A method for measuring gas adsorption based on applied electric field
By measuring the resistance change of gas-sensitive materials in an electric field environment, the problem of measuring the adsorption performance of gas-sensitive materials is solved, the detection and analysis of the characteristic decomposition components in SF6 insulation equipment is realized, and the safe operation of the power system is guaranteed.
Patent Information
- Application Number
- CN202310559577.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-05-17
AI Technical Summary
The existing technology is difficult to effectively measure the gas adsorption performance of gas-sensitive materials in an electric field environment, especially in the detection and analysis of characteristic decomposition components in SF6 insulation equipment.
A gas adsorption measurement method based on an applied electric field is used. The gas-sensitive material is coated on an acrylic plate, and a spiral micrometer is used to adjust the electrode spacing and applied voltage, and the resistance change of the material is measured to evaluate its adsorption performance.
It realizes the convenient measurement of gas-sensitive materials in an electric field environment and can analyze the decomposition components of sulfur hexafluoride, which provides an effective means to evaluate the operating status of insulation equipment and ensure the safety of power systems.
Smart Images

Figure CN116593534B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of gas adsorption, and in particular to a method for measuring gas adsorption based on an external electric field. Background Art
[0002] Gas-sensitive semiconductors, as a device for detecting gas composition and concentration, are widely used in the detection of various flammable, explosive or harmful gases in factories, workshops and mines, and in the detection of flammable gas leaks in households, so as to achieve the purpose of fire prevention, explosion prevention and poisoning prevention to ensure the safety of life and property. As the core of the sensor, the gas-sensitive material determines the detection and performance of the sensor. The performance of the gas-sensitive material will change with the change of the environment. However, it is currently more troublesome to measure the adsorption performance of gas in an electric field environment using gas-sensitive materials.
[0003] Insulation defects are inevitable inside SF6 electrical insulation equipment that has been in operation for a long time, which can cause local discharge, local overheating and other faults, leading to the decomposition of SF6 gas and the generation of stable characteristic decomposition components, including H2S, SO2, SOF2 and SO2F2, under the promotion of micro-H2O and micro-O2. These decomposition components will weaken the insulation performance of SF6, deteriorate the insulation state of the equipment, and pose a threat to the safe operation of the power system. Studies have shown that the type and severity of failure of SF6 insulation equipment are closely related to the type and content of its characteristic decomposition components. Therefore, online detection of SF6 decomposition components is an effective measure to evaluate the operating status of insulation equipment and ensure the stability and safety of the power system. Summary of the invention
[0004] The present invention provides a method for measuring gas adsorption based on an external electric field, which can effectively solve the problem in the above-mentioned background technology that it is relatively troublesome to measure the adsorption performance of gas using gas-sensitive materials in an electric field environment.
[0005] To achieve the above object, the present invention provides the following technical solution: a method for measuring gas adsorption based on an applied electric field, comprising the following steps:
[0006] S1. Evenly coat the gas-sensitive material to be tested on the acrylic plate, and place it on the annular groove plate of the experimental chamber 1 after drying;
[0007] S2. Open the gas cylinder and deliver the gas from the air hole to the acrylic plate. Control the gas flow rate to fill the experimental cavity with gas.
[0008] S3, calculate the electric field strength E to be applied, adjust the distance between the two plate electrodes by means of a screw micrometer, and record it;
[0009] S4, applying voltage and recording;
[0010] S5. Read the material resistance value R in the measuring circuit and record it.
[0011] According to the above technical solution, in S1, the gas-sensitive material is coated on the metal wire and the metal sheet, and the external resistance measuring device is connected to the coating material through a flying wire to measure the resistance change of the gas-sensitive material in the experimental stage;
[0012] The acrylic plate is designed with both front and back sides, and the acrylic plate is arranged between the two pole plates.
[0013] According to the above technical solution, in the S2, the gas is blue, and the gas is SO2 / SO2F2 / H2S / SOF2 / CS2 / CO with SF6 as the standard gas;
[0014] According to the above technical solution, in S3, screw micrometers are set at both ends of the experimental cavity to measure the screw-in distance of the two flat electrodes and calculate the distance between the two plates;
[0015] The screw-in mechanism of the flat electrode adopts a cylinder design.
[0016] According to the above technical solution, in S3, E=U / d, U is the applied voltage, d is the distance between the two plate electrodes, d is adjusted by a screw micrometer, and U is adjusted by a DC or AC power supply.
[0017] According to the above technical solution, in S4, voltage access positions are provided at both ends of the experimental cavity, and the access positions are insulated from the screw micrometer positions.
[0018] According to the above technical solution, the experimental cavity includes a cylindrical cavity, an air hole, an aviation plug and an annular groove plate;
[0019] Two air holes are arranged on the outside of the cylindrical cavity, one of which is an air inlet hole connected to the gas cylinder, and the other is an air outlet hole connected to the gas recovery device.
[0020] According to the above technical solution, in S3, two flat electrodes are arranged at the inner top and bottom of the cylindrical cavity, a metal rod is connected to the middle of the flat electrode, and an upper brush and a lower brush are installed at the top and bottom of the cylindrical cavity;
[0021] The upper brush and the lower brush are both connected to the power supply;
[0022] Two flat electrodes, two metal rods, an upper brush and a lower brush form an external electric field structure;
[0023] The top and bottom of the cylindrical cavity are both equipped with cylinders, a micrometer screw is installed inside the cylinder, and an insulating block is installed between the micrometer screw and the cylinder.
[0024] According to the above technical solution, a coating groove is opened in the middle of the acrylic plate, a metal sheet is arranged inside the coating groove, a metal wire is arranged inside the coating groove, and flying wire interfaces are arranged at both ends of the coating groove;
[0025] The acrylic plate, the coating tank, the metal sheet, the metal wire, and the flying wire interface constitute the material coating structure.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The gas-sensitive material is coated on an acrylic plate, the acrylic plate is placed between two flat electrodes, the distance between the two flat electrodes is adjusted by a screw micrometer and a cylinder, thereby adjusting the surrounding electric field. After the gas is introduced, the resistance of the gas-sensitive material is measured, and the gas adsorption performance of the gas-sensitive material is measured according to the change in resistance value. The adsorption of the gas-sensitive material under power-on can be measured through a simple structure and operation, which is convenient for the subsequent selection and research of the material.
[0028] The present invention can analyze the decomposition components of sulfur hexafluoride, and the electric field strength can be calculated through data such as voltage and plate spacing, so as to read the material resistance value, provide a reference for portable monitoring of sulfur hexafluoride gas, and provide sufficient guarantee for evaluating the operating status of insulating equipment and ensuring the safe and stable operation of the power system. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0030] Figure 1 It is a measurement step diagram of the present invention;
[0031] Figure 2 is a diagram of the overall measuring device of the present invention;
[0032] Figure 3 It is a schematic diagram of the internal structure of the cylindrical cavity of the present invention;
[0033] Figure 4 It is a structural schematic diagram of the upper micrometer screw of the present invention;
[0034] Figure 5 It is a structural schematic diagram of the screw micrometer of the present invention;
[0035] Figure 6 It is a schematic diagram of the material coating structure of the present invention;
[0036] Figure 7 It is a structural block diagram of the measuring device of the present invention;
[0037] Explanation of the markings in the figure: 1, experimental cavity; 101, cylindrical cavity; 102, air hole; 103, aviation plug; 104, annular groove plate;
[0038] 2. External electric field structure; 201. upper plate electrode; 202. upper metal rod; 203. upper brush; 204. lower plate electrode; 205. lower metal rod; 206. lower brush;
[0039] 3. Screw-in adjustment structure; 301. Upper cylinder; 302. Upper micrometer screw; 303. Upper insulating block; 304. Lower cylinder; 305. Lower micrometer screw; 306. Lower insulating block;
[0040] 4. Material coating structure; 401. Acrylic plate; 402. Coating tank; 403. Metal sheet; 404. Metal wire; 405. Flying wire interface. DETAILED DESCRIPTION
[0041] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0042] Example: Figure 1-7 As shown, the present invention provides a technical solution, a method for measuring gas adsorption based on an external electric field, comprising the following steps:
[0043] S1, evenly coating the gas-sensitive material to be detected on the acrylic plate 401, and placing it on the annular groove plate 104 of the experimental chamber 1 after drying;
[0044] S2, open the gas cylinder, deliver the gas from the gas hole 102 to the position of the acrylic plate 401, control the gas flow rate, and fill the experimental cavity 1 with gas;
[0045] S3, calculate the electric field strength E to be applied, adjust the distance between the two plate electrodes by means of a screw micrometer, and record it;
[0046] S4, applying voltage and recording;
[0047] S5. Read the material resistance value R in the measuring circuit and record it.
[0048] According to the above technical solution, in S1, the gas-sensitive material is coated on the metal wire 404 and the metal sheet 403, and the external resistance measuring device is connected to the coating material through a flying wire to measure the resistance change of the gas-sensitive material in the experimental stage;
[0049] The acrylic plate 401 is designed with both front and back sides, and the acrylic plate 401 is arranged between the two electrode plates.
[0050] According to the above technical solution, in S2, the gas is blue, and the gas is SO2 / SO2F2 / H2S / SOF2 / CS2 / CO with SF6 as the standard gas;
[0051] According to the above technical solution, in S3, screw micrometers are set at both ends of the experimental cavity 1 to measure the screw-in distance of the two flat electrodes and calculate the distance between the two plates;
[0052] The screw-in mechanism of the flat electrode adopts a cylinder design.
[0053] According to the above technical solution, in S3, E=U / d, U is the applied voltage, d is the distance between the two plate electrodes, d is adjusted by a screw micrometer, and U is adjusted by a DC or AC power supply.
[0054] According to the above technical solution, in S4, voltage access positions are provided at both ends of the experimental cavity 1, and the access positions are insulated from the screw micrometer positions.
[0055] According to the above technical solution, the experimental chamber 1 includes a cylindrical chamber 101, an air hole 102, an aviation plug 103 and an annular groove plate 104;
[0056] Two air holes 102 are provided on the outside of the cylindrical cavity 101 , one of the air holes 102 is an air inlet connected to the gas cylinder, and the other air hole 102 is an air outlet connected to the gas recovery device.
[0057] According to the above technical solution, in S3, two flat electrodes are arranged at the inner top and bottom of the cylindrical cavity 101, a metal rod is connected to the middle of the flat electrode, and an upper brush 203 and a lower brush 206 are installed at the top and bottom of the cylindrical cavity 101;
[0058] The upper brush 203 and the lower brush 206 are both connected to a power source;
[0059] Two flat electrodes, two metal rods, an upper brush 203 and a lower brush 206 form an external electric field structure 2;
[0060] Cylinders are installed at the top and bottom of the cylindrical cavity 101, a micrometer screw is installed inside the cylinder, and an insulating block is installed between the micrometer screw and the cylinder.
[0061] According to the above technical solution, a coating groove 402 is opened in the middle of the acrylic plate 401, a metal sheet 403 is arranged inside the coating groove 402, a metal wire 404 is arranged inside the coating groove 402, and flying wire interfaces 405 are provided at both ends of the coating groove 402;
[0062] The acrylic plate 401 , the coating tank 402 , the metal sheet 403 , the metal wire 404 , and the flying lead interface 405 constitute a material coating structure 4 .
[0063] The two flat plate electrodes are an upper flat plate electrode 201 and a lower flat plate electrode 204. The upper flat plate electrode 201 is connected to the top with an upper metal rod 202, which is connected to an upper brush 203. The lower flat plate electrode 204 is installed with a lower metal rod 205 at the bottom, which is connected to a lower brush 206.
[0064] The cylindrical cavity 101 is provided with a screw-in adjustment structure 3 at both ends, and the screw-in adjustment structure 3 includes an upper cylinder 301 connected to the upper metal rod 202, an upper screw micrometer 302 is connected to the top of the upper cylinder 301, and a lower cylinder 304 connected to the lower metal rod 205, and a lower screw micrometer 305 is connected to the bottom of the lower cylinder 304;
[0065] An upper insulating block 303 is provided at the connection position between the upper cylinder 301 and the upper micrometer screw 302 , and a lower insulating block 306 is provided at the connection position between the lower cylinder 304 and the lower micrometer screw 305 .
[0066] Finally, it should be noted that the above description is only a preferred example of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for measuring gas adsorption based on an applied electric field, characterized in that: The method comprises the following steps: S1. Evenly coat the gas-sensitive material to be detected on the acrylic plate (401), dry it, and place it on the annular groove plate (104) of the experimental cavity (1); S2, open the gas cylinder, deliver the gas from the gas hole (102) to the position of the acrylic plate (401), and control the gas flow rate to fill the experimental cavity (1) with gas; S3, calculate the electric field strength E to be applied, adjust the distance between the two plate electrodes by means of a screw micrometer, and record it; S4, applying voltage and recording; S5. Read the material resistance value R in the measuring circuit and record it.
2. The method for measuring gas adsorption based on an applied electric field according to claim 1, characterized in that: In S1, the gas-sensitive material is coated on the metal wire (404) and the metal sheet (403), and the external resistance measuring device is connected to the coating material through a flying wire to measure the resistance change of the gas-sensitive material in the experimental stage; The acrylic plate (401) is designed with two sides, and is arranged between the two electrode plates for coating the gas-sensitive material. The gas-sensitive material is coated on both sides of the metal sheet to detect whether the adsorption degree of the material is modulated by the direction of the electric field.
3. The method for measuring gas adsorption based on an applied electric field according to claim 1, characterized in that: In the S2, the gas selected is SO2 / SO2F2 / H2S / SOF2 / CS2 / CO with SF6 as the standard gas.
4. The method for measuring gas adsorption based on an applied electric field according to claim 1, characterized in that: In S3, screw micrometers are provided at both ends of the experimental chamber (1) to measure the screw-in distance of the two flat electrodes and calculate the distance between the two plates; The screw-in mechanism of the flat electrode adopts a cylinder design.
5. The method for measuring gas adsorption based on an applied electric field according to claim 1, characterized in that: In S3, E=U / d, U is the applied voltage, d is the distance between the two plate electrodes, d is adjusted by a micrometer, and U is adjusted by a DC or AC power supply.
6. The method for measuring gas adsorption based on an applied electric field according to claim 1, characterized in that: In the above S4, voltage access positions are provided at both ends of the experimental cavity (1), and the access positions are insulated from the screw micrometer positions.
7. The method for measuring gas adsorption based on an applied electric field according to claim 1, characterized in that: The experimental chamber (1) comprises a cylindrical chamber (101), an air hole (102), an aviation plug (103) and an annular groove plate (104); Two air holes (102) are provided on the outside of the cylindrical cavity (101), one air hole (102) is an air inlet hole connected to a gas cylinder, and the other air hole (102) is an air outlet hole connected to a gas recovery device.
8. The method for measuring gas adsorption based on an applied electric field according to claim 1, characterized in that: In S3, two flat electrodes are arranged at the inner top and bottom of the cylindrical cavity (101), a metal rod is connected to the middle of the flat electrode, and an upper brush (203) and a lower brush (206) are installed at the top and bottom of the cylindrical cavity (101); The upper brush (203) and the lower brush (206) are both connected to a power source; Two flat electrodes, two metal rods, an upper brush (203) and a lower brush (206) form an external electric field structure (2); A cylinder is installed at the top and bottom of the cylindrical cavity (101), a micrometer screw is installed inside the cylinder, and an insulating block is installed between the micrometer screw and the cylinder.
9. The method for measuring gas adsorption based on an applied electric field according to claim 1, characterized in that: A coating groove (402) is provided in the middle of the acrylic plate (401), a metal sheet (403) is arranged inside the coating groove (402), a metal wire (404) is arranged inside the coating groove (402), and flying wire interfaces (405) are provided at both ends of the coating groove (402); The acrylic plate (401), the coating tank (402), the metal sheet (403), the metal wire (404), and the flying wire interface (405) constitute a material coating structure (4).
Citation Information
Patent Citations
SO2F2 gas sensor
CN112798661A
Resistance-type gas-sensitive performance testing device
CN215179860U