A high-strength, low-fog, transparent polypropylene material and preparation method thereof
By adding polymethyl methacrylate modified microspheres to polypropylene, combining other components and processes, the problem of taking into account both the mechanical strength and transparency of polypropylene is solved, and a high-strength, low-haze polypropylene material is achieved, suitable for multiple A kind of application scenario.
Patent Information
- Application Number
- CN202310407824.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-04-17
AI Technical Summary
The prior art is difficult to maintain its transparency and low haze while improving the mechanical strength of polypropylene, which limits the application prospects of transparent polypropylene in packaging, medical devices and other fields.
By adding polymethyl methacrylate modified microspheres to polypropylene and combining random copolymerized polypropylene, low-density polyethylene copolymer, compatibility agent, antioxidant and nucleating agent, the emulsion polymerization method is prepared and modified by emulsion polymerization method. Microspheres significantly increase the mechanical strength of polypropylene and maintain high light transmittance.
It realizes the high-strength, low haze characteristics of polypropylene materials, has excellent mechanical properties and high light transmittance, and is suitable for a variety of application scenarios.
Smart Images

Figure BDA0004182094380000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a high-strength, low-fog, transparent polypropylene material and a preparation method thereof. Background Art
[0002] Polypropylene (PP) is one of the five most widely used general synthetic resins. It has good heat resistance, chemical corrosion resistance, processability and insulation. It is widely used in automobiles, aviation, electronics, daily necessities and medical fields. However, PP is a partially crystalline resin. Under normal processing conditions, the crystallization rate is relatively slow, and it is easy to form large spherulites, which makes it difficult for light to pass through the entire PP product. Therefore, the transparency and glossiness of PP products are poor, and the appearance lacks aesthetics, which limits its application in packaging, medical devices, household products and other fields. In order to improve the transparency of polypropylene, random copolymer polypropylene is generally used as the matrix, and a small amount of nucleating agent is added to obtain polypropylene with higher transparency. However, the mechanical strength of the transparent polypropylene obtained by this method is not high, which limits the application of transparent polypropylene. Adding a small amount of glass fiber or whisker can improve the mechanical strength of transparent polypropylene, but it has a great impact on the transparency of the product, and the haze value is significantly improved, which does not have practical application value.
[0003] Chinese patent application CN103030886A discloses a transparent polypropylene and a method for preparing the same. The method modifies polypropylene by compounding sorbitol and organic phosphate nucleating agents, thereby improving the transparency of polypropylene to a certain extent, but the mechanical strength of the material is not high. Chinese patent application CN103613853A discloses a transparent glass fiber reinforced polypropylene composite material and a method for preparing the same. The method greatly improves the mechanical strength of polypropylene through glass fiber, but the light transmittance is greatly reduced. Chinese patent application CN114316426A discloses a high modulus and high heat-resistant transparent polypropylene composition and a method for preparing the same. The method improves the mechanical strength of transparent polypropylene by introducing PMMA cross-linked microspheres, but does not solve the compatibility problem between PMMA and polypropylene, resulting in limited improvement in the mechanical strength of the material.
[0004] Improving the mechanical strength of polypropylene while maintaining good transparency and low haze is of great significance for improving the application prospects of transparent polypropylene. However, the existing technology has not achieved this goal. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned background technology and provide a high-strength, low-haze transparent polypropylene material and a preparation method thereof. The polypropylene material of the present invention is added with polymethyl methacrylate modified microspheres, which significantly improves the mechanical strength of polypropylene and maintains a high light transmittance of polypropylene. The prepared transparent polypropylene not only has excellent mechanical properties, but also has high light transmittance and low haze value.
[0006] To achieve the purpose of the present invention, the high-strength, low-fog, transparent polypropylene material of the present invention comprises, by weight:
[0007] Random copolymer polypropylene: 85-95 parts;
[0008] Polymethyl methacrylate modified microspheres: 8-12 parts;
[0009] Low density polyethylene copolymer: 2-5 parts;
[0010] Compatibilizer: 3-5 parts;
[0011] Antioxidant: 0.2-1 part;
[0012] Nucleating agent: 0.2-1 part;
[0013] Lubricant: 1-3 parts.
[0014] Further, in some embodiments of the present invention, the high-strength, low-haze, transparent polypropylene material of the present invention comprises, by weight:
[0015] Random copolymer polypropylene: 89-91 parts;
[0016] Polymethyl methacrylate modified microspheres: 9-11 parts;
[0017] Low density polyethylene copolymer: 2-5 parts;
[0018] Compatibilizer: 3-5 parts;
[0019] Antioxidant: 0.2-1 part;
[0020] Nucleating agent: 0.2-1 part;
[0021] Lubricant: 1-3 parts.
[0022] Furthermore, in some embodiments of the present invention, the polymethyl methacrylate modified microspheres are prepared by emulsion polymerization.
[0023] Furthermore, in some embodiments of the present invention, the random copolymer polypropylene has a melt index of 15-20 g / 10 min.
[0024] Furthermore, in some embodiments of the present invention, the low-density polyethylene copolymer has a melt index of 20-30 g / 10 min.
[0025] Furthermore, in some embodiments of the present invention, the compatibilizer is polystyrene grafted with maleic anhydride.
[0026] Furthermore, in some embodiments of the present invention, the antioxidant is one or more of a hindered phenol antioxidant and a phosphite antioxidant.
[0027] Furthermore, in some embodiments of the present invention, the nucleating agent is one or more of an acetal nucleating agent, a phosphate nucleating agent, and an amide nucleating agent.
[0028] Furthermore, in some embodiments of the present invention, the lubricant is one or more of zinc stearate, calcium stearate, and magnesium stearate.
[0029] Furthermore, in some embodiments of the present invention, the preparation method of the polymethyl methacrylate modified microspheres is: add water to a reaction container, stir and heat in a water bath in an inert gas atmosphere, add an emulsifier, phenyl methacrylate monomer, and methyl methacrylate monomer, and continue stirring. When the temperature reaches 68-72°C, add an initiator, raise the temperature to 78-82°C, continue stirring for 3-5 hours, then cool to room temperature, filter and dry to obtain polymethyl methacrylate modified microspheres.
[0030] Furthermore, in some embodiments of the present invention, the mass ratio of the emulsifier, phenyl methacrylate monomer, methyl methacrylate monomer, and initiator is 0.05-0.1: 5-10: 50-80: 0.1-0.5.
[0031] Furthermore, in some embodiments of the present invention, the emulsifier is one or more of sodium dodecyl sulfate, sodium dodecyl sulfonate, and sodium dodecylbenzene sulfonate.
[0032] Furthermore, in some embodiments of the present invention, the initiator is potassium persulfate.
[0033] On the other hand, the present invention also provides a method for preparing the above-mentioned high-strength, low-fog, transparent polypropylene material, the method comprising the following steps:
[0034] (1) preparing polymethyl methacrylate modified microspheres;
[0035] (2) adding random copolymerized polypropylene, polymethyl methacrylate modified microspheres, low-density polyethylene copolymer, compatibilizer, antioxidant, nucleating agent, and lubricant into a mixer according to required weight proportions and mixing them uniformly to obtain a mixed material;
[0036] (3) The mixture obtained in step (2) is added into a twin-screw extruder for extrusion, and water-cooled and pelletized to obtain the final product.
[0037] Furthermore, in some embodiments of the present invention, the temperature of zone 1 of the twin-screw extruder is 150-160°C, the temperature of zone 2 is 160-180°C, the temperature of zone 3 is 180-200°C, the temperature of zone 4 is 180-220°C, the temperature of zone 5 is 180-220°C, and the temperature of zone 6 is 180-200°C.
[0038] Compared with the prior art, the advantages of the present invention include but are not limited to:
[0039] (1) In the present invention, rigid groups are introduced into polymethyl methacrylate modified microspheres by emulsion polymerization, which significantly improves the mechanical strength of the modified microspheres;
[0040] (2) In the present invention, the polymethyl methacrylate modified microspheres are uniformly distributed in the polypropylene as a dispersed phase, which can absorb a large amount of energy when the material is impacted, thereby improving the toughness of the material;
[0041] (3) The polystyrene grafted maleic anhydride in the material of the present invention has good compatibility in the two phases, which can effectively improve the compatibility of polymethyl methacrylate and polypropylene, and further improve the mechanical strength of the material.
[0042] (4) The polymethyl methacrylate modified microspheres in the present invention maintain a high light transmittance of polypropylene, and the obtained transparent polypropylene not only has excellent mechanical properties, but also has high light transmittance and low haze value. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiments. Additional aspects and advantages of the present invention will be given in part in the following description, and part will become apparent from the following description, or will be understood through the practice of the present invention. It should be understood that the following description is only used to explain the present invention and is not intended to limit the present invention.
[0044] When amount, concentration or other value or parameter is expressed as range, preferred range or a series of upper preferred value and lower preferred value limit range, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value and any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when disclosing range "1 to 5", described range should be interpreted as including range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the range is intended to include its end value and all integers and fractions within the range.
[0045] Singular forms include plural references unless the context clearly indicates otherwise. "Optional" or "either" means that the subsequently described event or incident may or may not occur, and that the description includes instances where the event occurs and instances where it does not.
[0046] The indefinite articles "a" and "an" before the elements or components of the present invention have no limitation on the quantity requirements (i.e. the number of occurrences) of the elements or components. Therefore, "a" or "an" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the quantity obviously refers to the singular form only.
[0047] In addition, the description of the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" described in the present invention means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic expressions of the above terms do not necessarily refer to the same embodiment or example. Moreover, the technical features involved in the various embodiments of the present invention can be combined with each other as long as they do not conflict with each other.
[0048] Example 1
[0049] A high-strength, low-haze, transparent polypropylene material comprising:
[0050] Random copolymer polypropylene: 90 parts;
[0051] Polymethyl methacrylate modified microspheres: 10 parts;
[0052] Low density polyethylene copolymer: 2 parts;
[0053] Polystyrene grafted maleic anhydride: 3 parts;
[0054] Antioxidant 1010: 0.2 parts;
[0055] Acetal nucleating agent: 0.2 parts;
[0056] Zinc stearate: 1 part.
[0057] The preparation method of the above-mentioned high-strength low-fog transparent polypropylene material is as follows:
[0058] (1) Add 200 mL of deionized water to a three-necked flask filled with nitrogen, start stirring and heat in a water bath; add 0.05 g of sodium dodecyl sulfate, 5 g of phenyl methacrylate monomer, and 50 g of methyl methacrylate monomer to the three-necked flask, and continue stirring for 3 minutes; when the temperature reaches 70°C, add 0.1 g of potassium persulfate to the three-necked flask, raise the temperature to 80°C, and continue stirring for 3 hours; cool to room temperature, filter under reduced pressure, and place in an 80°C forced air drying oven for drying to obtain polymethyl methacrylate modified microspheres.
[0059] (2) adding 90 parts of random copolymer polypropylene with a melt index of 15 g / 10 min, 10 parts of polymethyl methacrylate modified microspheres obtained in step (1), 2 parts of low-density polyethylene copolymer with a melt index of 20 g / 10 min, 3 parts of polystyrene grafted maleic anhydride, 0.2 parts of antioxidant 1010, 0.2 parts of acetal nucleating agent, and 1 part of zinc stearate into a mixer and mixing well to obtain a mixed material;
[0060] (3) adding the mixed material into a twin-screw extruder for extrusion, wherein the extrusion process of the twin-screw extruder is as follows: the temperature of the first zone is 150° C., the temperature of the second zone is 160° C., the temperature of the third zone is 180° C., the temperature of the fourth zone is 180° C., the temperature of the fifth zone is 180° C., the temperature of the sixth zone is 180° C., and water-cooling and pelletizing are performed to obtain the final product.
[0061] Example 2
[0062] A high-strength, low-haze, transparent polypropylene material comprising:
[0063] Random copolymer polypropylene: 90 parts;
[0064] Polymethyl methacrylate modified microspheres: 10 parts;
[0065] Low density polyethylene copolymer: 2 parts;
[0066] Polystyrene grafted maleic anhydride: 4 parts;
[0067] Antioxidant 1010: 0.1 part;
[0068] Antioxidant 168: 0.1 part;
[0069] Phosphate nucleating agent: 0.5 parts;
[0070] Calcium stearate: 2 parts.
[0071] The preparation method of the above-mentioned high-strength low-fog transparent polypropylene material is as follows:
[0072] (1) Add 200 mL of deionized water to a three-necked flask filled with nitrogen, start stirring and heat in a water bath; add 0.08 g of sodium dodecyl sulfonate, 8 g of phenyl methacrylate monomer, and 60 g of methyl methacrylate monomer to the three-necked flask, and continue stirring for 4 minutes; when the temperature reaches 70°C, add 0.3 g of potassium persulfate to the three-necked flask, raise the temperature to 80°C, and continue stirring for 3 hours; cool to room temperature, filter under reduced pressure, and place in an 80°C forced air drying oven for drying to obtain polymethyl methacrylate modified microspheres.
[0073] (2) adding 90 parts of random copolymer polypropylene with a melt index of 20 g / 10 min, 10 parts of polymethyl methacrylate modified microspheres obtained in step (1), 2 parts of low-density polyethylene copolymer with a melt index of 30 g / 10 min, 4 parts of polystyrene grafted maleic anhydride, 0.1 parts of antioxidant 1010, 0.1 parts of antioxidant 168, 0.5 parts of phosphate nucleating agent, and 2 parts of calcium stearate into a mixer and mixing well to obtain a mixed material;
[0074] (3) adding the mixed material into a twin-screw extruder for extrusion, wherein the extrusion process of the twin-screw extruder is as follows: the temperature of the first zone is 160° C., the temperature of the second zone is 170° C., the temperature of the third zone is 190° C., the temperature of the fourth zone is 200° C., the temperature of the fifth zone is 210° C., the temperature of the sixth zone is 190° C., and water-cooling and pelletizing are performed to obtain the final product.
[0075] Example 3
[0076] A high-strength, low-haze, transparent polypropylene material comprising:
[0077] Random copolymer polypropylene: 90 parts;
[0078] Polymethyl methacrylate modified microspheres: 10 parts;
[0079] Low density polyethylene copolymer: 5 parts;
[0080] Polystyrene grafted maleic anhydride: 5 parts;
[0081] Antioxidant 168: 0.2 parts;
[0082] Amide nucleating agent: 1 part;
[0083] Magnesium stearate: 3 parts.
[0084] The preparation method of the above-mentioned high-strength low-fog transparent polypropylene material is as follows:
[0085] (1) Add 200 mL of deionized water to a three-necked flask filled with nitrogen, start stirring and heat in a water bath; add 0.1 g of sodium dodecylbenzene sulfonate, 10 g of phenyl methacrylate monomer, and 80 g of methyl methacrylate monomer to the three-necked flask, and continue stirring for 4 minutes; when the temperature reaches 70°C, add 0.5 g of potassium persulfate to the three-necked flask, raise the temperature to 80°C, and continue stirring for 5 hours; cool to room temperature, filter under reduced pressure, and place in an 80°C forced air drying oven for drying to obtain polymethyl methacrylate modified microspheres.
[0086] (2) adding 90 parts of random copolymer polypropylene with a melt index of 20 g / 10 min, 10 parts of polymethyl methacrylate modified microspheres obtained in step (1), 5 parts of low-density polyethylene copolymer with a melt index of 30 g / 10 min, 5 parts of polystyrene grafted maleic anhydride, 0.2 parts of antioxidant 168, 1 part of amide nucleating agent, and 3 parts of magnesium stearate into a mixer and mixing well to obtain a mixed material;
[0087] (3) adding the mixed material into a twin-screw extruder for extrusion, wherein the extrusion process of the twin-screw extruder is as follows: the temperature of the first zone is 160° C., the temperature of the second zone is 180° C., the temperature of the third zone is 200° C., the temperature of the fourth zone is 220° C., the temperature of the fifth zone is 220° C., the temperature of the sixth zone is 200° C., and water-cooling and pelletizing are performed to obtain the final product.
[0088] Comparative Example 1
[0089] A polypropylene material, comprising:
[0090] Random copolymer polypropylene: 90 parts;
[0091] Low density polyethylene copolymer: 2 parts;
[0092] Polystyrene grafted maleic anhydride: 3 parts;
[0093] Antioxidant 1010: 0.2 parts;
[0094] Acetal nucleating agent: 0.2 parts;
[0095] Zinc stearate: 1 part.
[0096] The preparation method of the above-mentioned polypropylene material is as follows:
[0097] (1) 90 parts of random copolymer polypropylene with a melt index of 15 g / 10 min, 2 parts of low-density polyethylene copolymer with a melt index of 20 g / 10 min, 3 parts of polystyrene grafted maleic anhydride, 0.2 parts of antioxidant 1010, 0.2 parts of acetal nucleating agent, and 1 part of zinc stearate are added into a mixer and mixed uniformly to obtain a mixed material;
[0098] (2) adding the mixed material into a twin-screw extruder for extrusion, wherein the extrusion process of the twin-screw extruder is as follows: the temperature of the first zone is 150° C., the temperature of the second zone is 160° C., the temperature of the third zone is 180° C., the temperature of the fourth zone is 180° C., the temperature of the fifth zone is 180° C., the temperature of the sixth zone is 180° C., and water-cooling and pelletizing are performed to obtain the final product.
[0099] Comparative Example 2
[0100] A polypropylene material, comprising:
[0101] Random copolymer polypropylene: 90 parts;
[0102] Polymethyl methacrylate modified microspheres: 10 parts;
[0103] Low density polyethylene copolymer: 2 parts;
[0104] Polypropylene grafted maleic anhydride: 4 parts;
[0105] Antioxidant 1010: 0.1 part;
[0106] Antioxidant 168: 0.1 part;
[0107] Phosphate nucleating agent: 0.5 parts;
[0108] Calcium stearate: 2 parts.
[0109] The preparation method of the above-mentioned polypropylene material is as follows:
[0110] (1) Add 200 mL of deionized water to a three-necked flask filled with nitrogen, start stirring and heat in a water bath; add 0.08 g of sodium dodecyl sulfonate, 8 g of phenyl methacrylate monomer, and 60 g of methyl methacrylate monomer to the three-necked flask, and continue stirring for 4 minutes; when the temperature reaches 70°C, add 0.3 g of potassium persulfate to the three-necked flask, raise the temperature to 80°C, and continue stirring for 3 hours; cool to room temperature, filter under reduced pressure, and place in an 80°C forced air drying oven for drying to obtain polymethyl methacrylate modified microspheres.
[0111] (2) adding 90 parts of random copolymer polypropylene with a melt index of 20 g / 10 min, 10 parts of polymethyl methacrylate modified microspheres obtained in step (1), 2 parts of low-density polyethylene copolymer with a melt index of 30 g / 10 min, 4 parts of polypropylene grafted maleic anhydride, 0.1 parts of antioxidant 1010, 0.1 parts of antioxidant 168, 0.5 parts of phosphate nucleating agent, and 2 parts of calcium stearate into a mixer and mixing well to obtain a mixed material;
[0112] (3) adding the mixed material into a twin-screw extruder for extrusion, wherein the extrusion process of the twin-screw extruder is as follows: the temperature of the first zone is 160° C., the temperature of the second zone is 170° C., the temperature of the third zone is 190° C., the temperature of the fourth zone is 200° C., the temperature of the fifth zone is 210° C., the temperature of the sixth zone is 190° C., and water-cooling and pelletizing are performed to obtain the final product.
[0113] Comparative Example 3
[0114] A polypropylene material, comprising:
[0115] Random copolymer polypropylene: 90 parts;
[0116] MX-1500 polymethyl methacrylate cross-linked microspheres: 10 parts;
[0117] Low density polyethylene copolymer: 2 parts;
[0118] Polystyrene grafted maleic anhydride: 3 parts;
[0119] Antioxidant 1010: 0.2 parts;
[0120] Acetal nucleating agent: 0.2 parts;
[0121] Zinc stearate: 1 part.
[0122] The preparation method of the above-mentioned polypropylene material is as follows:
[0123] (1) adding 90 parts of random copolymer polypropylene with a melt index of 20 g / 10 min, 10 parts of MX-1500 polymethyl methacrylate crosslinked microspheres, 5 parts of low-density polyethylene copolymer with a melt index of 30 g / 10 min, 5 parts of polystyrene grafted maleic anhydride, 0.2 parts of antioxidant 168, 1 part of amide nucleating agent, and 3 parts of magnesium stearate into a mixer and mixing uniformly to obtain a mixed material;
[0124] (2) adding the mixed material into a twin-screw extruder for extrusion, wherein the extrusion process of the twin-screw extruder is as follows: the temperature of the first zone is 160° C., the temperature of the second zone is 180° C., the temperature of the third zone is 200° C., the temperature of the fourth zone is 220° C., the temperature of the fifth zone is 220° C., the temperature of the sixth zone is 200° C., and water-cooling and pelletizing are performed to obtain the final product.
[0125] The evaluation results of the above-mentioned application examples 1-3 and comparative examples 1-3 are shown in Table 1.
[0126] Table 1: Test results of various embodiments and comparative embodiments
[0127]
[0128] From the above test results, it can be seen that the polypropylene materials obtained in Examples 1-3 of the present invention have excellent light transmittance, low haze and high mechanical strength. Comparing Example 1 with Comparative Example 1, it can be seen that the polymethyl methacrylate modified microspheres can significantly improve the mechanical strength of polypropylene and maintain a high light transmittance of polypropylene; Comparing Example 2 with Comparative Example 2, it can be seen that compared with conventional polypropylene compatibilizers, the compatibilizer polystyrene grafted maleic anhydride can effectively improve the compatibility of polypropylene and polymethyl methacrylate modified microspheres, improve the mechanical strength of the material, and is more suitable for the modification of the transparent polypropylene material of the present invention. Comparing Example 3 with Comparative Example 3, it can be seen that compared with the commercially available polymethyl methacrylate cross-linked microspheres, the polymethyl methacrylate modified microspheres of the present invention have a more significant improvement in the mechanical strength of the transparent polypropylene material and a better light transmittance.
[0129] Those skilled in the art will easily understand that the above descriptions are merely embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high-strength, low-fog, transparent polypropylene material, characterized in that: The high-strength, low-fog, transparent polypropylene material comprises, by weight: Random copolymer polypropylene: 85-95 parts; Polymethyl methacrylate modified microspheres: 8-12 parts; Low density polyethylene copolymer: 2-5 parts; Compatibilizer: 3-5 parts; Antioxidant: 0.2-1 part; Nucleating agent: 0.2-1 part; Lubricant: 1-3 parts; The preparation method of the polymethyl methacrylate modified microspheres is as follows: water is added into a reaction container, stirred and heated in a water bath in an inert gas atmosphere, an emulsifier, a phenyl methacrylate monomer, and a methyl methacrylate monomer are added, and stirring is continued; when the temperature reaches 68-72° C., an initiator is added, the temperature is raised to 78-82° C., stirring is continued for 3-5 hours, and then the temperature is lowered to room temperature, filtered, and dried to obtain polymethyl methacrylate modified microspheres; The compatibilizer is polystyrene grafted with maleic anhydride.
2. The high-strength, low-haze, transparent polypropylene material according to claim 1, characterized in that: The antioxidant is one or more of a hindered phenol antioxidant and a phosphite antioxidant.
3. The high-strength, low-haze, transparent polypropylene material according to claim 1, characterized in that: The nucleating agent is one or more of an acetal nucleating agent, a phosphate nucleating agent, and an amide nucleating agent.
4. The high-strength, low-haze, transparent polypropylene material according to claim 1, characterized in that: The lubricant is one or more of zinc stearate, calcium stearate and magnesium stearate.
5. The high-strength, low-haze, transparent polypropylene material according to claim 1, characterized in that: The mass ratio of the emulsifier, phenyl methacrylate monomer, methyl methacrylate monomer and initiator is 0.05-0.1:5-10:50-80:0.1-0.
5.
6. The high-strength, low-haze, transparent polypropylene material according to claim 1, characterized in that: The emulsifier is one or more of sodium dodecyl sulfate, sodium dodecyl sulfonate, and sodium dodecylbenzene sulfonate.
7. The high-strength, low-haze, transparent polypropylene material according to claim 1, characterized in that: The initiator is potassium persulfate.
8. The method for preparing the high-strength, low-fog, transparent polypropylene material according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: (1) preparing polymethyl methacrylate modified microspheres; (2) adding random copolymerized polypropylene, polymethyl methacrylate modified microspheres, low-density polyethylene copolymer, compatibilizer, antioxidant, nucleating agent, and lubricant into a mixer according to required weight proportions and mixing them uniformly to obtain a mixed material; (3) The mixture obtained in step (2) is added into a twin-screw extruder for extrusion, and water-cooled and pelletized to obtain the final product.
9. The method for preparing the high-strength, low-fog, transparent polypropylene material according to claim 8, characterized in that: The temperature of the twin-screw extruder zone 1 is 150-160°C, the temperature of zone 2 is 160-180°C, the temperature of zone 3 is 180-200°C, the temperature of zone 4 is 180-220°C, the temperature of zone 5 is 180-220°C, and the temperature of zone 6 is 180-200°C.
Citation Information
Patent Citations
Transparent polypropylene and preparing method thereof
CN103030886A
Transparent glass fiber reinforced polypropylene (PP) composite material and preparation method thereof
CN103613853A
High-modulus high-heat-resistance transparent polypropylene composition and preparation method thereof
CN114316426A
Transparent ageing-resistant water cup and preparation method thereof
CN106349572A
High-transparency and anti-impact polypropylene material and preparation method thereof
CN108456366A