A colored silicon nitride ceramic material and preparation method thereof
Through wet grinding and sintering processes, Eu2O3 and Dy2O3 are used to control the color and density of silicon nitride ceramics, solving the problems of single color and insufficient performance of silicon nitride ceramic materials, and preparing yellow-brown ceramic materials to meet the requirements of backplanes of terminal communication equipment. performance requirements.
Patent Information
- Application Number
- CN202310530553.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-05-12
AI Technical Summary
Existing silicon nitride ceramic materials have a single color, high density, and insufficient impact resistance and thermal shock resistance, making it difficult to meet the needs of terminal communication equipment backplanes.
Wet grinding method is used to prepare silicon nitride, Eu2O3 and Dy2O3 as raw materials, and colored silicon nitride ceramic materials are prepared through drying and sintering processes. Eu2O3 and Dy2O3 are used as colorants and toners, and main group metal oxides are used as sintering materials. Additives to improve the density and mechanical properties of materials.
A yellow-brown silicon nitride ceramic material is prepared, which has high density, excellent fracture toughness and good mechanical properties, meeting the needs of terminal communication equipment backplanes while maintaining good electromagnetic shielding performance.
Smart Images

Figure CN116589283B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silicon nitride ceramics, and in particular relates to a colored silicon nitride ceramic material and a preparation method thereof. Background Art
[0002] With the development of the times and the advancement of science and technology, terminal communication equipment (such as mobile phones and laptops) has become an increasingly important role in daily life. The shell of terminal communication equipment is not only one of the concerns of people when purchasing, but also an important component to protect its internal electronic devices and ensure smooth communication signals. Therefore, it is extremely important to prepare terminal communication equipment shell materials with bright colors, excellent mechanical properties, and good electromagnetic wave transmittance to meet people's life needs.
[0003] Ceramic materials have become the most promising materials. Their excellent wear resistance and dielectric properties can not only meet people's demand for high-end products, but also adapt to the new challenges brought by technological development (5G technology). At present, ZrO2 ceramic materials are mostly used on the market. Although its research on color has gradually matured, ZrO2 has poor impact resistance and thermal shock resistance, and its high density increases the weight of terminal communication equipment, making it difficult to meet people's demand for lightweight terminal communication equipment. Therefore, Si3N4 ceramics with low density and excellent mechanical properties have become potential materials for making backplanes of terminal communication equipment. However, Si3N4 ceramics are still limited in application due to shortcomings such as single color and low toughness.
[0004] Rare earth oxides have attracted extensive attention from researchers due to their stable chemical properties. In addition to being used as sintering aids to promote the sintering of Si3N4, they also exhibit excellent coloring ability. It has been reported that yellow, green and other colored silicon nitride ceramic materials have been successfully fired using rare earth oxides as colorants. However, the colors of colored silicon nitride ceramics are still relatively single and cannot meet market demand. Summary of the invention
[0005] The purpose of the present invention is to provide a colored silicon nitride ceramic material and a preparation method thereof. The colored silicon nitride ceramic material prepared by the present invention is yellow-brown, enriching the color of silicon nitride ceramics, and has high density, excellent fracture toughness, good mechanical properties and electromagnetic shielding properties, and can meet its demand as a backplane material for terminal communication equipment.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a colored silicon nitride ceramic material, comprising the following steps:
[0008] Wet grinding the raw materials to obtain a wet mixed material; the raw materials include silicon nitride, a sintering aid, Eu2O3 and Dy2O3; the sintering aid includes a main group metal oxide and other rare earth metal oxides except Eu2O3 and Dy2O3;
[0009] Drying the wet mixed material and then sieving it to obtain a mixed powder;
[0010] The mixed powder is heated and sintered to obtain the colored silicon nitride ceramic material.
[0011] Preferably, the raw materials for preparation include the following components in percentage by mass: 78-91% silicon nitride, 5-15% sintering aid, 2-10% Eu2O3 and 2-10% Dy2O3.
[0012] Preferably, the main group metal oxides include MgO and / or Al2O3; the other rare earth metal oxides except Eu2O3 and Dy2O3 are one or more of Y2O3, La2O3 and Ce2O3.
[0013] Preferably, the sintering aids are Y2O3, Al2O3 and MgO; the mass ratio of Y2O3, Al2O3 and MgO is 5:5:2.
[0014] Preferably, the silicon nitride is α-silicon nitride, and the particle size of the silicon nitride is 0.5 to 1.5 μm.
[0015] Preferably, the co-solvent for wet grinding is anhydrous ethanol; the solid-liquid ratio of the wet grinding is (3-5):1; the ball-to-material ratio is (1-3):1; the grinding speed is 100-300 r / min; and the grinding time is 6-12 h.
[0016] Preferably, the sintering holding temperature is 1700-1850°C, and the holding time is 5-45 minutes;
[0017] The sintering includes gas pressure sintering, spark plasma sintering or pressureless sintering;
[0018] The sintering pressure of the gas pressure sintering or spark plasma sintering is independently 20-30 MPa; the sintering pressure of the pressureless sintering is normal pressure.
[0019] Preferably, the sintering temperature rising procedure is: heating from room temperature to an intermediate temperature according to a first heating rate for intermediate insulation; heating from the intermediate temperature to the sintering insulation temperature according to a second heating rate; the intermediate temperature is 1350-1400°C, the intermediate insulation time is 3-5min, and the first heating rate and the second heating rate are independently 80-100°C / min.
[0020] Preferably, the drying is forced air drying; the temperature of the forced air drying is 50-80°C.
[0021] The present invention provides a colored silicon nitride ceramic material prepared by the preparation method described in the above technical solution, and the color of the colored silicon nitride ceramic material is yellow-brown.
[0022] The present invention provides a method for preparing a colored silicon nitride ceramic material, comprising the following steps: wet grinding the raw materials to obtain a wet mixture; the raw materials include silicon nitride, a sintering aid, Eu2O3 and Dy2O3; the sintering aid includes a main group metal oxide and other rare earth metal oxides except Eu2O3 and Dy2O3; the wet mixture is dried and sieved to obtain a mixed powder; the mixed powder is heated and sintered to obtain the colored silicon nitride ceramic material. The preparation method provided by the present invention uses Eu2O3 as a colorant and Dy2O3 as a toner, and controls the original gray color of the silicon nitride material by combining Eu2O3 and Dy2O3, thereby obtaining a yellow-brown silicon nitride ceramic, which enriches the color of the silicon nitride ceramic. At the same time, the present invention uses main group metal oxides and other rare earth metal oxides except Eu2O3 and Dy2O3 as sintering aids, and cooperates with Eu2O3 and Dy2O3 to effectively improve the density of colored silicon nitride ceramics, thereby improving their mechanical properties. The results of the examples show that the silicon nitride ceramics prepared by the present invention have good mechanical properties and electromagnetic shielding properties, which can meet the needs of being used as a backplane material for terminal communication equipment. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Optical photographs of silicon nitride ceramic materials prepared in Comparative Examples 1 to 3 of the present invention;
[0024] Figure 2 Optical photographs of silicon nitride ceramic materials prepared in Examples 1 to 3 of the present invention and Comparative Example 1;
[0025] Figure 3 X-ray diffraction patterns of silicon nitride ceramic materials prepared in Examples 1 to 3 of the present invention and Comparative Example 1;
[0026] Figure 4 These are SEM images of the surface and cross-section of the silicon nitride ceramic materials prepared in Examples 1 to 3 of the present invention and Comparative Example 1.
[0027] Figure 5 This is a SEM image of the indentation crack of the silicon nitride ceramic material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0028] The present invention provides a method for preparing a colored silicon nitride ceramic material, comprising the following steps:
[0029] Wet grinding the raw materials to obtain a wet mixed material; the raw materials include silicon nitride, a sintering aid, Eu2O3 and Dy2O3; the sintering aid includes a main group metal oxide and other rare earth metal oxides except Eu2O3 and Dy2O3;
[0030] Drying the wet mixed material and then sieving it to obtain a mixed powder;
[0031] The mixed powder is heated and sintered to obtain the colored silicon nitride ceramic material.
[0032] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.
[0033] The present invention wet-grinds the raw materials to obtain a wet mixed material; the raw materials include silicon nitride, a sintering aid, Eu2O3 and Dy2O3; the sintering aid includes main group metal oxides and other rare earth metal oxides except Eu2O3 and Dy2O3.
[0034] In the present invention, the preparation raw materials preferably include the following components in percentage by mass: silicon nitride 78-91%, sintering aid 5-15%, Eu2O3 2-10% and Dy2O3 2-10%; more preferably: silicon nitride 78-85%, sintering aid 8-13%, Eu2O3 3-6% and Dy2O3 2-6%; further preferably: silicon nitride 78-80%, sintering aid 12%, Eu2O34% and Dy2O3 4-6%.
[0035] In the present invention, the silicon nitride is specifically α-silicon nitride; the particle size of the silicon nitride is preferably 0.5 to 1.5 μm, more preferably 1.0 to 1.5 μm.
[0036] In the present invention, the main group metal oxide preferably includes MgO and / or Al2O3, more preferably MgO and Al2O3; other rare earth metal oxides except Eu2O3 and Dy2O3 are preferably one or more of Y2O3, La2O3 and Ce2O3, more preferably Y2O3.
[0037] In the present invention, the sintering aid is preferably Y2O3, Al2O3 and MgO. The mass ratio of Y2O3, Al2O3 and MgO is preferably 5:5:2.
[0038] In the present invention, the sintering aids are preferably Y2O3, Al2O3 and MgO. The present invention uses Y2O3, Al2O3 and MgO together as sintering aids, which can effectively reduce the sintering temperature of the ceramic and improve its density.
[0039] In the present invention, the sintering aid is preferably Y2O3, Al2O3 and MgO, the colorant is Eu2O3, and the toner is Dy2O3. The present invention can effectively increase the ratio of α-phase silicon nitride converted to β-phase silicon nitride by adding sintering aids, colorants and toners, thereby making the fracture toughness of the prepared silicon nitride ceramic material more excellent, and the addition of colorants and toners does not have a significant negative impact on the electromagnetic shielding properties of silicon nitride, and still meets the requirements for it to be used as a backplane material for terminal communication equipment.
[0040] In the present invention, the specific implementation of the wet grinding is preferably wet ball milling. The wet grinding preferably includes the following steps: putting the raw materials and ball milling beads into a ball milling jar, adding a co-solvent and stirring and mixing them evenly, and then wet ball milling; the material of the ball milling jar is preferably polytetrafluoroethylene; the mesh number of the ball milling beads is preferably greater than 100 meshes.
[0041] In the present invention, the co-solvent for wet grinding is preferably anhydrous ethanol; the solid-liquid ratio of the wet grinding is preferably (3-5):1, more preferably 3:1.
[0042] In the present invention, the ball-to-material ratio of the wet grinding is preferably (1-3):1, more preferably 2:1.
[0043] In the present invention, the grinding speed of the wet grinding is preferably 100 to 300 r / min, more preferably 150 to 250 r / min; the grinding time is preferably 6 to 12 h, more preferably 6 to 10 h.
[0044] After obtaining the wet mixed material, the present invention dries the wet mixed material and then sieves it to obtain a mixed powder.
[0045] In the present invention, the drying is preferably air drying. In the present invention, the air drying is preferably carried out in an air drying oven, and the temperature of the air drying is preferably 50 to 80° C., more preferably 60 to 80° C. In the present invention, before the drying, the co-solvent in the wet mixture is preferably removed by rotary evaporation.
[0046] In the present invention, the mesh size of the sieve used for the sieving is preferably 100 meshes. In the present invention, the ball milling beads are preferably separated by sieving.
[0047] After obtaining the mixed powder, the present invention heats and sinters the mixed powder to obtain the colored silicon nitride ceramic material.
[0048] In the present invention, the sintering temperature rising program is preferably: heating from room temperature to an intermediate temperature according to a first heating rate for intermediate insulation; heating from the intermediate temperature to the sintering insulation temperature according to a second heating rate. In the present invention, the intermediate temperature is preferably 1350-1400°C, more preferably 1400°C; the intermediate insulation time is preferably 3-5min, more preferably 5min; the first heating rate is preferably 80-100°C / min, more preferably 100°C / min; the second heating rate is preferably 80-100°C / min, more preferably 100°C / min. The present invention preferably uses a segmented heating program to ensure that the mixed powder is heated evenly, which helps to transform silicon nitride from α phase to β phase during the sintering process.
[0049] In the present invention, the sintering holding temperature is preferably 1700-1850° C., more preferably 1750-1800° C.; the holding time is preferably 5-45 min, more preferably 30-45 min.
[0050] In the present invention, the specific implementation of the sintering preferably includes pressureless sintering, gas pressure sintering or spark plasma sintering, and more preferably spark plasma sintering.
[0051] In the present invention, the sintering pressure of the gas pressure sintering or spark plasma sintering is preferably 20 to 30 MPa, more preferably 22 to 27 MPa. In the present invention, the sintering pressure of the pressureless sintering is preferably normal pressure.
[0052] In the present invention, after the colored silicon nitride ceramic material is obtained by sintering, the present invention preferably performs a performance test on the prepared colored silicon nitride ceramic material, and the performance test includes a mechanical property test and a wave transmission performance test. Among them, the indicators of mechanical properties include hardness, bending strength and fracture toughness. The indicator of wave transmission performance is electromagnetic shielding effectiveness.
[0053] The above-mentioned preparation method provided by the present invention selects suitable sintering aids, colorants, and toners, and mixes them with α-silicon nitride according to the above-mentioned mass percentage through ball milling, drying, and screening, and then uses spark plasma sintering to prepare colored silicon nitride ceramic materials. The sintering aid can effectively reduce the sintering temperature of silicon nitride and promote the proportion of α phase transformation to β phase, thereby improving the fracture toughness of the silicon nitride material. The toner can regulate the original color of silicon nitride, enrich the color of silicon nitride, and make the prepared colored silicon nitride material more widely used in the backplane material of terminal communication equipment.
[0054] The present invention provides a colored silicon nitride ceramic material prepared by the preparation method described in the above technical solution, and the color of the colored silicon nitride ceramic material is yellow-brown.
[0055] The colored silicon nitride ceramic material provided by the present invention is yellow-brown, enriches the color of silicon nitride ceramics, has high density, excellent fracture toughness, good mechanical properties and electromagnetic shielding properties, and can meet the demand for it as a backplane material for terminal communication equipment.
[0056] The relative density of the colored silicon nitride ceramic material provided by the present invention is greater than 96.98%, the Vickers hardness is 1584-1635HV, the bending strength is 732-767MPa, and the fracture toughness is 7.3-8.5MPa·m 1 / 2 ;Total shielding effectiveness 4.8~5.2dB.
[0057] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0058] Comparative Example 1:
[0059] (1) α-silicon nitride is used as a raw material, and Y2O3-Al2O3-MgO is used as a sintering aid, wherein the mass ratio of α-silicon nitride, Y2O3, Al2O3 and MgO is 88:5:5:2, and they are weighed in sequence according to the above ratio;
[0060] (2) putting various powders and ball milling beads weighed in step (1) into a polytetrafluoroethylene ball milling jar, adding 40 mL of anhydrous ethanol and stirring thoroughly, placing the ball milling jar in a ball mill, and the ball milling parameters are: solid-liquid ratio of 3:1, ball-to-material ratio of 2:1, ball milling speed of 200 r / min, and ball milling time of 6 h;
[0061] (3) transferring the wet mixture obtained in step (2) into a flask, distilling out the anhydrous ethanol by a rotary evaporator, and drying the mixture in a forced air drying oven at 80° C., and then separating the ball powder with a 100-mesh sieve to obtain a mixed powder;
[0062] (4) The mixed powder obtained in step (3) is sintered into a mold by spark plasma sintering, with a heating rate of 100°C / min and a sintering pressure of 25MPa. The temperature is first raised to 1400°C, kept at this temperature for 5 minutes, and then continued to be raised to 1800°C, kept at this temperature for 45 minutes, and then cooled to room temperature to obtain a gray silicon nitride ceramic material.
[0063] (5) Performance testing: measuring the relative density, Vickers hardness, bending strength, fracture toughness, and total shielding effectiveness of the gray silicon nitride ceramic material prepared in step (4).
[0064] Comparative Example 2:
[0065] (1) α-silicon nitride is used as a raw material, Y2O3-Al2O3-MgO is used as a sintering aid, and Eu2O3 is used as a colorant, wherein the mass ratio of α-silicon nitride, Y2O3, Al2O3, MgO and Eu2O3 is 84:5:5:2:4, and they are weighed in sequence according to the above ratio;
[0066] (2) putting various powders and ball milling beads weighed in step (1) into a polytetrafluoroethylene ball milling jar, adding 40 mL of anhydrous ethanol and stirring thoroughly, placing the ball milling jar in a ball mill, and the ball milling parameters are: solid-liquid ratio of 3:1, ball-to-material ratio of 2:1, ball milling speed of 200 r / min, and ball milling time of 6 h;
[0067] (3) transferring the wet mixture obtained in step (2) into a flask, distilling out the anhydrous ethanol by a rotary evaporator, and drying the mixture in a forced air drying oven at 80° C., and then separating the ball powder with a 100-mesh sieve to obtain a mixed powder;
[0068] (4) The mixed powder obtained in step (3) is sintered into a mold by a spark plasma sintering process, with a heating rate of 100°C / min and a sintering pressure of 25MPa. The temperature is first raised to 1400°C, kept at this temperature for 5 minutes, and then continued to be raised to 1800°C, kept at this temperature for 45 minutes, and then cooled to room temperature to obtain a yellow silicon nitride ceramic material.
[0069] Comparative Example 3:
[0070] (1) Using α-silicon nitride as a raw material, Y2O3-Al2O3-MgO as a sintering aid, and Dy2O3 as a colorant, the mass ratio of α-silicon nitride, Y2O3, Al2O3, MgO and Dy2O3 is 84:5:5:2:4, and they are weighed in sequence according to the above ratio;
[0071] (2) putting various powders and ball milling beads weighed in step (1) into a polytetrafluoroethylene ball milling jar, adding 40 mL of anhydrous ethanol and stirring thoroughly, placing the ball milling jar in a ball mill, and the ball milling parameters are: solid-liquid ratio of 3:1, ball-to-material ratio of 2:1, ball milling speed of 200 r / min, and ball milling time of 6 h;
[0072] (3) transferring the wet mixture obtained in step (2) into a flask, distilling out the anhydrous ethanol by a rotary evaporator, and drying the mixture in a forced air drying oven at 80° C., and then separating the ball powder with a 100-mesh sieve to obtain a mixed powder;
[0073] (4) The mixed powder obtained in step (3) is sintered into a mold by a spark plasma sintering process, with a heating rate of 100°C / min and a sintering pressure of 25MPa. The temperature is first raised to 1400°C, kept at this temperature for 5 minutes, and then continued to be raised to 1800°C, kept at this temperature for 45 minutes, and then cooled to room temperature to obtain a gray silicon nitride ceramic material.
[0074] The optical photographs of the silicon nitride materials prepared in Comparative Examples 1 to 3 are as follows: Figure 1 As shown, from Figure 1 It can be observed that the silicon nitride material is gray when there is no colorant. The addition of Eu2O3 alone changes the color of the silicon nitride material from gray to bright yellow, and the color is more uniform. When Dy2O3 is added alone, the silicon nitride material is still gray. The above color changes indicate that Eu2O3 as a single colorant can change the color of the silicon nitride material, while Dy2O3 as a single colorant cannot change the color of the silicon nitride material. In addition, from the appearance, the sample has no cracks and no obvious pores on the surface.
[0075] Embodiment 1:
[0076] (1) α-silicon nitride is used as a raw material, Y2O3-Al2O3-MgO is used as a sintering aid, Eu2O3 is used as a colorant, and Dy2O3 is used as a toner. The mass ratio of α-silicon nitride, Y2O3, Al2O3, MgO, Eu2O3 and Dy2O3 is 82:5:5:2:4:2, and they are weighed in sequence according to the above ratio;
[0077] (2) putting various powders and ball milling beads weighed in step (1) into a polytetrafluoroethylene ball milling jar, adding 40 mL of anhydrous ethanol and stirring thoroughly, placing the ball milling jar in a ball mill, and the ball milling parameters are: solid-liquid ratio of 3:1, ball-to-material ratio of 2:1, ball milling speed of 200 r / min, and ball milling time of 6 h;
[0078] (3) transferring the wet mixture obtained in step (2) into a flask, distilling out the anhydrous ethanol by a rotary evaporator, and drying the mixture in a forced air drying oven at 80° C., and then separating the ball powder with a 100-mesh sieve to obtain a mixed powder;
[0079] (4) The mixed powder obtained in step (3) is sintered into a mold by a spark plasma sintering process, with a heating rate of 100°C / min and a sintering pressure of 25MPa. The temperature is first raised to 1400°C, kept at this temperature for 5 minutes, and then continued to be raised to 1800°C, kept at this temperature for 45 minutes, and then cooled to room temperature to obtain a yellow-brown silicon nitride ceramic material.
[0080] (5) Performance testing, measuring the relative density, Vickers hardness, bending strength, fracture toughness, and total shielding effectiveness of the yellow-brown silicon nitride ceramic material prepared in step (4).
[0081] Embodiment 2:
[0082] (1) α-silicon nitride is used as a raw material, Y2O3-Al2O3-MgO is used as a sintering aid, Eu2O3 is used as a colorant, and Dy2O3 is used as a toner. The mass ratio of α-silicon nitride, Y2O3, Al2O3, MgO, Eu2O3 and Dy2O3 is 80:5:5:2:4:4, and they are weighed in sequence according to the above ratio;
[0083] (2) putting various powders and ball milling beads weighed in step (1) into a polytetrafluoroethylene ball milling jar, adding 40 mL of anhydrous ethanol and stirring thoroughly, placing the ball milling jar in a ball mill, and the ball milling parameters are: solid-liquid ratio of 3:1, ball-to-material ratio of 2:1, ball milling speed of 200 r / min, and ball milling time of 6 h;
[0084] (3) transferring the wet mixture obtained in step (2) into a flask, distilling out the anhydrous ethanol by a rotary evaporator, and drying the mixture in a forced air drying oven at 80° C., and then separating the ball powder with a 100-mesh sieve to obtain a mixed powder;
[0085] (4) The mixed powder obtained in step (3) is sintered into a mold by a spark plasma sintering process, with a heating rate of 100°C / min and a sintering pressure of 25MPa. The temperature is first raised to 1400°C, kept at this temperature for 5 minutes, and then continued to be raised to 1800°C, kept at this temperature for 45 minutes, and then cooled to room temperature to obtain a yellow-brown silicon nitride ceramic material.
[0086] (5) Performance testing, measuring the relative density, Vickers hardness, bending strength, fracture toughness, and total shielding effectiveness of the yellow-brown silicon nitride ceramic material prepared in step (4).
[0087] Embodiment 3:
[0088] (1) α-silicon nitride is used as a raw material, Y2O3-Al2O3-MgO is used as a sintering aid, Eu2O3 is used as a colorant, and Dy2O3 is used as a toner. The mass ratio of α-silicon nitride, Y2O3, Al2O3, MgO, Eu2O3 and Dy2O3 is 78:5:5:2:4:6, and they are weighed in sequence according to the above ratio;
[0089] (2) putting various powders and ball milling beads weighed in step (1) into a polytetrafluoroethylene ball milling jar, adding 40 mL of anhydrous ethanol and stirring thoroughly, placing the ball milling jar in a ball mill, and the ball milling parameters are: solid-liquid ratio of 3:1, ball-to-material ratio of 2:1, ball milling speed of 200 r / min, and ball milling time of 6 h;
[0090] (3) transferring the wet mixture obtained in step (2) into a flask, distilling out the anhydrous ethanol by a rotary evaporator, and drying the mixture in a forced air drying oven at 80° C., and then separating the ball powder with a 100-mesh sieve to obtain a mixed powder;
[0091] (4) The mixed powder obtained in step (3) is sintered into a mold by a spark plasma sintering process, with a heating rate of 100°C / min and a sintering pressure of 25MPa. The temperature is first raised to 1400°C, kept at this temperature for 5 minutes, and then continued to be raised to 1800°C, kept at this temperature for 45 minutes, and then cooled to room temperature to obtain a yellow-brown silicon nitride ceramic material.
[0092] (5) Performance testing, measuring the relative density, Vickers hardness, bending strength, fracture toughness, and total shielding effectiveness of the yellow-brown silicon nitride ceramic material prepared in step (4).
[0093] The optical photographs of the silicon nitride materials prepared in Comparative Example 1 and Examples 1 to 3 are as follows: Figure 2 As shown, from Figure 2 It can be seen that with the increase of Dy2O3 content, the sample changes from yellow to yellow-brown, and the color gradually deepens, indicating that although Dy2O3 cannot change the color of silicon nitride alone, it can regulate the color based on the color of silicon nitride material.
[0094] The relative density, Vickers hardness, bending strength, fracture toughness and total shielding effectiveness of the yellow-brown silicon nitride materials prepared in Comparative Example 1 and Examples 1 to 3 were tested, and the results are shown in Table 1: Table 1 Relative density, Vickers hardness, bending strength, fracture toughness and total shielding effectiveness of the yellow-brown silicon nitride materials prepared in Examples 1 to 3
[0095] Relative density (%) Vickers hardness (HV) Bending strength(MPa) <![CDATA[Fracture toughness (MPa·m 1 / 2 )]]> Total shielding effectiveness (dB) Comparative Example 1 98.74 1865.69 921.84 7.14 4.71 Example 1 96.98 1584.63 732.65 8.45 4.83 Example 2 98.01 1634.51 764.01 7.96 5.02 Example 3 98.24 1652.32 766.64 7.35 5.14
[0096] The density of yellow-brown silicon nitride ceramics was measured by the Archimedean drainage method, and its relative density was calculated. The Vickers hardness of silicon nitride ceramic materials was tested by a Vickers hardness tester (FALCON 507), with a load of 9.8N and a holding time of 10s. A universal mechanical testing machine (CMT6103) was used for a three-point bending test, with a sample size of 2×3×25mm, a span of 20mm during the test, and a test loading rate of 0.5mm / min. The fracture toughness of silicon nitride materials was measured by an indentation method, with a load of 49N applied and held for 15s, and then the diagonal crack length of the indentation was measured using an optical microscope, such as Figure 5 The electromagnetic scattering S parameters of silicon nitride material were tested by a vector network analyzer (E5071C) at X-band (8.2-12.4 GHz). The sample size was 22.8×10.1×2 mm, and the total shielding effectiveness at 10 GHz was calculated.
[0097] The relative density of the yellow-brown silicon nitride material prepared in the above examples is higher than 96.98%. Figure 3 It can be seen that the peak value of the β(101) characteristic peak (PDF#33-1160) of the yellow-brown silicon nitride material at 2θ=33.665° is very obvious, and its β phase content is higher than 77.40%. The presence of β phase silicon nitride grains can be observed from the SEM images of its surface and cross section, such as Figure 4 In addition, the yellow-brown silicon nitride material prepared in the above examples has good mechanical properties, wherein the fracture toughness of the yellow-brown silicon nitride material in Example 1 can reach up to 8.45 MPa·m 1 / 2 ,from Figure 5 It can be observed that the indentation cracks of the yellow-brown silicon nitride material in Example 1 have transgranular fracture, crack deflection and crack bridging toughening mechanisms. In addition, the electromagnetic shielding performance of the yellow-brown silicon nitride material meets the requirements for use as a backplane material for terminal communication equipment.
[0098] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a colored silicon nitride ceramic material, characterized in that: The following steps are involved: Wet grinding the raw materials to obtain a wet mixed material; the raw materials include silicon nitride, a sintering aid, Eu2O3 and Dy2O3; the sintering aid is Y2O3, Al2O3 and MgO; the mass ratio of Y2O3, Al2O3 and MgO is 5:5:2; the raw materials include the following components in mass percentage: 78-91% silicon nitride, 5-15% sintering aid, 2-10% Eu2O3 and 2-10% Dy2O3; Drying the wet mixed material and then sieving it to obtain a mixed powder; The mixed powder is heated and sintered to obtain the colored silicon nitride ceramic material, and the color of the colored silicon nitride ceramic material is yellow-brown.
2. The preparation method according to claim 1, characterized in that: The silicon nitride is α-silicon nitride, and the particle size of the silicon nitride is 0.5 to 1.5 μm.
3. The preparation method according to claim 1, characterized in that: The auxiliary solvent of the wet grinding is anhydrous ethanol; the solid-liquid ratio of the wet grinding is (3-5):1; the ball-to-material ratio is (1-3):1; the grinding speed is 100-300 r / min; and the grinding time is 6-12 hours.
4. The preparation method according to claim 1, characterized in that: The sintering holding temperature is 1700-1850°C, and the holding time is 5-45 minutes; The sintering includes gas pressure sintering, spark plasma sintering or pressureless sintering; The sintering pressure of the gas pressure sintering or spark plasma sintering is independently 20-30 MPa; the sintering pressure of the pressureless sintering is normal pressure.
5. The preparation method according to claim 1, characterized in that: The sintering temperature rising procedure is: heating from room temperature to an intermediate temperature according to a first heating rate and then holding the temperature in the middle; heating from the intermediate temperature to the holding temperature for sintering according to a second heating rate; the intermediate temperature is 1350-1400°C, the intermediate holding time is 3-5 minutes, and the first heating rate and the second heating rate are independently 80-100°C / min.
6. The preparation method according to claim 1, characterized in that: The drying is forced air drying; the temperature of the forced air drying is 50-80°C.
7. The colored silicon nitride ceramic material prepared by the preparation method according to any one of claims 1 to 6, characterized in that: The color of the colored silicon nitride ceramic material is yellow-brown.
Citation Information
Patent Citations
Cyan silicon nitride ceramic and preparation method thereof
CN112110734A
Color-adjustable light storage ceramic and preparation method thereof
CN115557780A