A Co-based magnetic sensitive fiber material and its application

Through thermal drawing and composite heat treatment methods, the problem of deterioration of shape pole roll and magnetic properties of Co-based magnetic sensitive fiber materials in the drawing process is solved, and Co-based magnetic sensitive fiber materials with high consistency and high sensitivity are prepared to meet the modern Magnetic performance requirements of magnetic sensors.

CN116574940BActive Publication Date: 2024-12-06NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202310413481.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-11
Publication Date
2024-12-06
Estimated Expiration
2043-04-11

AI Technical Summary

Technical Problem

It is difficult to prepare Co-based magnetically sensitive fiber materials with good consistency, high straightness and excellent magnetic properties, especially in the drawing process of low plastic fiber materials, shape pole rolls and magnetic properties deteriorate.

Method used

Using a composite heat treatment method based on thermal drawing combined with stress annealing and axial magnetic field annealing, the Co-based magnetic sensitive fiber material is straightened and magnetic domain structure adjusted, which improves its axial magnetic permeability and overcomes the deterioration of magnetic properties caused by stress annealing. .

Benefits of technology

Co-based magnetic sensitive fiber materials with high consistency, high sensitivity and high permeability change rate were prepared to meet the demands of modern magnetic sensors for excellent magnetic performance, and overcome the lack of collimation and magnetic properties in batch production. The problem of decline.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116574940B_ABST
    Figure CN116574940B_ABST
Patent Text Reader

Abstract

The invention discloses a Co-based magnetic sensitive fiber material, which is prepared by subjecting a Co-based magnetic sensitive mother fiber material to thermal drawing, stress annealing and axial magnetic field annealing. The composition of the Co-based magnetic sensitive mother fiber material is Co a Fe b Si c B d M e , wherein a+b+c+d+e=100, M is one or two of Cr or Mo elements, and the atomic percentage of each element is 65≤a≤70, 4≤b≤6, 10≤c≤14, 6≤d≤12, 2≤e≤6. Stress annealing is annealing for 20‑40 min under the conditions of stress of 1400‑1680 MPa and temperature of 350‑450°C under nitrogen protection, and water quenching is performed immediately after the annealing. Magnetic field annealing is annealing under nitrogen protection with an axial magnetic field intensity of 0.5‑1T, heating the magnetic field furnace to above 260°C, but not exceeding the Curie temperature of the material, and annealing for 20‑40 min. The present invention also discloses the application of the Co-based magnetic sensitive fiber material in a magnetic sensor. The preparation method of the present invention is simple, and the obtained fiber material has the advantages of high consistency, good straightness, high sensitivity and large magnetic permeability change rate, which can meet the current demand of magnetic sensors for excellent magnetic performance materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of processing and manufacturing of magnetically sensitive fiber materials, and in particular relates to a Co-based magnetically sensitive fiber material and an application thereof. Background Art

[0002] Magnetic sensors play a vital role in modern technology. They are widely used in various engineering and industrial sectors, such as high-density magnetic recording, navigation, military and security, target detection and tracking, anti-theft systems, non-destructive testing, magnetic marking and labeling, geomagnetic measurement, space research, magnetic field measurement on spacecraft and human biomagnetic measurement. Compared with other types of magnetic sensors, GMI magnetic sensors are widely used in the field of weak magnetic field detection due to their advantages such as miniaturization and high sensitivity. High magnetic permeability Co-based magnetic sensitive fiber materials are irreplaceable key sensing elements in such magnetic sensors.

[0003] Alloy wire is the most sophisticated sensing module in weak magnetic detection sensors. The consistency of alloy wire is one of the most important indicators affecting the performance of sensor elements. At present, the main methods for preparing alloy wire in China are melt drawing method, glass coating method and inner circle water spinning method. However, no matter which preparation method is used, the consistency of the material (diameter change rate at different positions) will be limited by the stability of equipment and process.

[0004] At present, the surface of the fiber material is mainly reprocessed through the drawing process, and the consistency of the fiber material is improved by extrusion and stretching. The invention patent with the authorization announcement number CN 111633044 B discloses a surface processing process for nickel-titanium shape memory alloy microwires. The nickel-titanium shape memory alloy microwires with high fatigue life are obtained by subjecting the pretreated nickel-titanium shape memory alloy microwires to multiple cold drawing processes and then nitriding treatment. This method is mainly suitable for shape memory alloy microwires, and the shape of the alloy wire will not be affected by the drawing process due to its high plasticity. However, for low-plasticity fiber materials, due to the uneven distribution of stress after drawing, the shape of the low-plasticity wire will become extremely curled, which affects the mass production of magnetically sensitive fiber materials in the sensor field.

[0005] The invention patent with the authorization announcement number CN 105679486 B discloses a new method for preparing a magnetic sensitive material with high sensitivity and wide linear range. The method heat treats the amorphous material under stress and below the crystallization temperature, and applies a longitudinal stress less than the fracture strength to the treated material during the heat treatment of the amorphous material, thereby preparing a magnetic sensitive material with the advantages of wide linear range and high sensitivity. However, the use of stress annealing will deteriorate the magnetic properties of the wire, resulting in it being unable to meet the current demand for excellent magnetic performance materials for magnetic sensors.

[0006] With the widespread application of magnetic sensors, the performance requirements for alloy wires will become higher and higher. How to overcome the shortcomings of existing technologies and prepare circular cross-section magnetically sensitive fiber materials with good consistency, high straightness and excellent performance is an important research topic in related fields. Summary of the invention

[0007] In order to solve the problems existing in the prior art, the present invention provides a Co-based magnetically sensitive fiber material, which is prepared by hot drawing and composite heat treatment of a Co-based magnetically sensitive mother fiber material. The material has the advantages of high consistency, good straightness, high sensitivity and high magnetic permeability change rate, and can meet the current demand for magnetic sensors for excellent magnetic performance materials.

[0008] A Co-based magnetically sensitive fiber material is prepared by subjecting a Co-based magnetically sensitive mother fiber material to thermal drawing, stress annealing, and axial magnetic field annealing. The composition of the Co-based magnetically sensitive mother fiber material is Co a Fe b Si c B d M e , where a+b+c+d+e=100, M is one or both of Cr and Mo elements, and the atomic percentage of each element is 65≤a≤70, 4≤b≤6, 10≤c≤14, 6≤d≤12, and 2≤e≤6.

[0009] The present invention adopts a method of stress annealing combined with magnetic field annealing to perform composite heat treatment on the alloy wire after hot drawing. The alloy wire after hot drawing is extremely rolled, and stress annealing is used to straighten the alloy wire after hot drawing, and nitrogen protection is applied during annealing to prevent oxidation of the wire. The alloy wire after stress annealing and straightening is then subjected to magnetic field annealing in an axial magnetic field to adjust the magnetic domain structure of the wire, improve its axial magnetic permeability, and make up for the disadvantage of deterioration of the magnetic properties of the wire caused by stress annealing, thereby improving the magnetic properties of the wire.

[0010] The Co-based magnetically sensitive mother fiber material of the present invention can be prepared by the method disclosed in application number 202310095751.5, or can be obtained commercially on the market.

[0011] The pre-treatment temperature of the hot drawing can be customized according to the material composition, and the pre-treatment temperature of the hot drawing should not cause oxidation of the Co-based magnetic sensitive mother fiber material.

[0012] Preferably, the pre-treatment temperature of the hot drawing is 150-250°C.

[0013] Preferably, the hot drawing is performed at a temperature lower than the oxidation temperature of the Co-based magnetically sensitive mother fiber material.

[0014] Preferably, the diameter of the Co-based magnetically sensitive mother fiber material is 100-140 μm, and the total compression ratio of the Co-based magnetically sensitive mother fiber material is not less than 30%, but the total compression ratio cannot cause the Co-based magnetically sensitive mother fiber material to break.

[0015] Under nitrogen protection, stress is applied to the alloy wire after hot drawing. The magnitude of the applied stress value is proportional to the straightness of the alloy wire. The applied stress value should be less than the breaking strength of the alloy wire after hot drawing. The stress annealing temperature and time should not cause crystallization and oxidation of the fiber material. Straight alloy fiber material is obtained after stress annealing.

[0016] Preferably, the stress annealing conditions are: annealing for 20-40 min under nitrogen protection at a stress value of 1400-1680 MPa and an annealing temperature of 350-450° C., and water quenching immediately after annealing.

[0017] Preferably, the axial magnetic field annealing conditions are: under nitrogen protection, when the axial magnetic field strength is 0.5-1T, the magnetic field furnace is heated to above 260°C but not exceeding the Curie temperature of the Co-based magnetic sensitive mother fiber material, and annealing is performed for 20-40 minutes.

[0018] The intensity of the axial magnetic field should not be too low. In order to meet the needs of industrial continuous production, the magnetic field intensity is controlled not to exceed 1T in the present invention.

[0019] Preferably, the Co-based magnetically sensitive fiber material has a GMI of ≥1010%, a sensitivity of ≥101% / Oe, and an anisotropy field of ≤0.52Oe.

[0020] The present invention also provides the application of the Co-based magnetic sensitive fiber material in a magnetic sensor. The Co-based magnetic sensitive fiber material of the present invention has excellent magnetic properties and has good application prospects in magnetic sensors.

[0021] Compared with the prior art, the present invention has at least the following beneficial effects:

[0022] (1) The preparation method of the present invention is simple, and the prepared Co-based magnetic sensitive fiber material has high consistency, which solves the problem that the diameter uniformity of the existing magnetic sensitive fiber material is low and thus affects the consistency of the sensor.

[0023] (2) The present invention overcomes the shortcoming that non-aligned magnetically sensitive fiber materials cannot meet the requirements of mass industrial production, and the prepared aligned Co-based magnetically sensitive fiber materials can be mass-produced in the industrial field.

[0024] (3) The present invention combines stress annealing with magnetic field annealing, which overcomes the shortcoming of the prior art that only stress annealing leads to deterioration of the magnetic properties of the wire. The prepared Co-based magnetic sensitive fiber material has the advantages of high sensitivity and high magnetic permeability change rate, which can meet the current demand for magnetic sensors for excellent magnetic performance materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a schematic diagram of the heat treatment process for preparing the Co-based magnetic sensitive fiber material in Example 1;

[0026] Figure 2 This is a physical picture of the Co-based magnetic sensitive fiber material prepared in Example 1 and Comparative Examples 1-4;

[0027] Figure 3 hysteresis loop diagram of the Co-based magnetic sensitive fiber material prepared in Example 1 and Comparative Examples 1-4;

[0028] Figure 4 It is a GMI curve diagram of the Co-based magnetic sensitive fiber material prepared in Example 1 and Comparative Examples 1-4;

[0029] Figure 5 1 is a graph showing the magnetic permeability variation trend of the Co-based magnetic sensitive fiber materials prepared in Example 1 and Comparative Examples 1-4. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiment. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Those skilled in the art can make modifications or equivalent substitutions based on the understanding of the technical scheme of the present invention without departing from the spirit and scope of the technical scheme of the present invention, and all should be included in the protection scope of the present invention.

[0031] Example 1

[0032] This embodiment uses a commercially available Co-based magnetic sensitive mother fiber material (mother fiber, manufacturer: Ningbo Magnetic Material Application Technology Innovation Center Co., Ltd.; product name: cobalt-based magnetic sensitive fiber material; brand: CAS-120-LT), the composition of which is Co 68.1 Fe 4.3 Si 12.5 B 12 Cr3Mo 0.1 , with a diameter of 120μm.

[0033] In this embodiment, the Co-based magnetic sensitive fiber material is prepared by subjecting the Co-based magnetic sensitive mother fiber material to thermal drawing, high stress annealing and high magnetic field annealing. The heat treatment process conditions of high stress annealing and high magnetic field annealing are as follows: Figure 1The specific steps of preparing the Co-based magnetic sensitive mother fiber material in this embodiment are:

[0034] (1) Wind at least 30m long mother wire onto a bobbin for hot drawing. The pre-annealing temperature before drawing is 200℃, the furnace length is 300mm, and the wire feed speed is adjustable but oxidation of the mother wire should be prevented. The drawing passes are 5, each pass is compressed by 4μm, the mother wire is drawn from 120μm to 100μm, and the total compression ratio is 30%;

[0035] (2) Stress annealing was performed on the drawn wire under nitrogen protection. When the annealing furnace temperature was raised to 400°C, annealing was performed for 30 min. The applied stress was 1679 MPa. After annealing, water quenching was performed immediately.

[0036] (3) The alloy wire after stress annealing is subjected to magnetic field annealing under nitrogen protection. The magnetic field strength of the applied axial magnetic field is 1 T. The temperature conditions of the magnetic field annealing are: heating the magnetic field furnace to an annealing temperature of 260°C at a heating rate of 10°C / min, the annealing time is 30 minutes, and cooling to room temperature after annealing.

[0037] The properties of the prepared Co-based magnetic sensitive fiber material were tested. The test results show that straighter wires (such as Figure 2 ), the obtained Co-based magnetic sensitive fiber material has a higher initial magnetic permeability, faster saturation, and a higher rate of change of magnetic permeability (such as Figure 3 and Figure 5 The GMI test of the Co-based magnetic sensitive fiber material shows that the GMI of the magnetic sensitive fiber material prepared in this embodiment is 1010%, the sensitivity is 101% / Oe, and the anisotropy field is 0.52Oe (such as Figure 4 and Table 1), which indicates that the Co-based magnetic sensitive fiber material obtained after high tension annealing and high magnetic field annealing has excellent magnetic properties.

[0038] Comparative Example 1

[0039] The Co-based magnetically sensitive mother fiber material used in this embodiment is the same as that in Embodiment 1.

[0040] In this embodiment, the Co-based magnetically sensitive fiber material is prepared by hot drawing the Co-based magnetically sensitive mother fiber material. The specific steps are as follows:

[0041] The mother wire of at least 30m in length is wound onto a bobbin for hot drawing. The pre-annealing temperature before drawing is 200℃, the furnace length is 300mm, the wire feed speed is adjustable but the mother wire should be prevented from oxidation. The drawing passes are 5, each pass is compressed by 4μm, the mother wire is drawn from 120μm to 100μm, and the total compression ratio is 30%.

[0042] The performance of the Co-based magnetic sensitive fiber material obtained after hot drawing was tested. The test results show that the Co-based magnetic sensitive fiber material obtained only by hot drawing has a bending radius of 1.35 (such as Figure 2 and Table 1), the obtained Co-based magnetic sensitive fiber material has a higher initial magnetic permeability, faster saturation, and a higher rate of change of magnetic permeability (e.g. Figure 3 and Figure 5 ). The GMI test of the obtained Co-based magnetic sensitive fiber material shows that ( Figure 4 and Table 1), the GMI size of the Co-based magnetic sensitive fiber material prepared in this embodiment is 810%, the sensitivity is 81% / Oe, and the anisotropy field is 2Oe. Compared with the performance of the magnetic sensitive fiber material obtained in Example 1, the wire material obtained in this embodiment is more tangled and has poorer magnetic properties.

[0043] Comparative Example 2

[0044] The Co-based magnetically sensitive mother fiber material used in this embodiment is the same as that in Embodiment 1.

[0045] In this embodiment, the Co-based magnetic sensitive fiber material is prepared by performing heat drawing and low stress annealing on the Co-based magnetic sensitive fiber mother material. The specific steps are as follows:

[0046] (1) Wind at least 30m long mother wire onto a bobbin for hot drawing. The pre-annealing temperature before drawing is 200℃, the furnace length is 300mm, and the wire feed speed is adjustable but oxidation of the mother wire should be prevented. The drawing passes are 5, each pass is compressed by 4μm, the mother wire is drawn from 120μm to 100μm, and the total compression ratio is 30%;

[0047] (2) The drawn wire is subjected to stress annealing under nitrogen protection. When the annealing furnace temperature rises to 400°C, annealing is performed for 30 min. The applied stress is 60 MPa. Water quenching is performed immediately after annealing.

[0048] The performance of the Co-based magnetic sensitive fiber material obtained after small stress annealing was tested. The test results show that the bending radius of the Co-based magnetic sensitive fiber material obtained after small stress annealing is 1.85 (as shown in FIG. Figure 2 and Table 1), the bending radius of the magnetic sensitive fiber material obtained in Comparative Example 1 becomes larger, which indicates that annealing under relatively small stress can improve the curling of the wire. The initial magnetic permeability of the Co-based magnetic sensitive fiber material obtained after small stress annealing is similar to that of Comparative Example 1, but the saturation speed is slow and the magnetic permeability change rate is low (such as Figure 3 and Figure 5 The GMI test of the Co-based magnetic sensitive fiber material shows that the GMI of the magnetic sensitive fiber material prepared in this embodiment is 898%, the sensitivity is 44.9% / Oe, and the anisotropy field is 2.5Oe (such as Figure 4and Table 1). Compared with Comparative Example 1, the sensitivity of the magnetic sensitive fiber material prepared in this embodiment is significantly reduced.

[0049] Comparative Example 3

[0050] The Co-based magnetically sensitive mother fiber material used in this embodiment is the same as that in Embodiment 1.

[0051] In this embodiment, the Co-based magnetic sensitive fiber material is prepared by performing hot drawing and high stress annealing on the above-mentioned Co-based magnetic sensitive mother fiber material. The specific steps are as follows:

[0052] (1) Wind at least 30m long mother wire onto a bobbin for hot drawing. The pre-annealing temperature before drawing is 200℃, the furnace length is 300mm, and the wire feed speed is adjustable but oxidation of the mother wire should be prevented. The drawing passes are 5, each pass is compressed by 4μm, the mother wire is drawn from 120μm to 100μm, and the total compression ratio is 30%;

[0053] (2) The drawn wire is subjected to stress annealing under nitrogen protection. When the annealing furnace temperature rises to 400°C, annealing is performed for 30 min. The applied stress is 1679 MPa. Water quenching is performed immediately after annealing.

[0054] The performance of the Co-based magnetic sensitive fiber material obtained after high stress annealing was tested. The test results show that the Co-based magnetic sensitive fiber material obtained after high stress annealing is relatively straight, which shows that high stress annealing can directly solve the problem of wire curling (such as Figure 2 The Co-based magnetic sensitive fiber material obtained by high stress annealing has extremely low initial magnetic permeability, extremely slow saturation speed, and extremely low magnetic permeability change rate (such as Figure 3 and Figure 5 The GMI test of the Co-based magnetic sensitive fiber material shows that the GMI of the magnetic sensitive fiber material prepared in this embodiment is 91%, the sensitivity is 2.28% / Oe, and the anisotropy field is 29Oe (such as Figure 4 and Table 1). Compared with Comparative Examples 1 and 2, the GMI and sensitivity of the magnetic sensitive fiber material prepared in this embodiment are significantly reduced, which indicates that the high stress annealing leads to the deterioration of the magnetic properties of the wire.

[0055] Comparative Example 4

[0056] The Co-based magnetically sensitive mother fiber material used in this embodiment is the same as that in Embodiment 1.

[0057] In this embodiment, the Co-based magnetic sensitive fiber material is prepared by subjecting the above-mentioned Co-based magnetic sensitive mother fiber material to hot drawing, high stress annealing and low magnetic field annealing. The specific steps are as follows:

[0058] (1) Wind at least 30m long mother wire onto a bobbin for hot drawing. The pre-annealing temperature before drawing is 200℃, the furnace length is 300mm, and the wire feed speed is adjustable but oxidation of the mother wire should be prevented. The drawing passes are 5, each pass is compressed by 4μm, the mother wire is drawn from 120μm to 100μm, and the total compression ratio is 30%;

[0059] (2) Stress annealing was performed on the drawn wire under nitrogen protection. When the annealing furnace temperature was raised to 400°C, annealing was performed for 30 min. The applied stress was 1679 MPa. After annealing, water quenching was performed immediately.

[0060] (3) The alloy wire after stress annealing is subjected to magnetic field annealing under nitrogen protection. The magnetic field strength of the applied axial magnetic field is 0.1 T. The temperature conditions of the magnetic field annealing are: heating the magnetic field furnace to an annealing temperature of 260°C at a heating rate of 10°C / min, the annealing time is 30 minutes, and cooling to room temperature after annealing.

[0061] The Co-based magnetic sensitive fiber material obtained after high stress annealing and low magnetic field annealing was tested. The test results show that straighter wires can be obtained after high stress annealing and low magnetic field annealing, which shows that magnetic field annealing will not change the shape of the wire (such as Figure 2 Compared with Comparative Example 3, although the small magnetic field annealing can improve the magnetic properties of the Co-based magnetic sensitive fiber material, the initial magnetic permeability of the obtained Co-based magnetic sensitive fiber material is still low, the saturation speed is very slow, and the magnetic permeability change rate is very low (such as Figure 3 and Figure 5 The GMI test of the obtained Co-based magnetic sensitive fiber material shows that the magnetic properties of the magnetic sensitive fiber material prepared in this embodiment are poor. The GMI of the obtained magnetic sensitive fiber material is 239.6%, the sensitivity is 11.98% / Oe, and the anisotropy field is 8.5e (e.g. Figure 4 and Table 1).

[0062] Comparative Example 5

[0063] The Co-based magnetically sensitive mother fiber material used in this embodiment is the same as that in Embodiment 1.

[0064] In this embodiment, the Co-based magnetic sensitive fiber material is prepared by heat drawing and stress annealing the Co-based magnetic sensitive mother fiber material. In this embodiment, the stress annealing time is extended to 60 minutes. The specific steps are as follows:

[0065] The mother wire of at least 30m in length is wound onto a bobbin for hot drawing. The pre-annealing temperature before drawing is 200℃, the furnace length is 300mm, the wire feed speed is adjustable but the mother wire should be prevented from oxidation. The drawing passes are 5, each pass is compressed by 4μm, the mother wire is drawn from 120μm to 100μm, and the total compression ratio is 30%.

[0066] The drawn wire was subjected to stress annealing. When the annealing furnace temperature was raised to 400°C, the annealing time was 60 min. The surface of the wire turned yellow after annealing, and oxidation was obvious (Table 1).

[0067] Table 1 Performance parameters of Co-based magnetic sensitive fiber materials prepared in Examples and Comparative Examples

[0068]

[0069] Comparative Example 6

[0070] The Co-based magnetically sensitive mother fiber material used in this embodiment is the same as that in Embodiment 1.

[0071] In this embodiment, the Co-based magnetic sensitive fiber material is prepared by heat drawing and stress annealing the Co-based magnetic sensitive mother fiber material. In this embodiment, the stress annealing temperature is increased to 500° C. The specific steps are as follows:

[0072] The mother wire of at least 30m in length is wound onto a bobbin for hot drawing. The pre-annealing temperature before drawing is 200℃, the furnace length is 300mm, the wire feed speed is adjustable but the mother wire should be prevented from oxidation. The drawing passes are 5, each pass is compressed by 4μm, the mother wire is drawn from 120μm to 100μm, and the total compression ratio is 30%.

[0073] The wire after drawing was subjected to stress annealing. When the annealing furnace temperature was raised to 420°C, the annealing time was 30 min. After annealing, the wire became brittle and crystallization occurred (Table 1).

[0074] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A Co-based magnetically sensitive fiber material, characterized in that: The Co-based magnetic sensitive mother fiber material is prepared by heat drawing, stress annealing and axial magnetic field annealing. The composition of the Co-based magnetic sensitive mother fiber material is Co a Fe b Si c B d M e , wherein a+b+c+d+e=100, M is one or both of Cr and Mo elements, and the atomic percentage of each element is 65≤a≤70, 4≤b≤6, 10≤c≤14, 6≤d≤12, 2≤e≤6; The stress annealing conditions are: annealing for 20-40 minutes under nitrogen protection at a stress value of 1400-1680 MPa and an annealing temperature of 350-450°C, and water quenching immediately after annealing; The axial magnetic field annealing conditions are: under nitrogen protection, when the axial magnetic field strength is 0.5-1T, the magnetic field furnace is heated to above 260°C, but not exceeding the Curie temperature of the Co-based magnetic sensitive fiber mother material, and annealed for 20-40 minutes.

2. The Co-based magnetic sensitive fiber material according to claim 1, characterized in that: The pre-treatment temperature of the hot drawing is 150-250°C.

3. The Co-based magnetic sensitive fiber material according to claim 1, characterized in that: The thermal drawing is carried out at a temperature lower than the oxidation temperature of the Co-based magnetically sensitive mother fiber material.

4. The Co-based magnetic sensitive fiber material according to claim 1, characterized in that: The diameter of the Co-based magnetically sensitive mother fiber material is 100-140 μm, and the total compression ratio of the Co-based magnetically sensitive mother fiber material is not less than 30%, but the total compression ratio cannot cause the Co-based magnetically sensitive mother fiber material to break.

5. The Co-based magnetically sensitive fiber material according to any one of claims 1 to 4, characterized in that: The Co-based magnetic sensitive fiber material has a GMI of ≥1010%, a sensitivity of ≥101% / Oe, and an anisotropy field of ≤0.52Oe.

6. Use of the Co-based magnetic sensitive fiber material according to claim 5 in a magnetic sensor.

Citation Information

Patent Citations

  • A method for preparing a magnetosensitive material with high sensitivity and a wide linear region

    CN105679486B

  • A surface processing technology for nickel-titanium shape memory alloy microwires

    CN111633044B

  • Equipment and method for preparing continuous alloy wire with circular section

    CN116694940A

  • New method for preparing high-sensitivity and wide-linear-region magnetic sensitive material

    CN105679486A

  • Method for preparing magnetic sensitive material with high sensitivity and wide linear region by current stress annealing

    CN105695682A