the dispersed phase is polybutadiene, the polybutadiene is composed of a first butadiene rubber and a second butadiene The ene rubber is composed of olefin rubber, prepared by emulsion graft copolymerization and flocculation treatment, forming ABS powder with a higher loss modulus, improving the damping performance of the material.
The loss factor of ABS powder is improved, good noise reduction performance and lasting noise anti-noise effect are achieved, and noise in the vehicle is reduced.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of engineering plastics, and in particular to ABS rubber powder and a preparation method thereof, ABS material and vehicle interior decoration parts. Background Art
[0002] In recent years, the automotive industry has paid more and more attention to in-car noise. In-car noise mainly comes from the extrusion of joint parts in the car and the friction between parts. Loud in-car noise will directly affect the physical and mental health of drivers and passengers, and even affect driving safety.
[0003] In order to improve the noise problem, the usual method is to apply grease or felt on the extrusion surface or friction surface of the component to prevent direct contact between the components, so as to achieve the purpose of reducing noise, but this method cannot achieve a lasting anti-noise effect. Summary of the invention
[0004] Based on this, the present invention provides an ABS rubber powder and a preparation method thereof, an ABS material and a vehicle interior decoration part.
[0005] The first aspect of the present invention provides an ABS rubber powder, and its technical solution is as follows:
[0006] An ABS rubber powder, comprising a continuous phase and a dispersed phase dispersed in the continuous phase;
[0007] The continuous phase comprises acrylonitrile-styrene copolymer, and the dispersed phase comprises polybutadiene;
[0008] The polybutadiene includes a first butadiene rubber and a second butadiene rubber;
[0009] The average particle size of the first butadiene rubber is 250nm to 350nm, and the average particle size of the second butadiene rubber is 800nm to 2000nm;
[0010] The weight ratio of the first butadiene rubber to the second butadiene rubber is (40-50):(3-7).
[0011] In some embodiments, one or more of the following conditions are met:
[0012] 1) The second butadiene rubber is selected from butadiene rubber, styrene butadiene rubber or a combination thereof.
[0013] 2) The polybutadiene accounts for 49wt% to 70wt% of the ABS rubber powder;
[0014] 3) The acrylonitrile-styrene copolymer accounts for 30wt% to 51wt% of the ABS rubber powder, and the polymerization monomers of the acrylonitrile-styrene copolymer include acrylonitrile monomer and styrene monomer in a weight ratio of (50 to 150): (50 to 400).
[0015] The second aspect of the present invention provides a method for preparing ABS rubber powder, and its technical scheme is as follows:
[0016] Mixing a first butadiene latex and a second butadiene latex to prepare a seed latex, wherein the first butadiene latex includes a first butadiene rubber, the average particle size of the first butadiene rubber is 250nm-350nm, the second butadiene latex includes a second butadiene rubber, the average particle size of the second butadiene rubber is 800nm-2000nm, and in the seed latex, the weight ratio of the first butadiene rubber to the second butadiene rubber is (40-50):(3-7);
[0017] The seed latex, acrylonitrile monomer and styrene monomer are mixed, and an emulsion graft copolymerization reaction is carried out under the action of a chain transfer agent, an initiator, an emulsifier, a reducing agent and a solvent to obtain a grafted latex, and the grafted latex is flocculated and the solid is collected and then dried.
[0018] In some embodiments, the solid content of the first butadiene latex is 50 wt % to 65 wt %; and / or the solid content of the second butadiene latex is 15 wt % to 25 wt %.
[0019] In some embodiments, the second butadiene rubber is selected from butadiene rubber, styrene butadiene rubber or a combination thereof.
[0020] In some embodiments, the second butadiene latex further includes a solvent, and the solvent is a styrene monomer.
[0021] In some embodiments, the first butadiene latex is prepared by emulsion polymerization of butadiene monomer.
[0022] In some embodiments, one or more of the following conditions are met:
[0023] 1) controlling the weight of the seed latex so that the proportion of the polybutadiene in the ABS rubber powder is 49wt% to 70wt%;
[0024] 2) The weight of the acrylonitrile monomer and the styrene monomer is controlled so that the proportion of the acrylonitrile-styrene copolymer in the ABS rubber powder is 30wt% to 51wt%, and the polymerized monomers of the acrylonitrile-styrene copolymer include acrylonitrile monomer and styrene monomer in a weight ratio of (50-150):(50-400).
[0025] In some embodiments, the emulsion graft copolymerization reaction satisfies one or more of the following conditions:
[0026] 1) The chain transfer agent used in the emulsion graft copolymerization reaction is selected from one or more of tert-dodecyl mercaptan, n-dodecyl mercaptan, tetradecyl mercaptan, tridecyl mercaptan, undecyl mercaptan and decanyl mercaptan;
[0027] 2) The initiator used in the emulsion graft copolymerization reaction is selected from one or more of cumene hydroperoxide, sodium persulfate, potassium persulfate, ammonium persulfate and azobisisobutylnitrile;
[0028] 3) the emulsifier used in the emulsion graft copolymerization reaction is selected from one or more of naphthalenesulfonic acid formaldehyde condensate sodium salt, naphthalenesulfonic acid formaldehyde condensate potassium salt, potassium oleate, potassium stearate, disproportionated potassium rosin acid, sodium dodecylbenzene sulfonate and sodium dodecyl sulfonate;
[0029] 4) The reducing agent used in the emulsion graft copolymerization reaction is selected from one or more of sodium ethylenediaminetetraacetate, ferrous sulfate, glucose, sodium pyrophosphate and sodium sulfite;
[0030] 5) The solvent used in the emulsion graft copolymerization reaction is water;
[0031] 6) The flocculant used in the flocculation treatment is one or more selected from magnesium sulfate, sulfuric acid and calcium chloride.
[0032] A third aspect of the present invention provides an ABS material, which comprises the above-mentioned ABS rubber powder or the ABS rubber powder prepared by the above-mentioned preparation method, and SAN resin.
[0033] In some of the embodiments, the weight ratio of the ABS rubber powder to the SAN resin is (15-35): (65-85).
[0034] A fourth aspect of the present invention provides a vehicle interior trim, the components of which include the above-mentioned ABS rubber powder or the ABS rubber powder prepared by the above-mentioned preparation method or the above-mentioned ABS material.
[0035] Compared with the traditional solution, the present invention has the following beneficial effects:
[0036] The dispersed phase of the ABS rubber powder of the present invention includes polybutadiene, and the polybutadiene includes a first butadiene rubber and a second butadiene rubber, wherein the average particle size of the first butadiene rubber is 250nm-350nm, and the average particle size of the second butadiene rubber is 800nm-2000nm, and the weight ratio of the first butadiene rubber to the second butadiene rubber is controlled to be (40-50):(3-7). In the presence of the first butadiene rubber with a small particle size and the second butadiene rubber with a large particle size, a dispersed phase with cavities can be formed, thereby increasing the loss modulus of the synthesized ABS rubber powder, thereby increasing the loss factor of the ABS rubber powder, and thus being beneficial to reducing the noise of the ABS rubber powder. The ABS rubber powder of the present invention has good damping performance itself, thereby having good noise reduction performance, and can achieve a lasting anti-noise effect. DETAILED DESCRIPTION
[0037] The present invention will be further described in detail below in conjunction with specific embodiments. The present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly understood.
[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0039] the term
[0040] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0041] In the present invention, "plurality", "multiple", "multiple times", "multiple" and the like, unless otherwise specified, refer to a number greater than or equal to 2. For example, "one or more" means one or greater than or equal to two.
[0042] In the present invention, “preferred”, “better”, “more preferred” and “suitable” are only used to describe implementation methods or examples with better effects, and it should be understood that they do not constitute limitations on the scope of protection of the present invention.
[0043] In the present invention, the words “further”, “furthermore”, “particularly”, etc. are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present invention.
[0044] In the present invention, "optionally", "optional" and "optional" refer to optional, that is, to any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.
[0045] In the present invention, in the "first aspect", "second aspect", "third aspect", "fourth aspect", etc., the terms "first", "second", "third", "fourth", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0046] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0047] In the present invention, when it comes to numerical intervals (i.e., numerical ranges), unless otherwise specified, the optional numerical distribution is considered continuous within the above numerical interval, and includes the two numerical endpoints (i.e., the minimum value and the maximum value) of the numerical range, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to the integers within the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints. In this article, it is equivalent to directly listing each integer, such as t is an integer selected from 1 to 10, indicating that t is any integer selected from the group of integers consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9 and 10. In addition, when multiple ranges are provided to describe features or characteristics, these ranges can be combined. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all sub-ranges included therein.
[0048] The temperature parameters in the present invention, if not specifically limited, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.
[0049] In the present invention, when it comes to percentage concentration, unless otherwise specified, it refers to the final concentration. The final concentration refers to the proportion of the added component in the system after the addition of the component.
[0050] In the present invention, wt% means weight percentage, and wt‰ means weight thousandth.
[0051] In the present invention, normal temperature refers to 20 to 30°C.
[0052] In the present invention, the first butadiene rubber and the second butadiene rubber in the ABS rubber powder can be characterized and observed by SEM.
[0053] In the present invention, the average particle size of the first butadiene rubber in the first butadiene latex, the average particle size of the second butadiene rubber in the second butadiene latex, and the weight ratio of the first butadiene rubber to the second butadiene rubber are tested according to the following method:
[0054] The first butadiene latex and the second butadiene latex were dissolved in acetone, and then ultrasonically dispersed. The particle size analysis dynamic light scattering method (DLS) was measured using a Malvern 3000 laser particle size analyzer in accordance with GB / T 29022-2012.
[0055] Improving the damping of materials is a way to reduce noise. Compared with applying grease or felt on the extrusion surface and friction surface of components to prevent direct contact between components for noise reduction, improving the damping of the materials used in the components can achieve a more lasting anti-noise effect.
[0056] An embodiment of the present invention provides an ABS rubber powder, which improves the anti-noise effect of the ABS rubber powder from the perspective of improving the damping of the ABS rubber powder, and includes a continuous phase and a dispersed phase dispersed in the continuous phase;
[0057] The continuous phase comprises acrylonitrile-styrene copolymer, and the dispersed phase comprises polybutadiene;
[0058] The polybutadiene includes a first butadiene rubber and a second butadiene rubber;
[0059] The average particle size of the first butadiene rubber is 250nm to 350nm, and the average particle size of the second butadiene rubber is 800nm to 2000nm;
[0060] The weight ratio of the first butadiene rubber to the second butadiene rubber is (40-50):(3-7).
[0061] The damping of a material is generally measured by the loss tangent value tanδ (or loss factor, damping factor), which represents the ratio of the loss modulus to the storage modulus of the material. Because polymers have both viscous and elastic properties, when external force acts on polymer materials, part of the energy will be stored, that is, the storage modulus, and the material will show elastic recovery; the other part of the energy will be dissipated due to viscous heat generation, that is, the loss modulus, and this part of the energy cannot be recovered; therefore, the damping performance of the material mainly comes from the internal friction of the polymer. The larger the loss factor, the more mechanical energy will be converted into heat energy and dissipated, which shows a better shock and noise reduction effect.
[0062] The dispersed phase in the above ABS rubber powder includes polybutadiene, and the polybutadiene includes a first butadiene rubber and a second butadiene rubber, wherein the average particle size of the first butadiene rubber is 250nm-350nm, and the average particle size of the second butadiene rubber is 800nm-2000nm, and the weight ratio of the first butadiene rubber to the second butadiene rubber is controlled to be (40-50): (3-7). In the presence of the first butadiene rubber with a small particle size and the second butadiene rubber with a large particle size, the loss modulus of the synthesized ABS rubber powder is increased, thereby increasing the loss factor of the ABS rubber powder, which is beneficial to reducing the noise of the ABS rubber powder. The ABS rubber powder of the present invention has good damping performance, thus has good noise reduction performance, and can achieve a lasting anti-noise effect.
[0063] It can be understood that the average particle size of the first butadiene rubber includes, but is not limited to, 250 nm, 280 nm, 300 nm, 330 nm, and 350 nm.
[0064] It can be understood that the average particle size of the second butadiene rubber includes but is not limited to: 800nm, 900nm, 1000nm, 1100nm, 1200nm, 1300nm, 1400nm, 1500nm, 1600nm, 1700nm, 1800nm, 2000nm.
[0065] It can be understood that the weight ratio of the first butadiene rubber to the second butadiene rubber includes, but is not limited to, 40:4, 44:4, 47:4, 40:5, 44:5, 47:5, 40:6, 44:6, and 47:6.
[0066] Optionally, the second butadiene rubber is selected from butadiene rubber, styrene butadiene rubber or a combination thereof. Preferably, the second butadiene rubber is butadiene rubber.
[0067] Optionally, the ABS rubber powder can be ABS high-rubber powder or ABS low-rubber powder. Preferably, the ABS rubber powder is ABS high-rubber powder, and the content of polybutadiene is 49wt% to 70wt%.
[0068] Optionally, the content of acrylonitrile-styrene copolymer in the ABS rubber powder is 30wt% to 51wt%, and the polymerization monomers of the acrylonitrile-styrene copolymer include acrylonitrile monomer and styrene monomer in a weight ratio of (50-150):(50-400).
[0069] An embodiment of the present invention further provides a method for preparing ABS rubber powder, which improves the anti-noise effect of ABS rubber powder from the perspective of improving the damping of ABS rubber powder, and comprises the following steps:
[0070] Mixing a first butadiene latex and a second butadiene latex to prepare a seed latex, wherein the first butadiene latex includes a first butadiene rubber, the first butadiene rubber has an average particle size of 250nm to 350nm, the second butadiene latex includes a second butadiene rubber, the second butadiene rubber has an average particle size of 800nm to 2000nm, and the weight ratio of the first butadiene rubber to the second butadiene rubber is (40 to 50): (3 to 7);
[0071] The seed latex, acrylonitrile monomer and styrene monomer are mixed, and an emulsion graft copolymerization reaction is carried out under the action of a chain transfer agent, an initiator, an emulsifier, a reducing agent and a solvent to obtain a grafted latex, and the grafted latex is flocculated and the solid is collected and then dried.
[0072] In this embodiment, the first butadiene latex and the second butadiene latex are used as seed latexes, wherein the first butadiene latex includes a first butadiene rubber with an average particle size of 250nm to 350nm, and the second butadiene latex includes a second butadiene rubber with an average particle size of 800nm to 2000nm. The weight ratio of the first butadiene rubber to the second butadiene rubber is controlled to be (40 to 50): (3 to 7). In the presence of the first butadiene rubber with a small particle size and the second butadiene rubber with a large particle size, it is beneficial to form a dispersed phase with voids during the subsequent graft copolymerization process, thereby increasing the loss modulus of the synthesized ABS rubber powder, thereby increasing the loss factor of the ABS rubber powder, and thus helping to reduce the noise of the ABS rubber powder.
[0073] It can be understood that the weight ratio of the first butadiene rubber to the second butadiene rubber includes, but is not limited to, 40:4, 44:4, 47:4, 40:5, 44:5, 47:5, 40:6, 44:6, and 47:6.
[0074] Optionally, the solid content of the first butadiene latex is 50 wt% to 65 wt%.
[0075] Optionally, the solid content of the second butadiene latex is 15 wt% to 25 wt%.
[0076] In this embodiment, the first butadiene latex provides a system environment for the latex. Optionally, the first butadiene latex can be prepared by emulsion polymerization of butadiene monomers. However, the particle size of the first butadiene latex prepared by emulsion polymerization of butadiene monomers is usually small. In this embodiment, the average particle size of the first butadiene rubber is 250nm to 350nm. It is understandable that the average particle size of the first butadiene rubber includes but is not limited to: 250nm, 280nm, 300nm, 330nm, 350nm.
[0077] Optionally, in the presence of an electrolyte, an initiator, an emulsifier and a chain transfer agent, butadiene monomer undergoes an emulsion polymerization reaction to obtain a first butadiene latex.
[0078] Optionally, the reaction time of the emulsion polymerization reaction is 20 h to 40 h, and the reaction temperature is 51° C. to 93° C.
[0079] In some examples, the method for preparing the first butadiene latex comprises the following steps:
[0080] The butadiene monomer, electrolyte, initiator, emulsifier and chain transfer agent are mixed, and the temperature of the obtained mixed system is raised from 51° C. to 61° C. to 83° C. to 93° C. within 20 h to 40 h.
[0081] Optionally, the initiator used in the emulsion polymerization is selected from one or more of cumene hydroperoxide, sodium persulfate, potassium persulfate, ammonium persulfate and azobisisobutylnitrile.
[0082] Optionally, the initiator accounts for 0.2 wt% to 1.5 wt% of the butadiene monomer.
[0083] Optionally, the electrolyte used in the emulsion polymerization is selected from one or more of sodium carbonate, sodium bicarbonate, sodium hydroxide, potassium carbonate and potassium hydroxide.
[0084] Optionally, the electrolyte accounts for 2 wt% to 15 wt% of the butadiene monomer.
[0085] Optionally, the emulsifier used in the emulsion polymerization is selected from one or more of naphthalenesulfonic acid formaldehyde condensate sodium salt, naphthalenesulfonic acid formaldehyde condensate potassium salt, potassium oleate, potassium stearate, potassium disproportionated rosin acid, sodium dodecylbenzene sulfonate and sodium dodecyl sulfonate.
[0086] Optionally, the emulsifier accounts for 2 wt% to 15 wt% of the butadiene monomer.
[0087] Optionally, the chain transfer agent used in the emulsion polymerization is one or more selected from tert-dodecyl mercaptan, n-dodecyl mercaptan, tetradecyl mercaptan, tridecyl mercaptan, undecyl mercaptan and decanyl mercaptan.
[0088] Optionally, the chain transfer agent accounts for 0.5 wt% to 5 wt% of the butadiene monomer.
[0089] In order to increase the damping of ABS rubber powder, this embodiment introduces a second butadiene rubber with a larger particle size by adding a second butadiene latex on the basis of the latex system provided by the first butadiene latex. In this embodiment, the average particle size of the second butadiene rubber is 800nm to 2000nm. It can be understood that the average particle size of the second butadiene rubber includes but is not limited to: 800nm, 900nm, 1000nm, 1100nm, 1200nm, 1300nm, 1400nm, 1500nm, 1600nm, 1700nm, 1800nm, 2000nm.
[0090] Optionally, the second butadiene rubber is selected from butadiene rubber, styrene butadiene rubber or a combination thereof. Preferably, the second butadiene rubber is butadiene rubber.
[0091] Optionally, the second butadiene latex further comprises a solvent, and the solvent is a styrene monomer.
[0092] In this embodiment, after the seed latex is obtained, the seed latex, acrylonitrile monomer and styrene monomer undergo emulsion graft copolymerization in the presence of a reducing agent, an emulsifier, an initiator, a chain transfer agent and a solvent to obtain a grafted latex.
[0093] Optionally, the reaction time of the emulsion graft copolymerization reaction is 5 h to 9 h, and the reaction temperature is 10° C. to 72° C.
[0094] In some examples, the method for preparing the grafted latex comprises the following steps:
[0095] The seed latex and the reducing agent are mixed, and the resulting mixed system is heated to 62°C to 72°C, and acrylonitrile monomer, styrene monomer, emulsifier, initiator, chain transfer agent and solvent are added. After keeping the temperature for 1 to 3 hours, the mixture is naturally cooled and reacted for 4 hours to 6 hours.
[0096] Optionally, the weight of the seed latex is controlled so that the proportion of the polybutadiene in the ABS rubber powder is 49wt% to 70wt%.
[0097] Optionally, the weight of the acrylonitrile monomer and the styrene monomer is controlled so that the acrylonitrile-styrene copolymer accounts for 30wt% to 51wt% of the ABS rubber powder, and the polymerized monomers of the acrylonitrile-styrene copolymer include acrylonitrile monomer and styrene monomer in a weight ratio of (50 to 150):(50 to 400).
[0098] Optionally, the chain transfer agent used in the emulsion graft copolymerization reaction is one or more selected from tert-dodecyl mercaptan, n-dodecyl mercaptan, tetradecyl mercaptan, tridecyl mercaptan, undecyl mercaptan and decanyl mercaptan.
[0099] The chain transfer agent accounts for 0.2wt‰ to 10wt‰ of the seed latex.
[0100] Optionally, the initiator used in the emulsion graft copolymerization reaction is selected from one or more of cumene hydroperoxide, sodium persulfate, potassium persulfate, ammonium persulfate and azobisisobutylnitrile.
[0101] Optionally, the initiator accounts for 1 wt‰ to 10 wt‰ of the seed latex.
[0102] Optionally, the emulsifier used in the emulsion graft copolymerization reaction is selected from one or more of naphthalenesulfonic acid formaldehyde condensate sodium salt, naphthalenesulfonic acid formaldehyde condensate potassium salt, potassium oleate, potassium stearate, potassium disproportionated rosin acid, sodium dodecylbenzene sulfonate and sodium dodecyl sulfonate.
[0103] Optionally, the emulsifier accounts for 2wt‰ to 20wt‰ of the seed latex.
[0104] Optionally, the reducing agent used in the emulsion graft copolymerization reaction is selected from one or more of sodium ethylenediaminetetraacetate, ferrous sulfate, glucose, sodium pyrophosphate and sodium sulfite.
[0105] Optionally, the reducing agent accounts for 0.01 wt‰ to 0.05 wt‰ of the seed latex.
[0106] Optionally, the solvent used in the emulsion graft copolymerization reaction is water.
[0107] In this embodiment, a flocculant is added to the grafted latex to perform a flocculation treatment to prepare a flocculated slurry.
[0108] Optionally, the flocculation treatment time is 2h to 6h, and the reaction temperature is 70°C to 100°C.
[0109] Optionally, the flocculant used in the flocculation treatment is selected from one or more of magnesium sulfate, sulfuric acid and calcium chloride.
[0110] Optionally, the weight ratio of the grafted latex to the flocculant is 1000:(40-50).
[0111] It is understood that the flocculant is added to the graft latex in the form of an aqueous solution of the flocculant.
[0112] In some examples, the method for preparing the flocculated slurry comprises the following steps:
[0113] The grafted latex is heated to 70°C to 80°C, and a flocculant aqueous solution is added, wherein the flocculant aqueous solution is added within 1 hour to 3 hours, and then the temperature is raised to 90°C to 100°C and kept warm for 1 hour to 3 hours.
[0114] Optionally, in the aqueous flocculant solution, the concentration of the flocculant is 0.5 wt% to 5 wt%.
[0115] In this embodiment, the method further includes adding a washing liquid to the flocculation slurry for washing.
[0116] Optionally, the washing liquid is water.
[0117] In this embodiment, after washing, the solid can be collected by centrifugation, filtration or the like, and the solid can be dried to obtain ABS rubber powder.
[0118] The above preparation method requires less modification to the original emulsion production line, has less impact on the production cycle and energy consumption, is conducive to continuous large-scale production, has low preparation cost and high production efficiency.
[0119] Optionally, the product prepared by the above preparation method is ABS rubber powder, which can be ABS high-rubber powder or ABS low-rubber powder. Preferably, the prepared ABS rubber powder is ABS high-rubber powder, and the content of polybutadiene is 49wt% to 70wt%.
[0120] An embodiment of the present application further provides an ABS material, comprising the above-mentioned ABS rubber powder or the ABS rubber powder prepared by the above-mentioned preparation method, and SAN resin.
[0121] By blending ABS rubber powder with SAN resin, the content of acrylonitrile, butadiene and styrene can be flexibly adjusted, leaving a large room for modification.
[0122] Optionally, the weight ratio of ABS rubber powder to SAN resin can be adjusted according to actual use requirements. In some embodiments, the weight ratio of ABS rubber powder to SAN resin is (15-35): (65-85).
[0123] It can be understood that the ABS material can be prepared by extruding and pelletizing a powder containing ABS rubber powder and SAN resin. Optionally, the extrusion temperature is 180°C to 210°C, the screw speed is 200r / min to 300r / min, and the screw aspect ratio is (35 to 45):1.
[0124] One embodiment of the present invention provides a vehicle interior trim, the components of which include the above-mentioned ABS rubber powder or the ABS rubber powder prepared by the above-mentioned preparation method or the above-mentioned ABS material. .
[0125] The following is further described in conjunction with specific examples and comparative examples. The raw materials involved in the following specific examples and comparative examples, unless otherwise specified, can all be commercially available. The instruments used, unless otherwise specified, can all be commercially available. The processes involved, unless otherwise specified, are routinely selected by those skilled in the art. The parts involved in the following examples and comparative examples, unless otherwise specified, are parts by weight. The particle sizes involved in the following examples and comparative examples, unless otherwise specified, are average particle sizes.
[0126] Among them, butadiene monomer is industrial grade butadiene with a purity greater than 96%, from Huarui Chemical; butadiene rubber 35AE and butadiene rubber 55AE are from Asahi Kasei Corporation of Japan; butadiene rubber 50AF and butadiene rubber 30AF are from Dushanzi Petrochemical Company; butadiene rubber 565T and butadiene rubber 8497 are from Lanxess of Germany. Styrene monomer with a purity greater than or equal to 99% is from Aladdin Reagent Company; acrylonitrile monomer with a purity greater than or equal to 99% is from Aladdin Reagent Company; tert-dodecyl mercaptan TDM is a chain transfer agent; SAN resin is a styrene-acrylonitrile copolymer with a grade of PN-128, from Chi Mei of Taiwan, China.
[0127] Example 1
[0128] This embodiment provides an ABS rubber powder, an ABS material and a preparation method thereof, and the steps are as follows:
[0129] Step 1: preparing the first butadiene latex
[0130] 100 parts of butadiene monomer, 0.5 parts of sodium persulfate (initiator), 5 parts of sodium carbonate (electrolyte), 5 parts of potassium disproportionate rosin acid (emulsifier) and 2 parts of tert-dodecyl mercaptan (chain transfer agent) were mixed, the temperature was raised to 56°C to start emulsion polymerization reaction, the temperature was continuously raised to 88°C within 30 hours, the reaction was terminated after 30 hours, and the first butadiene latex with a particle size of 310 nm and a solid content of 58wt% was obtained.
[0131] Step 2: Preparation of the second butadiene latex
[0132] Take butadiene rubber 35AE and styrene monomer in a weight ratio of 20:80, stir at room temperature for 24 hours, and obtain a second butadiene latex with a particle size of 1000 nm and a solid content of 20wt%.
[0133] Step 3: Preparation of seed latex
[0134] The first butadiene latex and the second butadiene latex are mixed in a weight ratio of 80:20 to obtain a seed latex.
[0135] Step 4: Prepare ABS material
[0136] 1000 parts of seed latex were added into the reactor, 0.015 parts of ferrous sulfate were added into the reactor and stirred evenly, the reactor was heated to 67°C, 2.51 parts of cumene hydroperoxide, 100 parts of acrylonitrile monomer, 140 parts of styrene monomer, 1.5 parts of TDM, 5 parts of potassium disproportionate rosin acid and 175 parts of deionized water were added, and after keeping warm for 2 hours, the reaction was naturally cooled and reacted for 5 hours to obtain the grafted latex.
[0137] Take 1000 parts of grafted latex and add it to the flocculation reactor, start stirring and heat to 75°C, gradually add 450 parts of 10wt% magnesium sulfate aqueous solution, add it within 2 hours, and raise the temperature to 95°C and maintain the temperature for 2 hours. Filter the product with a 325-mesh filter to obtain a flocculation slurry.
[0138] Take the flocculated slurry and add deionized water for washing, wherein the flow rate of the flocculated slurry is 2 tons / h and the flow rate of water is 1 ton / h. The mixed liquid enters the centrifuge for dehydration, and then enters the fluidized bed for drying at 60°C for 6 hours to obtain ABS rubber powder 1 with a moisture content of <1wt%.
[0139] 25 parts of the above ABS rubber powder 1 and 75 parts of SAN resin were mixed, extruded through a twin-screw extruder, cooled, and pelletized to obtain ABS material 1, wherein the extrusion temperature was 200°C, the screw speed was 250 r / min, and the screw aspect ratio was 40:1.
[0140] Example 2
[0141] This embodiment provides an ABS rubber powder, an ABS material and a preparation method thereof, which are basically the same as those in Embodiment 1, except that: in step 3, the first butadiene latex and the second butadiene latex are mixed in a weight ratio of 70:30 to obtain a seed latex; in step 4, 1080 parts of the seed latex are added to a reaction kettle, and 40.8 parts of styrene monomer are added. This embodiment produces ABS rubber powder 2 and ABS material 2.
[0142] Example 3
[0143] This embodiment provides an ABS rubber powder, an ABS material and a preparation method thereof, which are basically the same as those in Embodiment 1, except that in step 2, cis-1,4-butadiene rubber 35AE is replaced with cis-1,4-butadiene rubber 55AE to obtain a second butadiene latex with a particle size of 2000 nm and a solid content of 20 wt%. This embodiment obtains ABS rubber powder 3 and ABS material 3.
[0144] Example 4
[0145] This embodiment provides an ABS rubber powder, an ABS material and a preparation method thereof, which are basically the same as those in Embodiment 3, except that: in step 3, the first butadiene latex and the second butadiene latex are mixed in a weight ratio of 70:30 to obtain a seed latex; in step 4, 1080 parts of the seed latex are added to a reaction kettle, and 40.8 parts of styrene monomer are added. This embodiment obtains ABS rubber powder 4 and ABS material 4.
[0146] Example 5
[0147] This embodiment provides an ABS rubber powder, an ABS material and a preparation method thereof, which are basically the same as those in Example 1, except that in step 2, cis-butadiene rubber 35AE is replaced with cis-butadiene rubber 50AF to obtain a second butadiene latex with a particle size of 1500nm and a solid content of 20wt%. This embodiment produces ABS rubber powder 5 and ABS material 5.
[0148] Example 6
[0149] This embodiment provides an ABS rubber powder, an ABS material and a preparation method thereof, which are basically the same as those in Embodiment 1, except that in step 2, cis-1,4-butadiene rubber 35AE is replaced with cis-1,4-butadiene rubber 565T to obtain a second butadiene latex with a particle size of 800 nm and a solid content of 20 wt%. This embodiment produces ABS rubber powder 6 and ABS material 6.
[0150] Example 7
[0151] This embodiment provides an ABS rubber powder, an ABS material and a preparation method thereof, which are basically the same as those in Embodiment 1, except that in step 4, the seed latex is adjusted from 1000 parts to 1100 parts, the acrylonitrile monomer is adjusted from 100 parts to 150 parts, and the styrene monomer is adjusted from 140 parts to 50 parts. This embodiment produces ABS rubber powder 7 and ABS material 7.
[0152] Example 8
[0153] This embodiment provides an ABS rubber powder, an ABS material and a preparation method thereof, which are basically the same as those in Embodiment 1, except that: in step 4, the seed latex is adjusted from 1000 parts to 900 parts, the acrylonitrile monomer is adjusted from 100 parts to 50 parts, and the styrene monomer is adjusted from 140 parts to 200 parts. 20 parts of the above ABS rubber powder 1 and 80 parts of SAN resin are taken, mixed, extruded through a twin-screw extruder, cooled, and pelletized. This embodiment produces ABS rubber powder 8 and ABS material 8.
[0154] Example 9
[0155] This embodiment provides an ABS rubber powder, an ABS material and a preparation method thereof, which are basically the same as those in Embodiment 1, except that: in step 3, the first butadiene latex and the second butadiene latex are mixed in a weight ratio of 75:25 to obtain a seed latex; in step 4, 1040 parts of the seed latex are added to a reaction kettle, and 92 parts of styrene monomer are added. This embodiment produces ABS rubber powder 9 and ABS material 9.
[0156] Comparative Example 1
[0157] This comparative example provides an ABS rubber powder, an ABS material and a preparation method thereof, which are basically the same as Example 1, except that: in step 2, cis-butadiene rubber 35AE is replaced with cis-butadiene rubber 30AF to obtain a second butadiene latex with a particle size of 500nm and a solid content of 20wt%. This comparative example obtains ABS rubber powder 10 and ABS material 10.
[0158] Comparative Example 2
[0159] This comparative example provides an ABS rubber powder, an ABS material and a preparation method thereof, which are basically the same as those in Example 1, except that no second butadiene latex is added. The steps are as follows:
[0160] Step 1: Prepare ABS material
[0161] 869 parts of the first butadiene latex of step 1 in Example 1 are added to a reactor, 0.015 parts of ferrous sulfate is added to the reactor and stirred evenly, the reactor is heated to 67°C, 2.51 parts of cumene hydroperoxide, 100 parts of acrylonitrile monomer, 300 parts of styrene monomer, 1.5 parts of TDM, 5 parts of potassium disproportionate rosin acid and 175 parts of deionized water are added, and the addition is continued dropwise for 2 hours. After heating is completed, the reaction is continued for 5 hours to obtain a grafted latex.
[0162] Take 1000 parts of grafted latex and add it to the flocculation reactor, start stirring and heat to 75°C, gradually add 450 parts of 10wt% magnesium sulfate aqueous solution, add it within 2 hours, and raise the temperature to 95°C and maintain the temperature for 2 hours. Filter the product with a 325-mesh filter to obtain a flocculation slurry.
[0163] The flocculated slurry was taken and washed with deionized water, wherein the flow rate of the flocculated slurry was 2 tons / h and the flow rate of water was 1 ton / h. The mixed liquid was dehydrated in a centrifuge and then dried in a fluidized bed at 60°C for 6 hours to obtain ABS rubber powder 11 with a moisture content of <1wt%.
[0164] 25 parts of the above ABS rubber powder 8 and 75 parts of SAN resin are mixed, extruded through a twin-screw extruder, cooled, and pelletized to obtain ABS material 11, wherein the extrusion temperature is 200°C, the screw speed is 250 r / min, and the screw aspect ratio is 40:1.
[0165] Comparative Example 3
[0166] This comparative example provides an ABS rubber powder, an ABS material and a preparation method thereof, which are basically the same as Example 1, except that the cis-butadiene rubber 35AE is replaced with cis-butadiene rubber 8497 to obtain a second butadiene latex with a particle size of 3000 nm and a solid content of 20 wt%. This comparative example obtains ABS rubber powder 12 and ABS material 12.
[0167] The ABS materials of the above embodiments and comparative examples were subjected to performance tests. The test items and methods are as follows. The test results are shown in Tables 1 and 2.
[0168] Tensile strength refers to ISO 527-2012 50mm / min;
[0169] Bending strength refers to ISO 178-2010 2mm / min;
[0170] The notched impact strength of simply supported beam is in accordance with ISO 179-2010 at 23°C;
[0171] The loss factor tanδ (damping factor) is tested according to the free vibration attenuation method;
[0172] The noise risk factor (RPN value) is tested according to the German automotive industry standard VDA 230-206-2005 method, which meets 40N and a speed of 1mm / s. Risk factors 1-3 are low noise risks, risk factors 4-6 are medium noise risks, and risk factors 7-10 are high noise risks.
[0173] Table 1
[0174]
[0175] Table 2
[0176]
[0177]
[0178] As shown in Table 1 and Table 2, in Examples 1 to 9, the first butadiene latex and the second butadiene latex are used as seed latexes to prepare ABS rubber powder, and then prepare ABS materials, wherein the particle size of the second butadiene rubber is in the range of 800nm to 2000nm. Under the above particle size range, the RPN value of the ABS material is 1 to 3, the RPN value is relatively low, the loss factor tanδ is 0.021 to 0.033, and the loss factor tanδ is relatively high, which is conducive to reducing the noise of the ABS material. At the same time, the mechanical properties of the ABS material such as tensile strength and bending strength are maintained well. Combined with Examples 1, 3, 5, 7, 8, and 9, when the particle size of the second butadiene rubber is in the range of 1500nm to 2000nm, the RPN value is 1 to 2, the loss factor tanδ is 0.027 to 0.028, and the noise reduction effect is better. In combination with Examples 1, 2, and 9 or in combination with Examples 3 and 4, adjusting the ratio of the first butadiene rubber to the second butadiene rubber is also beneficial to enhancing the noise reduction effect of the ABS material, wherein the smaller the weight ratio of the first butadiene rubber to the second butadiene rubber is, the better the noise reduction effect is.
[0179] Comparative Example 1 added a second butadiene rubber with a particle size of 500 nm, Comparative Example 2 did not add a second butadiene, and Comparative Example 3 added a second butadiene with a particle size of 3000 nm. The noise reduction effects were all inferior to those of Example 1.
[0180] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0181] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An ABS rubber powder, characterized in that: The ABS rubber powder comprises a continuous phase and a dispersed phase dispersed in the continuous phase; The continuous phase comprises acrylonitrile-styrene copolymer, and the dispersed phase comprises polybutadiene; The polybutadiene includes a first butadiene rubber and a second butadiene rubber; The average particle size of the first butadiene rubber is 250nm to 350nm, and the average particle size of the second butadiene rubber is 800nm to 2000nm; The weight ratio of the first butadiene rubber to the second butadiene rubber is (40-50):(3-7).
2. The ABS rubber powder according to claim 1, characterized in that: One or more of the following conditions are met: 1) the second butadiene rubber is selected from butadiene rubber, styrene butadiene rubber or a combination thereof; 2) The polybutadiene accounts for 49wt% to 70wt% of the ABS rubber powder; 3) The acrylonitrile-styrene copolymer accounts for 30wt% to 51wt% of the ABS rubber powder, and the polymerization monomers of the acrylonitrile-styrene copolymer include acrylonitrile monomer and styrene monomer in a weight ratio of (50 to 150): (50 to 400).
3. A method for preparing ABS rubber powder, characterized in that: The following steps are involved: Mixing a first butadiene latex and a second butadiene latex to prepare a seed latex, wherein the first butadiene latex includes a first butadiene rubber, the average particle size of the first butadiene rubber is 250nm-350nm, the second butadiene latex includes a second butadiene rubber, the average particle size of the second butadiene rubber is 800nm-2000nm, and in the seed latex, the weight ratio of the first butadiene rubber to the second butadiene rubber is (40-50):(3-7); The seed latex, acrylonitrile monomer and styrene monomer are mixed, and an emulsion graft copolymerization reaction is carried out under the action of a chain transfer agent, an initiator, an emulsifier, a reducing agent and a solvent to obtain a grafted latex, and the grafted latex is flocculated and the solid is collected and then dried.
4. The method for preparing ABS rubber powder according to claim 3, characterized in that: The solid content of the first butadiene latex is 50 wt% to 65 wt%; and / or the solid content of the second butadiene latex is 15 wt% to 25 wt%.
5. The method for preparing ABS rubber powder according to claim 3, characterized in that: The second butadiene rubber is selected from butadiene rubber, styrene butadiene rubber or a combination thereof.
6. The method for preparing ABS rubber powder according to claim 5, characterized in that: The second butadiene latex further includes a solvent, and the solvent is a styrene monomer.
7. The method for preparing ABS rubber powder according to claim 3, characterized in that: The first butadiene latex is prepared by emulsion polymerization of butadiene monomer.
8. The method for preparing ABS rubber powder according to any one of claims 3 to 7, characterized in that: One or more of the following conditions are met: 1) controlling the weight of the seed latex so that the proportion of the polybutadiene in the ABS rubber powder is 49wt% to 70wt%; 2) The weight of the acrylonitrile monomer and the styrene monomer is controlled so that the proportion of the acrylonitrile-styrene copolymer in the ABS rubber powder is 30wt% to 51wt%, and the polymerized monomers of the acrylonitrile-styrene copolymer include acrylonitrile monomer and styrene monomer in a weight ratio of (50-150):(50-400).
9. The method for preparing ABS rubber powder according to any one of claims 3 to 7, characterized in that: The emulsion graft copolymerization reaction satisfies one or more of the following conditions: 1) The chain transfer agent used in the emulsion graft copolymerization reaction is selected from one or more of tert-dodecyl mercaptan, n-dodecyl mercaptan, tetradecyl mercaptan, tridecyl mercaptan, undecyl mercaptan and decanyl mercaptan; 2) The initiator used in the emulsion graft copolymerization reaction is selected from one or more of cumene hydroperoxide, sodium persulfate, potassium persulfate, ammonium persulfate and azobisisobutylnitrile; 3) the emulsifier used in the emulsion graft copolymerization reaction is selected from one or more of naphthalenesulfonic acid formaldehyde condensate sodium salt, naphthalenesulfonic acid formaldehyde condensate potassium salt, potassium oleate, potassium stearate, disproportionated potassium rosin acid, sodium dodecylbenzene sulfonate and sodium dodecyl sulfonate; 4) The reducing agent used in the emulsion graft copolymerization reaction is selected from one or more of sodium ethylenediaminetetraacetate, ferrous sulfate, glucose, sodium pyrophosphate and sodium sulfite; 5) The solvent used in the emulsion graft copolymerization reaction is water; 6) The flocculant used in the flocculation treatment is one or more selected from magnesium sulfate, sulfuric acid and calcium chloride.
10. An ABS material, characterized in that: The ABS material comprises the ABS rubber powder according to any one of claims 1 to 2 or the ABS rubber powder prepared by the preparation method according to any one of claims 3 to 9, and SAN resin.
11. The ABS material according to claim 10, characterized in that: The weight ratio of the ABS rubber powder to the SAN resin is (15-35):(65-85).
12. A vehicle interior component, characterized in that: Its components include the ABS rubber powder described in any one of claims 1 to 2, or the ABS rubber powder prepared by the preparation method described in any one of claims 3 to 9, or the ABS material described in any one of claims 10 to 11.