Yellowing-resistant polyvinyl butyral and preparation method thereof
By combining polyvinyl butyral resin with modifier and hydroxypropyl methylcellulose, treatment with ultrasonic dispersion and silane coupling agent, yellow-resistant polyvinyl butyral with high light stability and thermal stability is formed , solves the problems of poor yellowing resistance and heat resistance in the prior art, and achieves good mechanical properties and environmental protection properties.
Patent Information
- Application Number
- CN202310593366.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-05-24
AI Technical Summary
The existing polyvinyl butyral resin has poor yellowing and heat resistance and insufficient mechanical properties, which leads to aging, degradation and yellowing during storage or use. The commonly used yellowing and resistance technology is costly and environmentally friendly. Harmful and anti-yellowing effect is poor.
By combining polyvinyl butyral resin with modifier and hydroxypropyl methylcellulose, a resin solution is formed, and ultrasonic dispersion, silane coupling agent and grafting agent are used to form a resin solution with enhanced light stability and Thermal stability of yellowing resistance to polyvinyl butyral.
Effectively delay the aging and yellowing of polyvinyl butyral, improve its mechanical properties and high temperature resistance, and the preparation method is simple and low-cost. The modifiers used and hydroxypropyl methylcellulose have good environmental protection. performance.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer material preparation, in particular to yellowing-resistant polyvinyl butyral and a preparation method thereof. Background Art
[0002] Polyvinyl butyral (PVB) is a thermoplastic resin, a condensation product of vinyl alcohol and butyraldehyde. Its chemical structure contains a large number of hydroxyl and methylene groups, which give it excellent processing properties, optical properties, mechanical properties, bonding properties and weather resistance. It is widely used in glass bonding, packaging materials, coatings, optical films, textile coatings, electronic materials and other fields. However, due to the residual impurities such as acid and butyraldehyde in PVB resin, it is prone to aging and degradation during storage or use, resulting in yellowing problems.
[0003] Yellowing-resistant polyvinyl butyral is a polymer material with good durability and stability. At present, the commonly used preparation technologies of yellowing-resistant polyvinyl butyral mainly include the following: UV stabilizer method, by adding UV stabilizers to improve the yellowing resistance of polyvinyl butyral. Heat stabilizer method, by adding heat stabilizers, such as dithiophenol (DNTP), zinc oxide, calcium oxide, etc., to improve the heat resistance and stability of polyvinyl butyral. Photooxidant method, by adding photooxidants, such as benzoyl peroxide, acetone peroxide, etc., to promote the oxidation reaction of polyvinyl butyral, thereby improving its yellowing resistance. Oxidant-reducing agent composite method, by adding a composite system of oxidants and reductants, such as sodium thiosulfate / sodium sulfite composite system, hydrogen peroxide / sodium sulfite composite system, etc., to improve the yellowing resistance of polyvinyl butyral.
[0004] Although the currently commonly used anti-yellowing technology can improve its durability and stability, it still has some disadvantages, including high cost, harmful to the environment, poor anti-yellowing effect, insufficient heat resistance, and poor mechanical properties.
[0005] The invention patent application CN113880971A discloses a method for preparing a yellowing-resistant polyvinyl butyral resin. The method comprises the following steps: adding polyvinyl alcohol and water into a dissolving kettle, heating the temperature to 90°C to 98°C, stirring and dissolving, filtering, cooling the temperature to 35°C to 50°C, adding n-butyraldehyde and stirring to obtain a polyvinyl alcohol / n-butyraldehyde mixed solution; respectively introducing the polyvinyl alcohol / n-butyraldehyde mixed solution and a hydrochloric acid aqueous solution into a tubular reactor at a temperature of 35°C to 50°C for reaction, transferring the materials into an aging kettle at a temperature of 35°C to 50°C for reaction, adding a hydrochloric acid aqueous solution, heating the temperature to 55°C to 70°C for reaction; adding a sodium hydroxide aqueous solution to make the reaction solution pH=10, filtering, washing the solid with water and drying to obtain a yellowing-resistant polyvinyl butyral resin; the yellowing-resistant polyvinyl butyral resin obtained by the invention does not turn yellow after being baked in an electric constant temperature blast drying oven at 200°C for 1h, and is suitable for automobile windshields, building safety glass, etc. However, the yellowing resistance of the yellowing-resistant polyvinyl butyral resin prepared by the invention is still poor, and the mechanical properties are insufficient. Summary of the invention
[0006] In view of the disadvantages of the prior art polyvinyl butyral resin in terms of poor yellowing resistance and heat resistance and low mechanical properties, the technical problem to be solved by the present invention is to provide a yellowing-resistant polyvinyl butyral with good yellowing resistance and heat resistance and strong mechanical properties and a preparation method thereof.
[0007] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:
[0008] A method for preparing yellowing-resistant polyvinyl butyral is as follows:
[0009] The polyvinyl butyral resin is added into a solvent to form a resin solution, and then a modifier and hydroxypropyl methylcellulose are added, stirred, heated and stirred to remove the solvent, and yellowing-resistant polyvinyl butyral is obtained.
[0010] The preparation method of the yellowing-resistant polyvinyl butyral is as follows, in parts by weight:
[0011] Add 4-6 parts of polyvinyl butyral resin to 80-120 parts of solvent to form a resin solution, then add a modifier and hydroxypropyl methylcellulose, stir at 100-500 rpm for 0.5-2h, heat to 50-70°C, stir at 100-300 rpm to remove the solvent, and obtain yellowing-resistant polyvinyl butyral.
[0012] Preferably, the solvent is at least one of methanol, ethanol, isopropanol, N,N-dimethylformamide, and N-methyl-2-pyrrolidone.
[0013] Preferably, the mass of the modifier is 1-3% of the mass of the resin solution; the mass of the hydroxypropyl methylcellulose is 0.5-2% of the mass of the resin solution.
[0014] The preparation method of the modifier is as follows:
[0015] S1. Ultrasonic dispersion of the powder in anhydrous ethanol, then adding silane coupling agent KH-550, stirring and refluxing, centrifuging, collecting the solid, washing, and drying to obtain a composite material;
[0016] S2, adding cinnamic acid to thionyl chloride, refluxing under nitrogen, and then evaporating under reduced pressure to obtain a grafting agent;
[0017] S3, adding the grafting agent and triethylamine prepared in step S2 to the composite material dispersion, reacting at room temperature, centrifuging, washing, and drying to obtain a modifier.
[0018] Preferably, the preparation method of the modifier is as follows, in parts by weight:
[0019] S1. Ultrasonic dispersion of 0.4-0.8 parts of powder in 80-120 parts of anhydrous ethanol, with an ultrasonic time of 0.3-0.8 h, an ultrasonic power of 100-400 W, and an ultrasonic frequency of 40-60 kHz, and then adding 0.4-0.8 parts of silane coupling agent KH-550, stirring and refluxing at 60-90 ° C and 100-500 rpm for 5-24 h, centrifuging at 6000-12000 rpm for 3-10 min, collecting the solid, washing it with anhydrous ethanol for 1-3 times, and drying it in a vacuum oven at 60-90 ° C for 5-24 h to obtain a composite material;
[0020] S2, adding 0.5-2 parts of cinnamic acid to 8-12 parts of thionyl chloride, reflux for 2-6 hours under nitrogen, and then evaporate under reduced pressure to obtain a grafting agent;
[0021] S3. Add 0.1-0.3 parts of the grafting agent prepared in step S2 and 0.5-2 parts of triethylamine to 40-60 parts of the composite material dispersion, react at room temperature for 10-30 hours, centrifuge at 6000-12000 rpm for 3-10 minutes, wash with anhydrous ethanol 1-3 times, and dry in a vacuum oven at 60-85° C. for 1-6 hours to obtain a modifier.
[0022] Preferably, the powder is at least one of silicon dioxide, talc, aluminum hydroxide and calcium carbonate.
[0023] Preferably, the concentration of the composite material dispersion is 8-12 mg / mL, and the composite material dispersion is prepared by adding the composite material prepared in step S1 into tetrahydrofuran.
[0024] Preferably, in step S2, the reduced pressure evaporation is performed for 1 to 3 hours, the vacuum degree of the reduced pressure evaporation is 0.03 to 0.05 MPa, and the reduced pressure evaporation temperature is 80 to 90°C.
[0025] The present invention forms a resin solution by adding polyvinyl butyral resin to N,N-dimethylformamide, then adding a modifier and hydroxypropyl methylcellulose to the resin solution, stirring at room temperature, and stirring at elevated temperature to obtain yellowing-resistant polyvinyl butyral. The polyvinyl butyral resin is prepared by using polyvinyl alcohol and n-butyraldehyde under acidic conditions, and then filtered and centrifuged under alkaline conditions to obtain the modifier. The modifier is prepared by ultrasonically dispersing aluminum hydroxide in anhydrous ethanol, then adding a silane coupling agent, stirring and refluxing, centrifuging, washing, and drying to obtain a composite material; adding cinnamic acid to thionyl chloride, refluxing, and then evaporating under reduced pressure to obtain a grafting agent; adding the grafting agent and triethylamine to a composite material dispersion, reacting at room temperature, centrifuging, washing, and drying to obtain the modifier.
[0026] When yellowing-resistant polyvinyl butyral is exposed to light, due to the pumping effect of the unsaturated bonds in cinnamic acid, photoelectrons will be transferred from aluminum hydroxide to cinnamic acid, which will promote the separation of photogenerated electron-hole pairs in aluminum hydroxide and enhance the absorption of light. The cinnamic groups on the surface of aluminum hydroxide also promote the dispersion of aluminum hydroxide in N,N-dimethylformamide, thereby reducing the visible light scattering caused by agglomeration. The addition of silane coupling agent is conducive to reducing the agglomeration of aluminum hydroxide.
[0027] The strengthening effect is mainly due to the transfer of load from the polyvinyl butyral matrix to the rigid aluminum hydroxide. The rigid group benzene ring on the surface of aluminum hydroxide further promotes the reinforcing effect of the modifier on the polyvinyl butyral matrix, thereby improving the tensile strength. However, the addition of rigid aluminum hydroxide will inevitably lead to a reduction in elongation at break, because the rigid structure will limit the movement of the polyvinyl butyral molecular chain. The yellowing-resistant polyvinyl butyral film prepared by the present invention still maintains a higher elongation at break under the same load, which is due to the addition of modifiers and hydroxypropyl methylcellulose aqueous solution, which can improve the dispersibility and interfacial compatibility of polyvinyl butyral resin, thereby improving the elongation at break of the material.
[0028] Hydroxypropyl methylcellulose is a water-soluble polymer compound. In the preparation process of yellowing-resistant polyvinyl butyral resin, adding hydroxypropyl methylcellulose aqueous solution can reduce yellowing due to light exposure. This is mainly because the hydroxypropyl methylcellulose molecule contains functional groups such as hydroxyl and methyl, which can form hydrogen bonds with polyvinyl butyral resin and form a protective layer on the resin surface, thereby improving the light stability of the resin and slowing down the yellowing rate due to light exposure. In addition, the hydroxypropyl methylcellulose molecule contains a certain amount of free radical scavengers, which can effectively remove free radicals generated in the resin, reduce the oxidation reaction caused by free radicals, and delay the molecular chain breakage and oxidative degradation of polyvinyl butyral to a certain extent, thereby delaying the aging and yellowing of yellowing-resistant polyvinyl butyral.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] 1) In the present invention, polyvinyl butyral resin is added to N,N-dimethylformamide to form a resin solution, and then a modifier and hydroxypropyl methylcellulose are added to the resin solution, and the mixture is stirred at room temperature and stirred at elevated temperature to obtain yellowing-resistant polyvinyl butyral; the aging and yellowing of the yellowing-resistant polyvinyl butyral are effectively delayed, and good mechanical properties are imparted.
[0031] 2) The addition of the modifier in the present invention can increase the initial decomposition temperature of polyvinyl butyral through various mechanisms, thereby making it have better high temperature resistance.
[0032] 3) The preparation method of the present invention is simple, easy to operate, can be carried out under conventional conditions, and has low cost.
[0033] 4) The modifier and hydroxypropyl methylcellulose aqueous solution used in the present invention also have good environmental performance. DETAILED DESCRIPTION
[0034] Main sources of substances:
[0035] Polyvinyl butyral resin: Shanghai Yunhe Material Technology Co., Ltd., model: BH-6.
[0036] Hydroxypropyl methylcellulose: Langfang Feitai New Material Technology Co., Ltd., model: 001.
[0037] Aluminum hydroxide, particle size: 40~80nm.
[0038] Silica, particle size: 20 nm.
[0039] Example 1
[0040] A method for preparing yellowing-resistant polyvinyl butyral is as follows:
[0041] Add 5g of polyvinyl butyral resin to 100g of N,N-dimethylformamide to form a resin solution, then add 2% of the mass of the resin solution by weight of a modifier and 1% of the mass of the resin solution by weight of hydroxypropyl methylcellulose, stir at 300rpm for 1h, heat to 80°C, stir at 200rpm to remove the solvent, and obtain yellowing-resistant polyvinyl butyral.
[0042] The preparation method of the modifier is as follows:
[0043] S1. Ultrasonic dispersion of 0.6 g aluminum hydroxide in 100 g anhydrous ethanol, with an ultrasonic time of 0.5 h, an ultrasonic power of 200 W, and an ultrasonic frequency of 60 kHz, followed by addition of 0.6 g silane coupling agent KH-550, stirring and reflux at 80 ° C and 200 rpm for 12 h, centrifugation at 8000 rpm for 5 min, collecting the solid, washing it with anhydrous ethanol for 3 times, and drying it in a vacuum oven at 80 ° C for 12 h to obtain a composite material;
[0044] S2, adding 1g of cinnamic acid to 10g of thionyl chloride, reflux under nitrogen for 4h, and then evaporate under reduced pressure for 2h, the vacuum degree of reduced pressure evaporation is 0.04MPa, and the reduced pressure evaporation temperature is 85°C to obtain a grafting agent;
[0045] S3. Add 0.2 g of the grafting agent prepared in step S2 and 1 g of triethylamine to 50 g of a 10 mg / mL composite material dispersion, wherein the composite material dispersion is prepared by adding the composite material prepared in step S1 to tetrahydrofuran, react at room temperature for 24 h, centrifuge at 8000 rpm for 5 min, wash with anhydrous ethanol for 3 times, and dry in a vacuum oven at 70° C. for 3 h to obtain a modifier.
[0046] Example 2
[0047] The preparation method of yellowing-resistant polyvinyl butyral is basically the same as that of Example 1, with the only difference being that the preparation method of the modifier is different.
[0048] The preparation method of the modifier is as follows:
[0049] S1. Ultrasonic dispersion of 0.6 g aluminum hydroxide in 100 g anhydrous ethanol, with an ultrasonic time of 0.5 h, an ultrasonic power of 200 W, and an ultrasonic frequency of 60 kHz, followed by addition of 0.6 g silane coupling agent KH-550, stirring and reflux at 80 ° C and 200 rpm for 12 h, centrifugation at 8000 rpm for 5 min, collecting the solid, washing it with anhydrous ethanol for 3 times, and drying it in a vacuum oven at 80 ° C for 12 h to obtain a composite material;
[0050] S2. Add 1 g of triethylamine to 50 g of a 10 mg / mL composite material dispersion, wherein the composite material dispersion is prepared by adding the composite material prepared in step S1 to tetrahydrofuran, react at room temperature for 24 h, centrifuge at 8000 rpm for 5 min, wash with anhydrous ethanol for 3 times, and dry in a vacuum oven at 70° C. for 3 h to obtain a modifier.
[0051] The preparation method of the yellowing-resistant polyvinyl butyral is the same as that in Example 1.
[0052] Example 3
[0053] The preparation method of yellowing-resistant polyvinyl butyral is basically the same as that of Example 1, with the only difference being that the preparation method of the modifier is different.
[0054] The preparation method of the modifier is as follows:
[0055] S1. Ultrasonic dispersion of 0.6 g of silicon dioxide in 100 g of anhydrous ethanol, with an ultrasonic time of 0.5 h, an ultrasonic power of 200 W, and an ultrasonic frequency of 60 kHz, followed by addition of 0.6 g of silane coupling agent KH-550, stirring and reflux at 80 ° C and 200 rpm for 12 h, centrifugation at 8000 rpm for 5 min, collecting the solid, washing it with anhydrous ethanol for 3 times, and drying it in a vacuum oven at 80 ° C for 12 h to obtain a composite material;
[0056] S2, adding 1g of cinnamic acid to 10g of thionyl chloride, reflux under nitrogen for 4h, and then evaporate under reduced pressure for 2h, the vacuum degree of reduced pressure evaporation is 0.04MPa, and the reduced pressure evaporation temperature is 85°C to obtain a grafting agent;
[0057] S3. Add 0.2 g of the grafting agent prepared in step S2 and 1 g of triethylamine to 50 g of a 10 mg / mL composite material dispersion, wherein the composite material dispersion is prepared by adding the composite material prepared in step S1 to tetrahydrofuran, react at room temperature for 24 h, centrifuge at 8000 rpm for 5 min, wash with anhydrous ethanol for 3 times, and dry in a vacuum oven at 70° C. for 3 h to obtain a modifier.
[0058] The preparation method of the yellowing-resistant polyvinyl butyral is the same as that in Example 1.
[0059] Example 4
[0060] A method for preparing yellowing-resistant polyvinyl butyral is substantially the same as that in Example 1, with the only difference being that the method for preparing the yellowing-resistant polyvinyl butyral is different.
[0061] A method for preparing yellowing-resistant polyvinyl butyral is as follows:
[0062] 5 g of polyvinyl butyral resin was added to 100 g of N,N-dimethylformamide to form a resin solution. Then, a modifier whose mass was 2% of the mass of the resin solution was added to the resin solution. The mixture was stirred at 300 rpm for 1 hour. The temperature was raised to 60° C. and the solvent was removed by stirring at 200 rpm to obtain yellowing-resistant polyvinyl butyral.
[0063] The preparation method of the modifier is the same as that of Example 1.
[0064] Comparative Example 1
[0065] A method for preparing yellowing-resistant polyvinyl butyral is as follows:
[0066] 5 g of polyvinyl butyral resin was added to 100 g of N,N-dimethylformamide to form a resin solution, and then a modifier was added in an amount of 2% by mass of the resin solution, and the mixture was stirred at 300 rpm for 1 hour. The mixture was heated to 80° C. and stirred at 200 rpm to remove the solvent to obtain yellowing-resistant polyvinyl butyral.
[0067] The preparation method of the modifier is as follows:
[0068] S1. Ultrasonic dispersion of 0.6 g of silicon dioxide in 100 g of anhydrous ethanol, with an ultrasonic time of 0.5 h, an ultrasonic power of 200 W, and an ultrasonic frequency of 60 kHz, followed by addition of 0.6 g of silane coupling agent KH-550, stirring and reflux at 80 ° C and 200 rpm for 12 h, centrifugation at 8000 rpm for 5 min, collecting the solid, washing it with anhydrous ethanol for 3 times, and drying it in a vacuum oven at 80 ° C for 12 h to obtain a composite material;
[0069] S2. Add 1 g of triethylamine to 50 g of a 10 mg / mL composite material dispersion, wherein the composite material dispersion is prepared by adding the composite material prepared in step S1 to tetrahydrofuran, react at room temperature for 24 h, centrifuge at 8000 rpm for 5 min, wash with anhydrous ethanol for 3 times, and dry in a vacuum oven at 70° C. for 3 h to obtain a modifier.
[0070] Comparative Example 2
[0071] A method for preparing yellowing-resistant polyvinyl butyral is as follows:
[0072] 5 g of polyvinyl butyral resin was added to 100 g of N,N-dimethylformamide to form a resin solution, which was then stirred at 300 rpm for 1 hour, heated to 80° C., and stirred at 200 rpm to remove the solvent to obtain yellowing-resistant polyvinyl butyral.
[0073] Test Example 1
[0074] Yellowing resistance test
[0075] Weigh 2000g of the yellowing-resistant polyvinyl butyral prepared by the present invention, spread it on the surface of 6cm×6cm, 2mm thick white float glass, put it into an electric constant temperature blast drying oven at 180℃ and bake it for 2h. Each group of samples has 3 samples. After the samples are taken out and cooled, observe whether the samples turn yellow and the degree of yellowing with the naked eye under a fluorescent lamp. Each group is tested three times, and the sample with the highest frequency is taken to evaluate the degree of yellowing, and the average value is taken. The test results are shown in Table 1.
[0076] Table 1: Yellowing resistance test results
[0077] Trial plan Yellowing degree Example 1 No obvious yellowing Example 2 Slight yellowing Example 3 Slight yellowing Example 4 Slight yellowing Comparative Example 1 Partially yellowed Comparative Example 2 A lot of yellowing
[0078] Test Example 2
[0079] Mechanical properties test
[0080] The yellowing-resistant polyvinyl butyral prepared by the present invention is made into a yellowing-resistant polyvinyl butyral film according to the requirements of GB / T 32020-2015 "Polyvinyl butyral interlayer film for laminated glass", and the tensile strength and elongation at break of the film are analyzed and tested, and the elongation at break and tensile strength of the film are tested with a universal testing machine. Test conditions: temperature 23°C, relative humidity 70%, tensile rate 20mm / min. The analysis and test results are compared with those of the standard polyvinyl butyral film.
[0081] Each group was tested three times and the average value was taken. The test results are shown in Table 2.
[0082] Table 2: Mechanical properties test results
[0083] Trial plan Tensile strength / MPa Elongation at break / % Example 1 24.92 239.21 Example 2 22.47 219.03 Example 3 22.03 216.82 Example 4 22.15 217.92 Comparative Example 1 21.61 209.51 Comparative Example 2 20.06 202.05 Standard value 20.00 200.00
[0084] Test Example 3
[0085] Initial decomposition temperature test
[0086] The decomposition temperature test adopts the thermogravimetric analysis (TGA) method, and the instrument adopts the TGA550 thermogravimetric analyzer to test the thermal stability of the material, the heating rate is 10°C / min, the heating range is 40-700°C, 5 mg of the yellowing-resistant polyvinyl butyral prepared by the present invention is weighed, and nitrogen is used as the protective gas and the purge gas, and the gas flow rates are 10 mL / min and 50 mL / min respectively. Determine the initial decomposition temperature. Each group is tested three times and the average value is taken. The test results are shown in Table 3.
[0087] Table 3: Initial decomposition temperature test results
[0088] Trial plan Initial decomposition temperature (℃) Example 1 154.5 Example 2 133.7 Example 3 136.1 Example 4 131.4 Comparative Example 1 122.4 Comparative Example 2 103.4 Standard value 20.00
[0089] From the test results of test examples 1 to 3, it can be seen that after comparing the physical properties of the yellowing-resistant polyvinyl butyral prepared by the present invention with the standard polyvinyl butyral film, it can be seen that the tensile strength and elongation at break of the yellowing-resistant polyvinyl butyral prepared by the present invention have reached the requirements of the physical and mechanical performance indicators of the polyvinyl butyral film in GB / T 32020-2015, and the initial decomposition temperature has been improved. Moreover, the comprehensive performance of Example 1 is the best, which may be because the present invention adds polyvinyl butyral resin to N, N-dimethylformamide to form a resin solution, then adds a modifier and hydroxypropyl methylcellulose to the resin solution, stirs at room temperature, and stirs at elevated temperature to obtain yellowing-resistant polyvinyl butyral. The polyvinyl butyral resin is prepared by using polyvinyl alcohol and n-butyraldehyde under acidic conditions, and then filtered and centrifuged under alkaline conditions to obtain. The modifier is prepared by ultrasonically dispersing aluminum hydroxide in anhydrous ethanol, adding a silane coupling agent, stirring and refluxing, centrifuging, washing and drying to obtain a composite material; adding cinnamic acid to thionyl chloride, refluxing, and then evaporating under reduced pressure to obtain a grafting agent; adding the grafting agent and triethylamine to the composite material dispersion, reacting at room temperature, centrifuging, washing and drying to obtain the modifier.
[0090] The presence of cinnamic acid effectively inhibits the agglomeration of aluminum hydroxide nanoparticles and promotes the uniform distribution of aluminum hydroxide nanoparticles in the polyvinyl butyral matrix. At the same time, the synergistic light absorption of photoelectrons from aluminum hydroxide to cinnamic acid is achieved, which makes the yellowing-resistant polyvinyl butyral have good light shielding properties. At the same time, under light irradiation, the reversible photoisomerization of cinnamic acid can dissipate light into heat, which also enhances the material's UV shielding ability.
[0091] The strengthening effect is mainly due to the transfer of load from the polyvinyl butyral matrix to the rigid aluminum hydroxide. The rigid group benzene ring on the aluminum hydroxide surface further promotes the reinforcing effect of the modifier on the polyvinyl butyral matrix, thereby improving the tensile strength. However, the addition of rigid aluminum hydroxide will inevitably lead to a reduction in elongation at break, because the rigid structure will limit the movement of the polyvinyl butyral molecular chain. The yellowing-resistant polyvinyl butyral film prepared by the present invention still maintains a higher elongation at break under the same load, mainly because the addition of the modifier and the hydroxypropyl methylcellulose aqueous solution is increased, and these additives can improve the dispersibility and interfacial compatibility of the polyvinyl butyral resin, thereby improving the elongation at break of the material.
[0092] Hydroxypropyl methylcellulose is a water-soluble polymer compound. In the preparation process of yellowing-resistant polyvinyl butyral resin, adding hydroxypropyl methylcellulose aqueous solution can reduce yellowing due to light exposure. This is mainly because the hydroxypropyl methylcellulose molecule contains functional groups such as hydroxyl and methyl, which can form hydrogen bonds with polyvinyl butyral resin and form a protective layer on the resin surface, thereby improving the light stability of the resin and slowing down the yellowing rate due to light exposure. In addition, the hydroxypropyl methylcellulose molecule contains a certain amount of free radical scavengers, which can effectively remove free radicals generated in the resin, reduce the oxidation reaction caused by free radicals, and delay the molecular chain breakage and oxidative degradation of polyvinyl butyral to a certain extent, thereby delaying the aging and yellowing of the resin.
[0093] The addition of modifiers can increase the initial decomposition temperature of polyvinyl butyral. The main reason is that aluminum hydroxide is a high-temperature stable inorganic compound that can stabilize the molecular structure of polyvinyl butyral at high temperatures, thereby improving its heat resistance. Silane coupling agents can form a thin film on the surface of aluminum hydroxide, react with the hydroxyl groups in the polyvinyl butyral resin to form chemical bonds, thereby strengthening the interaction between polymer molecules and improving the thermal stability of the polymer. Hydroxypropyl methylcellulose is an organic polymer compound that can form a cross-linked structure in the polyvinyl butyral resin, increase the molecular weight of the polymer, and thus improve the thermal stability of the polymer. Grafting agents can react with the hydroxyl groups in the polyvinyl butyral resin to form chemical bonds, connecting the grafting agent molecules with the polymer molecules, thereby increasing the molecular weight of the polymer and the complexity of the molecular structure, and improving the thermal stability of the polymer. In general, the addition of modifiers can increase the initial decomposition temperature of polyvinyl butyral through a variety of mechanisms, thereby giving it better high temperature resistance.
Claims
1. A method for preparing yellowing-resistant polyvinyl butyral, characterized in that: The steps are as follows: adding polyvinyl butyral resin to a solvent to form a resin solution, then adding a modifier and hydroxypropyl methylcellulose, stirring, heating and stirring to remove the solvent, and obtaining yellowing-resistant polyvinyl butyral; The preparation method of the modifier is as follows: S1. Ultrasonic dispersion of the powder in anhydrous ethanol, then adding silane coupling agent KH-550, stirring and refluxing, centrifuging, collecting the solid, washing, and drying to obtain a composite material; S2, adding cinnamic acid to thionyl chloride, refluxing under nitrogen, and then evaporating under reduced pressure to obtain a grafting agent; S3, adding the grafting agent and triethylamine prepared in step S2 to the composite material dispersion, reacting at room temperature, centrifuging, washing, and drying to obtain a modifier; The powder is at least one of silicon dioxide and aluminum hydroxide; The concentration of the composite material dispersion is 8-12 mg / mL, and the composite material dispersion is prepared by adding the composite material prepared in step S1 into tetrahydrofuran.
2. The method for preparing yellowing-resistant polyvinyl butyral according to claim 1, characterized in that: The solvent is at least one of methanol, ethanol, isopropanol, N,N-dimethylformamide and N-methyl-2-pyrrolidone.
3. The method for preparing yellowing-resistant polyvinyl butyral according to claim 1, characterized in that: The mass of the modifier is 1-3% of the mass of the resin solution; the mass of the hydroxypropyl methylcellulose is 0.5-2% of the mass of the resin solution.
4. The method for preparing yellowing-resistant polyvinyl butyral according to claim 1, characterized in that: In the step S2, the reduced pressure evaporation is performed for 1 to 3 hours, the vacuum degree of the reduced pressure evaporation is 0.03 to 0.05 MPa, and the reduced pressure evaporation temperature is 80 to 90° C.
5. A yellowing-resistant polyvinyl butyral, characterized in that: The method is prepared by the preparation method according to any one of claims 1 to 4.