A method for improving the antimony element recovery rate in the smelting of antimony-containing steel.

By using a mixture of antimony oxide powder and activated carbon or charcoal powder in the steel smelting process, the problems of low antimony recovery rate and high alloying cost have been solved, achieving efficient antimony alloying, improving the antimony recovery rate and reducing costs.

CN116590542BActive Publication Date: 2026-11-17LIANFENG STEEL (ZHANGJIAGANG) CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310503217.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2026-11-17
Estimated Expiration
2043-05-06

AI Technical Summary

Technical Problem

In existing technologies, the yield of antimony in steel smelting is low, alloying costs are high, and the smelting process is complex.

Method used

A mixture of antimony oxide powder and activated carbon powder or charcoal powder is used. After being mixed evenly by a powder mixer, the mixture is placed in a reaction bag and added to the molten steel during the tapping process. The rapid reducing agent reacts with the antimony oxide powder at high temperature to generate antimony metal, thereby improving the yield.

Benefits of technology

It significantly increases the antimony yield to over 90%, reduces alloying costs, simplifies the process, and shortens alloying time.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a method for improving the antimony yield during antimony-containing steel smelting, belonging to the field of iron and steel metallurgical technology. The method includes the following steps: S01, preparation of an antimony-oxygen powder mixture: mixing antimony-oxygen powder and a rapid reducing agent at a mass ratio of 1:(0.13~0.3), and loading the mixture into reaction bags, with each bag containing 5kg~30kg of the mixture; S02, before tapping, adding 0.14~0.32% of the antimony-oxygen powder mixture to the ladle based on the tapping weight; or at the start of tapping, adding 0.14~0.32% of the antimony-oxygen powder mixture to the steel stream based on the tapping weight. After tapping, the antimony content in the molten steel is detected, and the molten steel is stirred at an argon blowing station for 3~5 minutes while the antimony content is detected again, resulting in antimony-containing molten steel. This invention not only improves the antimony yield but also reduces the cost of antimony alloying.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for improving the antimony element recovery rate during the smelting of antimony-containing steel, belonging to the field of iron and steel metallurgical technology. Background Technology

[0002] Antimony (Sb) is a silvery-gray metal that is acid-resistant at room temperature. It has a relative density of 6.68 and a melting point of 630.0℃. It is brittle and non-ductile. Antimony is a poor conductor of electricity and heat, does not readily oxidize at room temperature, and has corrosion resistance. The addition of antimony (Sb) can improve the resistance of steel to uniform corrosion.

[0003] In current steelmaking processes, antimony is added in bulk form during LF refining. However, the large size of these antimony blocks makes them difficult to melt quickly in molten steel. Furthermore, antimony has a low melting point and is easily volatilized, resulting in a low yield of antimony alloying, only around 70%. Besides the high volatility of antimony, the price of antimony metal is also high, leading to high alloying costs.

[0004] Patent CN107177772A discloses a method for adding antimony during the smelting of antimony-containing steel. The process involves placing an aluminum alloy and an antimony alloy into a steel container, heating the container to 700–900°C, and holding it at that temperature for 0.5–2 hours to melt the two alloys. Then, during the tapping process in the converter, the steel container containing the liquid aluminum-antimony alloy is added to the molten steel in the ladle. The container melts, and the liquid aluminum-antimony alloy dissolves into the molten steel. This invention involves a complex process and places extremely high demands on the performance of the steel container.

[0005] Patent CN111519085A discloses an antimony-containing weathering steel, its smelting method, and its application. The method includes: obtaining molten steel from an electric furnace; subjecting the molten steel to vacuum treatment to obtain vacuum-treated molten steel; wherein the vacuum treatment pressure is ≤67 Pa, and the temperature of the vacuum-treated molten steel is 1635–1700 °C; and adding ferroantimony to the vacuum-treated molten steel to adjust its composition to obtain antimony-containing molten steel. This invention uses a method of directly adding ferroantimony to the molten steel, which cannot guarantee the antimony element recovery rate.

[0006] Patent CN105950829A discloses an antimony wire for RH refining and its addition method, which involves adding antimony ingots to molten steel using a wire feeding method. This invention employs a wire feeding method for antimony alloying, but the processing cycle is long.

[0007] The above smelting process can achieve the purpose of antimony alloying, but it has problems such as complex smelting process, low antimony yield, and high cost of antimony alloying. Summary of the Invention

[0008] The problem to be solved by the present invention is to provide a method for improving the antimony element recovery rate in the smelting of antimony-containing steel, so as to solve the problems of low antimony element recovery rate and high antimony alloying cost in the existing technology for smelting antimony-containing steel.

[0009] Meanwhile, the present invention provides a method for improving the antimony element recovery rate during the smelting of antimony-containing steel according to the present invention, thereby obtaining antimony-containing steel.

[0010] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows:

[0011] A method for improving the antimony element recovery rate during the smelting of antimony-containing steel includes the following steps:

[0012] S01, Preparation of antimony-oxygen powder mixture: Use a powder mixer to mix antimony-oxygen powder and rapid reducing agent at a mass ratio of 1:(0.13~0.3), and load the mixture into reaction bags, with each reaction bag containing 5kg~30kg of the mixture.

[0013] S02, before tapping, adds a mixture of antimony-oxygen powder equivalent to 0.14-0.32% of the tapping amount to the ladle; or at the beginning of tapping, adds a mixture of antimony-oxygen powder equivalent to 0.14-0.32% of the tapping amount to the steel stream. After tapping is completed, the antimony content in the molten steel is detected, and the molten steel is stirred at the argon blowing station for 3-5 minutes and the antimony content in the molten steel is detected again to obtain antimony-containing molten steel.

[0014] The antimony oxide powder comprises the following components by weight percentage: Sb₂O₃: 96.2%; S: 0.35%; SiO₂: 2.36%; CaO: 0.15%; FeO: 0.02%; Fe₂O₃: 0.58%; Al₂O₃: 0.13% and MgO: 0.21%.

[0015] Rapid reducing agents include activated carbon powder or charcoal powder.

[0016] Activated carbon powder comprises the following components by weight percentage: fixed carbon: 45.29–59.73%; ash: 5.26–6.65%; volatile matter: 33.62–45.45%; and H2O: 0–4.0%.

[0017] The steel is tapped from a converter or electric furnace at a temperature of 1600–1630℃; the argon flow rate at the argon blowing station is 200–300 Nm³. 3 / h.

[0018] The antimony content of the antimony-containing steel obtained by the method described in this invention is 0.0985% to 0.2%.

[0019] The antimony-containing steel of the present invention is a steel grade containing 0.0985% to 0.2% antimony.

[0020] The reaction bags are made of canvas, plastic, or linen, including but not limited to woven bags and burlap sacks.

[0021] The antimony-containing steel melt of this invention, after being processed through LF refining and VD refining processes, produces qualified cast billets (i.e., antimony-containing steel). This invention not only improves the antimony yield but also reduces the cost of antimony alloying.

[0022] The LF refining process of the present invention is as follows: the slag basicity is 2.0 to 2.6, the white slag time is more than 15 minutes, and the soft blowing argon time is more than 20 minutes.

[0023] The VD refining process of this invention is as follows: the vacuum degree is 30-70 Pa.

[0024] The antimony content in the antimony-containing steel finally obtained by this invention is 0.0985% to 0.2%, and the antimony recovery rate is >90%. To achieve the above objective, according to one aspect of this invention, an antimony-oxygen powder mixture and a reaction bag for the mixture are provided. First, antimony-oxygen powder and activated carbon powder or charcoal powder are used. The main component of the antimony-oxygen powder is Sb₂O₃, and the price of antimony metal in the antimony-oxygen powder is lower than that of antimony ingots. The antimony-oxygen powder and activated carbon powder (charcoal powder) are mixed evenly using a powder mixer, with a mass ratio of antimony-oxygen powder to activated carbon powder (charcoal powder) of 1:0.13 to 0.3. The mixture is then packaged in a reaction bag, which can be made of canvas, plastic, or hemp material, including but not limited to woven bags and burlap sacks. The reaction bag provided by this invention has two functions: First, since the antimony-oxygen powder mixture is a powdery substance, it is easily dispersed during the addition process. The reaction bag provided by this invention can prevent the powder from dispersing during the material addition process, thereby improving the antimony recovery rate. Secondly, the rapid reduction of antimony-oxygen powder requires a high-temperature environment. The reaction bag provided by this invention is easy to melt and melts immediately upon contact with molten steel, facilitating the rapid reaction of the antimony-oxygen powder mixture.

[0025] According to another aspect of the present invention, a novel process for antimony alloying is provided. During the tapping process in a converter or electric furnace, before tapping, a mixture of antimony and oxygen powder, equivalent to 0.14–0.32% of the tapped steel, is added to the ladle; or, at the beginning of tapping, the antimony and oxygen powder mixture is added to the steel stream. This mixture rapidly melts and reacts in the molten steel, achieving rapid alloying. Since the antimony alloying amount is only 0.0985%–0.2%, its impact on the temperature drop and quality of the molten steel is minimal and negligible.

[0026] Antimony oxide powder is a powdery substance whose main component is Sb2O3. The reaction of antimony oxide powder with carbon is shown in equations (1) to (3).

[0027] Sb2O3(s)+3C(s)=2Sb(s)+3CO Δ r G 0 =344400-498.39T (1)

[0028] Sb2O3(s)+3C(s)=2Sb(l)+3CO Δ r G 0 =384200-542.39T (2)

[0029] Sb2O3(l)+3C(s)=2Sb(l)+3CO Δ r G 0 =317450-455.42T (3)

[0030] Where l represents liquid, s represents solid, and Δ r G 0 The standard Gibbs free energy change represents the reaction, and T represents the reaction temperature in K.

[0031] The initial reaction temperatures of equations (1) to (3) are all below 500℃, indicating that Sb₂O₃ is easily reduced. The activated carbon powder or charcoal powder provided by this invention has a specific surface area of ​​100m². 2 / g or more, far exceeding the specific surface area of ​​ordinary pulverized coal (20m²). 2 (Below / g), with a large contact area with antimony oxide powder, the antimony oxide powder is mixed with activated carbon powder or charcoal powder using a powder mixer. The two can easily undergo a reduction reaction. The antimony metal generated by the reaction directly enters the molten steel, and the generated CO gas is discharged from the molten steel into the gas.

[0032] Given that the combination of antimony oxide powder, activated carbon powder or charcoal powder and reaction bag in this invention has the characteristic of easy reduction, the reduction of antimony oxide powder in this invention does not require the addition of additional flux.

[0033] Before or during tapping, the rapid reducing agent and reaction bag provided by this invention can quickly react with antimony oxide powder, thereby increasing the antimony yield.

[0034] The antimony-containing steel of the present invention has a high antimony recovery rate, low antimony alloying cost, and simple and convenient antimony alloying material preparation. At the same time, the antimony alloying time is short, and the antimony alloying can be completed after the steel is tapped.

[0035] The present invention has the following technical effects or advantages:

[0036] (1) The cost of antimony alloying raw materials (antimony-oxygen powder mixture) is lower than that of antimony ingots;

[0037] (2) The antimony yield is higher than that of antimony ingots;

[0038] (3) The raw materials for antimony alloying are all powders with a particle size much smaller than antimony blocks. The antimony alloying time is short and the process stability is strong.

[0039] (4) The amount of slag produced by antimony alloying is less than 0.1 kg / (t·steel), which can be ignored. Detailed Implementation

[0040] The present invention will be further described in detail below with reference to specific embodiments. The following embodiments are for illustrative purposes only and are not intended to limit the scope of the invention.

[0041] Example 1

[0042] A method for improving the antimony element recovery rate during the smelting of antimony-containing steel involves the following steps: In the converter tapping process of smelting 09CrCuSb, the tapping rate is 60t and the tapping temperature is 1630℃. At the beginning of tapping, 90kg of antimony-oxygen powder mixture (containing 75kg of antimony-oxygen powder and 15kg of activated carbon powder) is added to the steel stream. The mixture is packaged in woven bags. After tapping, the composition of the molten steel is tested, and the molten steel is stirred at the argon blowing station for 3min and the composition of the molten steel is tested again.

[0043] The composition of the antimony oxide powder is as follows: Sb2O3: 96.2%; S: 0.35%; SiO2: 2.36%; CaO: 0.15%; FeO: 0.02%; Fe2O3: 0.58%; Al2O3: 0.13% and MgO: 0.21%.

[0044] The activated carbon composition is as follows: fixed carbon: 45.29%; ash: 5.26%; volatile matter: 45.45%; and H2O: 4.0%.

[0045] The antimony content in the molten steel after tapping was 0.098%, and the antimony content in the molten steel after argon blowing was 0.0985%, with an antimony element recovery rate of 98%.

[0046] The antimony-containing steel obtained according to the method described in this embodiment has an antimony content of 0.0985% and an antimony recovery rate of 98%.

[0047] Example 2:

[0048] A method for improving the antimony element recovery rate during the smelting of antimony-containing steel involves the following steps: In the converter tapping process of smelting 09CrCuSb, the tapping rate is 60t and the tapping temperature is 1630℃. At the beginning of tapping, 85kg of a mixture (containing 75kg of antimony oxygen powder and 10kg of activated carbon powder) is added to the steel stream. The mixture is packaged in burlap sacks. After tapping, the composition of the molten steel is tested, and the molten steel is stirred at the argon blowing station for 5min and the composition of the molten steel is tested again.

[0049] The composition of the antimony oxide powder is as follows: Sb2O3: 96.2%; S: 0.35%; SiO2: 2.36%; CaO: 0.15%; FeO: 0.02%; Fe2O3: 0.58%; Al2O3: 0.13% and MgO: 0.21%.

[0050] The activated carbon composition is as follows: fixed carbon: 59.73%; ash: 6.65%; and volatile matter: 33.62%.

[0051] The antimony content in the molten steel after tapping was 0.098%, and the antimony content in the molten steel after argon blowing was 0.099%, with an antimony element recovery rate of 98.5%. The standard for antimony content determination was "Chemical Analysis Methods for Iron and Steel and Alloys: Determination of Antimony Content by Carrier Precipitation-Molybdenum Blue Spectrophotometry" (GB / T 223.47-1994).

[0052] The antimony-containing steel obtained according to the method described in this embodiment has an antimony content of 0.099% and an antimony recovery rate of 98.5%.

[0053] Example 3:

[0054] A method for improving the antimony element recovery rate during the smelting of antimony-containing steel involves the following steps in the converter steelmaking process of 09CrCuSb, with a tapping rate of 60t and a tapping temperature of 1630℃. At the start of tapping, 90kg of steel (containing 75kg of antimony oxide powder and 15kg of activated carbon powder) is added to the molten steel stream. The mixture is packaged in woven bags. After tapping, the composition of the molten steel is tested, and the mixture is then purged at an argon blowing station at a flow rate of 200Nm³. 3 Stir the molten steel for 3 minutes per hour and test the composition of the molten steel.

[0055] The composition of the antimony oxide powder is as follows: Sb2O3: 96.2%; S: 0.35%; SiO2: 2.36%; CaO: 0.15%; FeO: 0.02%; Fe2O3: 0.58%; Al2O3: 0.13% and MgO: 0.21%.

[0056] The activated carbon composition is as follows: fixed carbon: 45.29%; ash: 5.26%; volatile matter: 45.45%; and H2O: 4.0%.

[0057] The antimony content in the molten steel after tapping was 0.0985%, and the antimony content in the molten steel after argon blowing was 0.0988%, with an antimony element recovery rate of 98.3%.

[0058] The antimony-containing steel obtained according to the method described in this embodiment has an antimony content of 0.0988% and an antimony recovery rate of 98.3%.

[0059] Example 4:

[0060] A method for improving the antimony element recovery rate during the smelting of antimony-containing steel involves the following steps in the converter steelmaking process of 09CrCuSb, with a tapping rate of 60t and a tapping temperature of 1630℃. At the start of tapping, 90kg of a mixture (containing 75kg of antimony oxide powder and 15kg of activated carbon) is added to the molten steel stream. The mixture is packaged in woven bags. After tapping, the composition of the molten steel is tested, and argon is blown into the stream at a flow rate of 300Nm³. 3 Stir the molten steel for 5 minutes per hour and test the composition of the molten steel.

[0061] The composition of the antimony oxide powder is as follows: Sb2O3: 96.2%; S: 0.35%; SiO2: 2.36%; CaO: 0.15%; FeO: 0.02%; Fe2O3: 0.58%; Al2O3: 0.13% and MgO: 0.21%.

[0062] The activated carbon composition is as follows: fixed carbon: 45.29%; ash: 5.26%; volatile matter: 45.45%; and H2O: 4.0%.

[0063] The antimony content in the molten steel after tapping was 0.0980%, and the antimony content in the molten steel after argon blowing was 0.0995%, with an antimony element recovery rate of 99%.

[0064] The antimony-containing steel obtained according to the method described in this embodiment has an antimony content of 0.094% and an antimony recovery rate of 99%.

[0065] Example 5:

[0066] A method for improving the antimony element recovery rate during the smelting of antimony-containing steel involves the following steps in the converter tapping process of 09CrCuSb steelmaking, with a tapping rate of 60t and a tapping temperature of 1600℃. Before tapping begins, 90kg of a mixture (containing 75kg of antimony oxide powder and 15kg of charcoal powder) is added to the molten steel stream. The mixture is packaged in woven bags. After tapping, the composition of the molten steel is tested, and the molten steel is then purged at an argon blowing station at a flow rate of 250Nm³. 3 Stir the molten steel for 4 minutes per hour and test the composition of the molten steel.

[0067] The composition of the antimony oxide powder is as follows: Sb2O3: 96.2%; S: 0.35%; SiO2: 2.36%; CaO: 0.15%; FeO: 0.02%; Fe2O3: 0.58%; Al2O3: 0.13% and MgO: 0.21%.

[0068] The composition of the charcoal powder is as follows: fixed carbon: 59.73%; ash: 6.65%; volatile matter: 33.62%. The antimony content in the molten steel after tapping is 0.097%, and the antimony content in the molten steel after argon blowing is 0.099%, with an antimony element recovery rate of 98.5%.

[0069] The antimony-containing steel obtained according to the method described in this embodiment has an antimony content of 0.099% and an antimony recovery rate of 98.5%.

[0070] Example 6:

[0071] A method for improving the antimony element recovery rate during the smelting of antimony-containing steel involves the following steps in the converter steelmaking process of 09CrCuSb, with a tapping rate of 60t and a tapping temperature of 1630℃. At the start of tapping, 195kg of a mixture (containing 150kg of antimony oxide powder and 45kg of activated carbon) is added to the molten steel stream. The mixture is packaged in woven bags. After tapping, the composition of the molten steel is tested, and argon is blown into the stream at a flow rate of 300Nm³. 3 Stir the molten steel for 5 minutes per hour and test the composition of the molten steel.

[0072] The composition of the antimony oxide powder is as follows: Sb2O3: 96.2%; S: 0.35%; SiO2: 2.36%; CaO: 0.15%; FeO: 0.02%; Fe2O3: 0.58%; Al2O3: 0.13% and MgO: 0.21%.

[0073] The activated carbon composition is as follows: fixed carbon: 45.29%; ash: 5.26%; volatile matter: 45.45%; and H2O: 4.0%.

[0074] The antimony content in the molten steel after tapping was 0.19%, and the antimony content in the molten steel after argon blowing was 0.20%, with an antimony element recovery rate of 99.5%.

[0075] The antimony-containing steel obtained according to the method described in this embodiment has an antimony content of 0.20% and an antimony recovery rate of 99.5%.

[0076] Comparative Example 1:

[0077] The only difference between this comparative example and Example 4 is that 60 kg of antimony ingots (antimony content of 99.9%) are added to the steel stream at the beginning of tapping.

[0078] The antimony content in the molten steel after tapping was 0.085%, and the antimony content in the molten steel after argon blowing was also 0.085%, with an antimony element recovery rate of 85.1%.

[0079] Comparative Example 2:

[0080] The only difference between this comparative example and Example 4 is that: a method for improving the antimony element recovery rate during the smelting of antimony-containing steel, in the converter steelmaking process of smelting 09CrCuSb, the steel output is 60t, the steel output temperature is 1630℃, and at the beginning of steelmaking, 90kg of mixture (containing 75kg of antimony oxygen powder and 15kg of activated carbon) is added to the steel stream. The mixture is packaged in a steel packaging can. After steelmaking is completed, the composition of the molten steel is tested, and argon is blown at a flow rate of 300Nm at the argon blowing station.3 Stir the molten steel for 5 minutes per hour and test the composition of the molten steel.

[0081] The antimony content in the molten steel after tapping was 0.087%, and the antimony content in the molten steel after argon blowing was 0.088%, with an antimony element recovery rate of 87.6%.

[0082] It should be understood that, in order to simplify this disclosure and aid in understanding one or more of the various aspects of the invention, features of the invention are sometimes grouped together in a single embodiment or description thereof in the above description of exemplary embodiments of the invention. However, this method of disclosure should not be interpreted as reflecting an intention that the claimed invention requires more features than expressly recited in each claim. Rather, as reflected in the claims, inventive aspects lie in fewer than all the features of the foregoingly disclosed embodiments. Therefore, the claims following the detailed description are hereby expressly incorporated into that detailed description, wherein each claim itself is a separate embodiment of the invention.

[0083] Although the invention has been described with reference to a limited number of embodiments, those skilled in the art will understand from the foregoing description that other embodiments are conceivable within the scope of the invention described herein. Furthermore, it should be noted that the language used in this specification has been chosen primarily for readability and instructional purposes, and not for the purpose of interpreting or limiting the subject matter of the invention. Therefore, many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the appended claims. The disclosure of the invention is illustrative and not restrictive, and the scope of the invention is defined by the appended claims.

[0084] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method of improving the recovery of antimony in the smelting of antimony bearing steel, characterised in that, Includes the following steps: S01, Preparation of antimony-oxygen powder mixture: Mix antimony-oxygen powder and rapid reducing agent in a mass ratio of 1:(0.13~0.3) to obtain a mixture, and put the mixture into a reaction bag, with the weight of the mixture in each reaction bag being 5kg~30kg; Before tapping, an antimony-oxygen powder mixture prepared from SO1 is added to the ladle at a rate of 0.14-0.32% of the tapping amount; or at the start of tapping, an antimony-oxygen powder mixture prepared from SO1 is added to the steel stream at a rate of 0.14-0.32% of the tapping amount. After tapping, the antimony content in the molten steel is detected, and the molten steel is stirred at the argon blowing station for 3-5 minutes and the antimony content in the molten steel is detected again to obtain antimony-containing molten steel. Wherein, the fast reducing agent is activated carbon powder or charcoal powder, the tapping is converter or electric furnace tapping, the tapping temperature is 1600~1630℃; the argon flow rate of the argon blowing station stirring is 200~300 Nm 3 / h.

2. The method of claim 1, wherein, The antimony oxide powder comprises the following components by weight percentage: Sb₂O₃: 96.2%; S: 0.35%; SiO2: 2.36%; CaO: 0.15%; FeO: 0.02%; Fe2O3: 0.58%; Al2O3: 0.13% and MgO: 0.21%.

3. The method of claim 1, wherein, Activated carbon powder comprises the following components by weight percentage: fixed carbon: 45.29~59.73%; ash: 5.26~6.65%; volatile matter: 33.62~45.45%; and H2O: 0~4.0%.

4. The method of claim 1, wherein, The equipment used to mix the antimony oxide powder and the rapid reducing agent is a powder mixer.

5. The method of claim 1, wherein, The reaction bags used are made of canvas, plastic, or linen.

6. Antimony-containing steel obtained by the method according to any one of claims 1 to 5.

7. The antimony-containing steel according to claim 6 is a steel grade containing 0.0985% to 0.20% antimony.

Citation Information

Patent Citations

  • Antimony wire for RH refining and adding method thereof

    CN105950829A

  • Adding method of antimony in smelting process of antimony-containing steel

    CN107177772A

  • Antimony-containing weathering steel and smelting method and application thereof

    CN111519085A

  • Steelmaking method of microalloy steel with added vanadium nitride alloy in steel

    CN102220454A

  • Smelting method for low-temperature antimony reduction through antimony oxide

    CN105695742A