A kind of emulsion for water-based asphalt-based waterproof coating and its preparation method and application

By using amphoteric surfactant and nonionic surfactant in emulsified asphalt waterproof coatings, combined with internal and external crosslinking agents, the stability problems of emulsified asphalt and cationic emulsified asphalt are solved, and the tensile performance of the coating film is improved and compatibility, realize the effective application of water-based asphalt-based waterproof coatings.

CN116574424BActive Publication Date: 2024-11-22GUANGDONG HENGGUANG CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310519654.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-22
Estimated Expiration
2043-05-10

AI Technical Summary

Technical Problem

The existing emulsified asphalt waterproof coatings cannot be stablely fused with cationic emulsified asphalt, and the tensile performance of the coating film is poor and cannot be used as a waterproof material alone.

Method used

Using hydrophilic and oleophilic design, the polymerization particle size and molecular weight are controlled by combining amphoteric surfactants and nonionic surfactants, combining internal crosslinking monomers and diplomatic surfactants to ensure the stability and coating of emulsified particles. Tensile properties of the membrane.

Benefits of technology

The stable mixing of water-based asphalt-based waterproof coating and cationic emulsified asphalt is achieved, the tensile strength and tensile rate of the coating film are improved, and the compatibility and stability of the coating film are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

A water-based asphalt-based waterproof coating emulsion belongs to the field of asphalt-based waterproof coatings, and is composed of 120-160 parts of styrene, 350-380 parts of n-butyl acrylate, 5-15 parts of 2-ethylhexyl acrylate, 3-8 parts of acrylamide, 10-12 parts of hydroxypropyl acrylate, 0.5-1.5 parts of silane coupling agent, 5-8 parts of butoxydiglycol methacrylate, 1.5-2 parts of initiator, 5-7 parts of zwitterionic surfactant, 3.7-5 parts of nonionic surfactant, 0.5-1 parts of defoamer, and 1-1.5 parts of bactericide. The water-based asphalt-based waterproof coating emulsion prepared in the present invention can be stably mixed with cationic emulsified asphalt, is not easy to demulsify, and has excellent tensile properties and high elongation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of asphalt-based waterproof coatings, and in particular relates to an emulsion for water-based asphalt-based waterproof coatings, and a preparation method and application thereof. Background Art

[0002] Emulsified asphalt waterproof coating is mainly used for roof waterproofing, old house repair and leak repair, underground project moisture-proofing, etc. It has the advantages of easy operation and safe use, and reduces the cost by about 20% compared with the traditional "two felts and three oils". However, since emulsified asphalt does not add any modified materials, after the water evaporates, the film-forming substance still maintains the characteristics of flowing at high temperatures and being brittle at low temperatures, so it cannot be used as a waterproof material alone.

[0003] Acrylic emulsions have excellent adhesion, weather resistance and mechanical properties, and are therefore used to modify emulsified asphalt. There are many types of emulsified asphalt on the market, but most of the emulsions on the market can only be stably integrated with anionic and non-ionic asphalts, and are easily demulsified when mixed with cationic emulsified asphalt. In addition, in order to ensure the strength of the coating, more cross-linking agents are added to the commercially available emulsions, resulting in poor tensile properties of the coating. Summary of the invention

[0004] In order to solve the problems existing in the above-mentioned prior art, the present invention provides a method for preparing an emulsion for a water-based asphalt-based waterproof coating and an application thereof. The emulsion for a water-based asphalt-based waterproof coating of the present invention can be stably mixed with cationic emulsified asphalt, is not prone to demulsification, and has excellent tensile properties and a high elongation rate.

[0005] The specific technical solution adopted by the present invention is:

[0006] The invention discloses an emulsion for water-based asphalt-based waterproof coating, which comprises, by weight, 120-160 parts of styrene, 350-380 parts of n-butyl acrylate, 5-15 parts of 2-ethylhexyl acrylate, 3-8 parts of acrylamide, 10-12 parts of hydroxypropyl acrylate, 0.5-1.5 parts of silane coupling agent, 5-8 parts of butoxydiglycol methacrylate, 1.5-2 parts of initiator, 5-7 parts of zwitterionic surfactant, 3.7-5 parts of nonionic surfactant, 0.5-1 parts of defoamer and 1-1.5 parts of bactericide.

[0007] Furthermore, the water-based asphalt-based waterproof coating emulsion comprises, by weight, 150 parts of styrene, 370 parts of butyl acrylate, 10 parts of 2-ethylhexyl acrylate, 5 parts of acrylamide, 11 parts of hydroxypropyl acrylate, 1 part of silane coupling agent, 6 parts of butoxydiglycol methacrylate, 1.7 parts of initiator, 5.6 parts of amphoteric surfactant, 4.6 parts of nonionic surfactant, 0.5 parts of defoamer, and 1.2 parts of bactericide.

[0008] Furthermore, the zwitterionic surfactant includes 2-sulfonylpropyl methacrylate trimethylammonium chloride.

[0009] Furthermore, the nonionic surfactant comprises 3.5-4.5 parts of surfactant A and 0.2-0.5 parts of surfactant B, wherein the viscosity of the surfactant A is 110-130 mPas, 25°C, and the number of EO addition moles is 8-12; the viscosity of the surfactant B is 400-420 mPas, 25°C, and the number of EO addition moles is 18-22.

[0010] Furthermore, the initiator includes one or more of ammonium persulfate or sodium persulfate.

[0011] The method for preparing an emulsion for a water-based asphalt-based waterproof coating comprises the following steps:

[0012] A: According to the proportion of water-based asphalt waterproof coating emulsion, weigh each component and set aside;

[0013] B. Add 100-120 parts of water to the container, start stirring, add all the zwitterionic surfactants and 3.3-4.6 parts of nonionic surfactants, stir evenly, add all the styrene, n-butyl acrylate, 2-ethylhexyl acrylate, acrylamide, hydroxypropyl acrylate, butoxydiglycol methacrylate, continue stirring for 15-30 minutes, and prepare a pre-emulsion;

[0014] C. Add 230-250 parts of water to the container, start stirring, add the remaining non-ionic surfactant, and when the temperature rises to 80-85°C, add 3-5% of the pre-emulsion and 0.6-1 parts of the initiator. After the temperature stops rising, add the remaining pre-emulsion and the remaining initiator dropwise, and the dropping time is controlled at 180-240min. When the dropping time is 75-85%, add the silane coupling agent and stir evenly. After the remaining pre-emulsion and initiator are added, keep warm for 20-40min. After cooling to 65-68°C, add 0.4-0.8 parts of tert-butyl hydroperoxide and 0.4-0.6 parts of sodium bisulfite dropwise, and the dropping time is controlled at 20-40min. After the addition is completed, keep warm for 20-40min, then adjust the pH to 7.5-8, add a defoamer and a bactericide, and filter to obtain an emulsion for water-based asphalt-based waterproof coating.

[0015] Furthermore, the filtration in step C uses a filter screen with a mesh size of 200-400.

[0016] For example, the use of the above-mentioned emulsion for water-based asphalt-based waterproof coating as a modifier for water-based asphalt-based waterproof coating, the water-based asphalt-based waterproof coating includes, by weight, 150-180 parts of water, 2-4 parts of dispersant, 0.5-2 parts of preservative, 1.5-3 parts of defoaming agent, 340-360 parts of filler, 140-160 parts of emulsified asphalt, and 280-320 parts of emulsion for water-based asphalt-based waterproof coating.

[0017] Furthermore, the filler includes heavy calcium with a mesh size of 375-425 meshes.

[0018] The beneficial effects of the present invention are:

[0019] 1. In the present invention, in order to solve the problem that the current emulsion cannot be stably integrated with the cationic emulsified asphalt, a hydrophilic-lipophilic balance design is adopted. Through the reasonable ratio of the emulsifier, the selected amphoteric surfactant methacrylate-2-sulfonate propyl trimethylammonium chloride is compounded with a non-ionic surfactant. The amphoteric surfactant can both donate and accept protons, and has good dispersibility and emulsification. It can ensure the stability of the emulsified particles under any ionic conditions. The non-ionic surfactant increases the thickness of the hydration layer. The two work together to ensure the stability of the system and good compatibility with various types of emulsified asphalts, thereby improving the tensile properties of the coating.

[0020] 2. In the present invention, special internal cross-linking monomers and external cross-linking agents are selected. Although the use of external cross-linking agents alone will increase the cross-linking density on the film-forming surface, too high a surface cross-linking density will lead to a decrease in tensile strength. Therefore, internal cross-linking monomers are introduced at the same time as the external cross-linking agent, thereby increasing the internal cross-linking degree of the latex particles and the cross-linking degree between the particles during film formation, thereby increasing the tensile strength of the coating from the inside.

[0021] 3. In the preparation process of the emulsion for water-based asphalt-based waterproof coating of the present invention, the non-ionic surfactant is added in batches in step B and step C, which can make the pre-emulsion and other components better blended, and the heating temperature in step C is strictly controlled to avoid the temperature exceeding the cloud point of the non-ionic surfactant, causing the non-ionic surfactant to lose its effect.

[0022] 4. The present invention uses surfactants with different EO added molar numbers for compounding. Due to the different EO numbers, the effects on the polymerization particle size and molecular weight during the polymerization process are different. The compounding can not only well control the particle size and molecular weight, but also ensure the thickness of the hydration layer and the stability of the particles.

[0023] 5. The present invention adopts accurate monomer ratio to control the surface activity of water-phase polymer free radicals, cooperates with non-ionic surfactants, and adjusts the appropriate termination of water-phase polymer free radicals in the water phase, thereby controlling the formation of water-soluble polymers. DETAILED DESCRIPTION

[0024] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.

[0025] The defoamer in the present invention is NXZ defoamer produced by BASF of Germany, the bactericide is BIT20 bactericide produced by Shandong Xinwei Chemical Technology Co., Ltd., and the water is deionized water; other raw materials used can be purchased from the market unless otherwise specified. 1. Specific embodiments Specific embodiment 1

[0028] A: According to the ratio of emulsion for water-based asphalt waterproof coating, weigh 150 parts of styrene, 370 parts of butyl acrylate, 10 parts of 2-ethylhexyl acrylate, 5 parts of acrylamide, 11 parts of hydroxypropyl acrylate, 1 part of silane coupling agent, 6 parts of butoxydiglycol methacrylate, 1.7 parts of initiator, 5.6 parts of amphoteric surfactant, 4.6 parts of nonionic surfactant, 0.6 parts of defoamer, and 1.2 parts of bactericide;

[0029] B: Add 116 parts of deionized water to the pre-emulsification kettle, start stirring, add all the amphoteric surfactant methacrylate-2-sulfonate propyl trimethylammonium chloride, non-ionic surfactant ER10 3.8 parts, non-ionic surfactant ER30 0.5 parts, add measured monomers styrene, n-butyl acrylate, 2-ethylhexyl acrylate, acrylamide, hydroxypropyl acrylate, butoxydiglycol methacrylate after 15 minutes, continue high-speed stirring and emulsification for about 20 minutes to obtain a pre-emulsion;

[0030] C. Add 240 parts of deionized water to the reactor, start stirring, add 0.3 parts of non-ionic surfactant ER10, and when the temperature rises to 85°C, add 4.5% pre-emulsion and 0.7 parts of initiator. After the temperature rises to the highest and stabilizes for 2 minutes, start dripping the remaining pre-emulsion and the remaining initiator. The dripping temperature is controlled at 83-85°C, and the dripping time is 210 minutes. When the dripping reaches 170 minutes, add the silane coupling agent and stir evenly. After the pre-emulsion and initiator are dripped, keep the temperature for 30 minutes, cool to 66°C for post-treatment, cool to below 40°C, adjust the pH to 7.8 with 20% sodium hydroxide solution, add defoamer and bactericide, and filter to a fineness of ≤25μm to obtain an emulsion for water-based asphalt-based waterproof coating;

[0031] D. Add 160 parts of water, 3 parts of dispersant, 1 part of preservative, 2.4 parts of defoamer, 350 parts of 400-mesh heavy calcium, 150 parts of emulsified asphalt, and 300 parts of emulsion for water-based asphalt-based waterproof coating into a stirring tank, and stir for 30 minutes to obtain a water-based asphalt-based waterproof coating. Specific embodiment 2

[0033] A: According to the ratio of emulsion for water-based asphalt waterproof coating, weigh 120 parts of styrene, 350 parts of butyl acrylate, 5 parts of 2-ethylhexyl acrylate, 3 parts of acrylamide, 10 parts of hydroxypropyl acrylate, 0.5 parts of silane coupling agent, 5 parts of butoxydiglycol methacrylate, 1.5 parts of initiator, 5 parts of amphoteric surfactant, 3.7 parts of nonionic surfactant, 0.5 parts of defoamer, and 1 part of bactericide;

[0034] B: Add 100 parts of deionized water to the pre-emulsification kettle, start stirring, add all the amphoteric surfactant methacrylate-2-sulfonate propyl trimethylammonium chloride, non-ionic surfactant ER10 3.1 parts, non-ionic surfactant ER30 0.2 parts, add measured monomers styrene, n-butyl acrylate, 2-ethylhexyl acrylate, acrylamide, hydroxypropyl acrylate, butoxydiglycol methacrylate after 15 minutes, continue to stir and emulsify at high speed for about 15 minutes to obtain the pre-emulsion;

[0035] C. Add 230 parts of deionized water to the reactor, start stirring, add 0.4 parts of nonionic surfactant ER10, and when the temperature rises to 80°C, add 3% pre-emulsion and 0.6 parts of initiator. After the temperature rises to the highest and stabilizes for 2 minutes, start dripping the remaining pre-emulsion and the remaining initiator. The dripping temperature is controlled at 83-85°C, and the dripping time is 180 minutes. When the dripping reaches 135 minutes, add the silane coupling agent and stir evenly. After the pre-emulsion and initiator are added, keep the temperature for 20 minutes, cool to 65°C for post-treatment, cool to below 40°C, adjust the pH to 7.5 with 20% sodium hydroxide solution, add defoamer and bactericide, and filter to a fineness of ≤25μm to obtain an emulsion for water-based asphalt-based waterproof coating;

[0036] D. Add 150 parts of water, 2 parts of dispersant, 0.5 parts of preservative, 1.5 parts of defoamer, 340 parts of 375-mesh heavy calcium, 140 parts of emulsified asphalt, and 280 parts of emulsion for water-based asphalt-based waterproof coating into a stirred tank, and stir for 40 minutes to obtain a water-based asphalt-based waterproof coating. Specific embodiment 3

[0038] A: According to the ratio of emulsion for water-based asphalt waterproof coating, weigh 160 parts of styrene, 380 parts of butyl acrylate, 15 parts of 2-ethylhexyl acrylate, 8 parts of acrylamide, 12 parts of hydroxypropyl acrylate, 1.5 parts of silane coupling agent, 8 parts of butoxydiglycol methacrylate, 2 parts of initiator, 7 parts of amphoteric surfactant, 5 parts of nonionic surfactant, 1 part of defoamer, and 1.5 parts of bactericide;

[0039] B: Add 120 parts of deionized water to the pre-emulsification kettle, start stirring, add all the amphoteric surfactant methacrylate-2-sulfonate propyl trimethylammonium chloride, 4 parts of non-ionic surfactant ER10, and 0.5 parts of non-ionic surfactant ER30, and after 15 minutes, add the measured monomers styrene, n-butyl acrylate, 2-ethylhexyl acrylate, acrylamide, hydroxypropyl acrylate, and butoxydiglycol methacrylate, and continue to stir and emulsify at high speed for about 15 minutes to obtain a pre-emulsion;

[0040] C. Add 230 parts of deionized water to the reactor, start stirring, add 0.5 parts of non-ionic surfactant ER10, and when the temperature rises to 85°C, add 5% pre-emulsion and 1 part of initiator. After the temperature rises to the highest and stabilizes for 2 minutes, start dripping the remaining pre-emulsion and the remaining initiator. The dripping temperature is controlled at 83-85°C, and the dripping time is 240 minutes. When the dripping reaches 204 minutes, the silane coupling agent is added and stirred evenly. After the pre-emulsion and initiator are dripped, keep the temperature for 40 minutes, cool to 68°C for post-treatment, cool to below 40°C, adjust the pH to 8 with 20% sodium hydroxide solution, add defoamer and bactericide, and filter to a fineness of ≤25μm to obtain an emulsion for water-based asphalt-based waterproof coating;

[0041] D. Add 180 parts of water, 4 parts of dispersant, 2 parts of preservative, 3 parts of defoamer, 360 parts of 425-mesh heavy calcium, 160 parts of emulsified asphalt, and 320 parts of emulsion for water-based asphalt-based waterproof coating into the stirring tank, and stir for 30 minutes to obtain the water-based asphalt-based waterproof coating.

[0042] Comparative Example 1

[0043] The difference between Comparative Example 1 and Example 1 is that no nonionic surfactant is added in Comparative Example 1.

[0044] Comparative Example 2

[0045] The difference between Comparative Example 2 and Example 1 is that no zwitterionic surfactant is added in Comparative Example 2.

[0046] 2. Performance Test

[0047] The water-based asphalt-based waterproof coating emulsions prepared in the above embodiments and comparative examples were tested according to standard GB / T 16777-2008. The test results are shown in Table 1.

[0048]

[0049] Table 1 shows the results of performance testing of the water-based asphalt-based waterproof coating emulsions in Examples 1-3 and Comparative Examples 1-2, wherein the water-based asphalt-based waterproof coating emulsions in Examples 1-3 are stably mixed with cationic emulsified asphalt, with a tensile strength of ≥1.27MPa and an elongation of ≥625%.

[0050] From the comparison between Example 1 and Comparative Examples 1-2, it can be seen that no nonionic surfactant was added in Comparative Example 1. Although the prepared emulsion was stably mixed with cationic emulsified asphalt, its tensile strength and elongation were poor. No zwitterionic surfactant was added in Comparative Example 2, resulting in its inability to be stably mixed with cationic emulsified asphalt. In Example 1, both amphoteric surfactants and nonionic surfactants were added at the same time, and the two synergistically ensured the stability of the system and good compatibility with various types of emulsified asphalts, while the emulsion was able to ensure the stability of the emulsified particles under any ionic conditions and improve the tensile properties of the coating.

Claims

1. An emulsion for water-based asphalt-based waterproof coating, characterized in that: The waterproof coating emulsion is composed of 120-160 parts of styrene, 350-380 parts of n-butyl acrylate, 5-15 parts of 2-ethylhexyl acrylate, 3-8 parts of acrylamide, 10-12 parts of hydroxypropyl acrylate, 0.5-1.5 parts of silane coupling agent, 5-8 parts of butoxydiglycol methacrylate, 1.5-2 parts of initiator, 5-7 parts of zwitterionic surfactant, 3.7-5 parts of nonionic surfactant, 0.5-1 parts of defoamer, and 1-1.5 parts of bactericide in parts by weight; The nonionic surfactant is composed of 3.5-4.5 parts of surfactant A and 0.2-0.5 parts of surfactant B, wherein the viscosity of the surfactant A is 110-130 mPas, 25°C, and the number of EO addition moles is 8-12; the viscosity of the surfactant B is 400-420 mPas, 25°C, and the number of EO addition moles is 18-22; The zwitterionic surfactant is methacrylate-2-sulfonylpropyltrimethylammonium chloride.

2. The aqueous asphalt-based waterproof coating emulsion according to claim 1, characterized in that: The water-based asphalt-based waterproof coating emulsion is composed, by weight, of 150 parts of styrene, 370 parts of butyl acrylate, 10 parts of 2-ethylhexyl acrylate, 5 parts of acrylamide, 11 parts of hydroxypropyl acrylate, 1 part of silane coupling agent, 6 parts of butoxydiglycol methacrylate, 1.7 parts of initiator, 5.6 parts of amphoteric surfactant, 4.6 parts of nonionic surfactant, 0.5 parts of defoamer and 1.2 parts of bactericide.

3. The aqueous asphalt-based waterproof coating emulsion according to any one of claims 1 to 2, characterized in that: The initiator includes one or more of ammonium persulfate or sodium persulfate.

4. A method for preparing the aqueous asphalt-based waterproof coating emulsion according to any one of claims 1 to 2, comprising the following steps: A: According to the proportion of water-based asphalt waterproof coating emulsion, weigh each component and set aside; B. Add 100-120 parts of water to the container, start stirring, add all the zwitterionic surfactants and 3.3-4.6 parts of nonionic surfactants, stir evenly, add all the styrene, n-butyl acrylate, 2-ethylhexyl acrylate, acrylamide, hydroxypropyl acrylate, butoxydiglycol methacrylate, continue stirring for 15-30 minutes, and prepare a pre-emulsion; C. Add 230-250 parts of water to the container, start stirring, add the remaining non-ionic surfactant, and when the temperature rises to 80-85°C, add 3-5% of the pre-emulsion and 0.6-1 parts of the initiator. After the temperature stops rising, add the remaining pre-emulsion and the remaining initiator dropwise, and the dropping time is controlled at 180-240min. When the dropping time is 75-85%, add the silane coupling agent and stir evenly. After the remaining pre-emulsion and initiator are added, keep warm for 20-40min. After cooling to 65-68°C, add 0.4-0.8 parts of tert-butyl hydroperoxide and 0.4-0.6 parts of sodium bisulfite dropwise, and the dropping time is controlled at 20-40min. After the addition is completed, keep warm for 20-40min, then adjust the pH to 7.5-8, add a defoamer and a bactericide, and filter to obtain an emulsion for water-based asphalt-based waterproof coating.

5. The method for preparing an emulsion for a water-based asphalt-based waterproof coating according to claim 4, characterized in that: The filtration in step C uses a filter screen with a mesh size of 200-400.

6. The use of the water-based asphalt-based waterproof coating emulsion as claimed in any one of claims 1 to 2 as a modifier for water-based asphalt-based waterproof coatings, characterized in that: The water-based asphalt-based waterproof coating comprises, by weight, 150-180 parts of water, 2-4 parts of dispersant, 0.5-2 parts of preservative, 1.5-3 parts of defoamer, 340-360 parts of filler, 140-160 parts of emulsified asphalt, and 280-320 parts of emulsion for water-based asphalt-based waterproof coating.

7. The use according to claim 6, characterized in that: The filler includes heavy calcium with a mesh number of 375-425 meshes.