Cross-linked polyarylene sulfide, composition and method for producing molded article
Through the compression molding, porosity measurement, crushing and whole-particle treatment of uncrosslinked polyarylene sulfide, the melt viscosity deviation and quality stability problems in the manufacturing of crosslinked polyarylene sulfide are solved, and a more homogeneous and stable Crosslinking treatment.
Patent Information
- Application Number
- CN202180085175.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-12-24
- Filing Date
- 2021-08-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-08-26
AI Technical Summary
In the existing crosslinked polyarylene sulfide production method, there are problems of melt viscosity deviation between batches and poor quality stability.
By compressing and molding the uncrosslinked polyarylene sulfide, measuring porosity, pulverizing and whole particles, granulated substances with specific porosity are obtained for oxidative cross-linking, ensuring the consistency of melt viscosity and quality stability between batches.
It effectively suppresses the melt viscosity deviation between batches, improves the quality stability of cross-linked polyarylene sulfide, and achieves a more homogeneous and stable cross-linking treatment.
Smart Images

Figure BDA0004289204470000141 
Figure BDA0004289204470000151
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing a cross-linked polyarylene sulfide, a method for producing a composition containing the cross-linked polyarylene sulfide, and a method for producing a molded article obtained by melt-molding the composition. Background Art
[0002] The substance called crosslinked PAS among polyarylene sulfide (hereinafter also referred to as PAS) represented by polyphenylene sulfide (hereinafter also referred to as PPS) used in engineering plastics and the like is obtained by further oxidative crosslinking of granular PAS produced by solution polymerization until the desired melt flow rate (hereinafter also referred to as MFR, ASTM D-1238-74; measured at 316°C, load 5kg, unit g / 10min). The oxidative crosslinking is usually carried out by heating PAS in a solid phase state below the melting point or heating it to a molten state above the melting point in an oxygen-containing atmosphere.
[0003] As methods for oxidative crosslinking, there are the following methods: a method using a forced heated air circulation dryer (Patent Document 1), a method using a container-fixed heating mixing device with a double helical stirring blade (Patent Document 2), a method using a fluidized bed (Patent Document 3), a method using a fluidized bed with a cyclone separator, or a method using a fluidized bed with a built-in bag filter (Patent Document 4), etc.
[0004] The common point of the above methods is that PAS is handled in powder form, which leads to heat transfer obstruction caused by the formation of an adhesion layer on the inner wall of the reactor, extension of the crosslinking time, uneven product properties, and further dust generation during input and withdrawal, resulting in reduced recovery rate, productivity, and deterioration of workability. Therefore, a method for producing crosslinked PAS (also called a conventional method) is proposed, which compresses and granulates powdered PAS with a bulk density of 0.4 g / cm 3 The above-mentioned non-crosslinked PAS granules are heated in an oxygen-containing atmosphere to be oxidatively crosslinked (Patent Document 5).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: U.S. Patent No. 3,354,129
[0008] Patent Document 2: U.S. Patent No. 3,717,620
[0009] Patent Document 3: U.S. Patent No. 3,793,256
[0010] Patent Document 4: Japanese Patent Application Laid-Open No. 62-177027
[0011] Patent Document 5: Japanese Patent Application Laid-Open No. 4-248841 Summary of the invention
[0012] Problem that the invention aims to solve
[0013] However, it has been found that the above-mentioned conventional methods have large variations in melt viscosity between batches and that there is room for improvement in quality stability.
[0014] Therefore, the problem to be solved by the present invention is to provide a method for producing a cross-linked PAS having excellent quality stability while suppressing the variation of melt viscosity between batches. In addition, a method for producing a composition containing the cross-linked PAS and a method for producing a molded product obtained by melt-molding the composition are provided.
[0015] Solutions for solving problems
[0016] The inventors of the present application have conducted various studies and found that the above-mentioned existing method is a method of oxidatively crosslinking an uncrosslinked granulated product whose bulk density is adjusted to a specific range. Therefore, even if the bulk density is the same, the fluctuation of the space generated between the particles when stacked according to the difference in the particle shape of the granulated product is sometimes greatly different, and the result illustrates that deviations may occur in the melt viscosity between batches. Therefore, in order to meet more stringent market demands, the inventors of the present invention have conducted in-depth research, and the results show that it is useful to consider the presence of closed pores in the uncrosslinked granulated product (flakes). For this reason, after measuring the pores (void) present in the interior of the aforementioned compression molded product by porosity (void rate) according to measurement means such as X-ray CT scanning, the granulated product prepared by the compression molded product in a specific range is oxidatively crosslinked, so that a more homogeneous and stable crosslinking treatment can be performed, thereby suppressing the deviation of the melt viscosity between batches, and obtaining a crosslinked PAS with excellent quality stability, so as to solve the present invention.
[0017] That is, the present invention provides a method for producing a cross-linked polyarylene sulfide, characterized by comprising the following steps: a step of compression-molding powdered uncross-linked polyarylene sulfide to obtain a compression-molded product; a step of measuring the porosity of the compression-molded product; a step of crushing the compression-molded product within a specific porosity range to obtain a crushed product; a step of granulating the crushed product to obtain a granulated product; and a step of oxidatively cross-linking the granulated product obtained in the previous step.
[0018] The present invention further provides a method for producing a resin composition, comprising the steps of: producing a cross-linked polyarylene sulfide by the above-mentioned production method; and melt-kneading the obtained cross-linked polyarylene sulfide with other components.
[0019] The present invention further provides a method for producing a molded article, comprising the steps of: producing a resin composition by the above-mentioned production method; and melt-molding the obtained resin composition.
[0020] Effects of the Invention
[0021] According to the present invention, a method for producing a cross-linked PAS having excellent quality stability and suppressing the variation of melt viscosity between batches can be provided. In addition, according to the present invention, a method for producing a composition containing the cross-linked PAS and a method for producing a molded product obtained by melt-molding the composition can be provided. DETAILED DESCRIPTION
[0022] The method for producing a cross-linked polyarylene sulfide of the present invention is characterized by comprising the following steps:
[0023] The invention relates to a process of compressing powdered uncrosslinked polyarylene sulfide to obtain a compression molded product; a process of measuring the porosity of the compression molded product; a process of crushing the compression molded product within a specific porosity range to obtain a crushed product; a process of granulating the crushed product to obtain a granulated product; and a process of oxidatively crosslinking the granulated product obtained in the previous process.
[0024] First, powdery uncrosslinked PAS is synthesized, for example, by reacting at least one polyhalogenated aromatic compound with at least one thioetherification agent under appropriate polymerization conditions in an organic polar solvent such as N-methyl-2-pyrrolidone.
[0025] The polyhalogenated aromatic compound used in the present invention is, for example, a halogenated aromatic compound having two or more halogen atoms directly bonded to an aromatic ring, and specifically, dihalogenated aromatic compounds such as p-dichlorobenzene, o-dichlorobenzene, m-dichlorobenzene, trichlorobenzene, tetrachlorobenzene, dibromobenzene, diiodobenzene, tribromobenzene, dibromonaphthalene, triiodobenzene, dichlorodiphenylbenzene, dibromodiphenylbenzene, dichlorobenzophenone, dibromobenzophenone, dichlorodiphenyl ether, dibromodiphenyl ether, dichlorodiphenyl sulfide, dibromodiphenyl sulfide, dichlorobiphenyl, dibromobiphenyl, and mixtures thereof can be mentioned, and these compounds can be block copolymerized. Among them, dihalogenated benzenes are preferred, and p-dichlorobenzene containing 80 mol% or more is particularly preferred.
[0026] In addition, in order to increase the viscosity of the polyarylene sulfide by forming a branched structure, a polyhalogenated aromatic compound having three or more halogen substituents in one molecule may be used as a branching agent as desired. Examples of such polyhalogenated aromatic compounds include 1,2,4-trichlorobenzene, 1,3,5-trichlorobenzene, and 1,4,6-trichloronaphthalene.
[0027] Furthermore, polyhalogenated aromatic compounds having a functional group having active hydrogen such as an amino group, a mercapto group, or a hydroxyl group can be cited. Specifically, dihalogenated anilines such as 2,6-dichloroaniline, 2,5-dichloroaniline, 2,4-dichloroaniline, and 2,3-dichloroaniline; trihalogenated anilines such as 2,3,4-trichloroaniline, 2,3,5-trichloroaniline, 2,4,6-trichloroaniline, and 3,4,5-trichloroaniline; dihalogenated aminodiphenyl ethers such as 2,2'-diamino-4,4'-dichlorodiphenyl ether and 2,4'-diamino-2',4-dichlorodiphenyl ether; and mixtures thereof in which the amino group is substituted with a mercapto group or a hydroxyl group.
[0028] In addition, active hydrogen-containing polyhalogenated aromatic compounds in which hydrogen atoms bonded to carbon atoms forming aromatic rings in these active hydrogen-containing polyhalogenated aromatic compounds are substituted with other inactive groups, for example, hydrocarbon groups such as alkyl groups, may also be used.
[0029] Among these various active hydrogen-containing polyhalogenated aromatic compounds, active hydrogen-containing dihalogenated aromatic compounds are preferred, and dichloroaniline is particularly preferred.
[0030] Examples of the polyhalogenated aromatic compound having a nitro group include mono- or dihalogenated nitrobenzenes such as 2,4-dinitrochlorobenzene and 2,5-dichloronitrobenzene; dihalogenated nitrodiphenyl ethers such as 2-nitro-4,4'-dichlorodiphenyl ether; dihalogenated nitrodiphenyl sulfones such as 3,3'-dinitro-4,4'-dichlorodiphenyl sulfone; mono- or dihalogenated nitropyridines such as 2,5-dichloro-3-nitropyridine and 2-chloro-3,5-dinitropyridine; or various dihalogenated nitronaphthalenes.
[0031] The thioetherification agent used in the present invention includes alkali metal sulfides such as lithium sulfide, sodium sulfide, rubidium sulfide, cesium sulfide, and mixtures thereof. The alkali metal sulfides can be used in the form of hydrates, aqueous mixtures, or anhydrides. In addition, the alkali metal sulfide can also be derived by reacting an alkali metal hydrosulfide with an alkali metal hydroxide.
[0032] It should be noted that a small amount of alkali metal hydroxide may be added in order to react with the alkali metal hydrosulfide and alkali metal thiosulfate which are usually present in trace amounts in the alkali metal sulfide.
[0033] Examples of the organic polar solvent used in the present invention include amides such as N-methyl-2-pyrrolidone, formamide, acetamide, N-methylformamide, and N,N-dimethylacetamide; amide ureas such as N-methyl-ε-caprolactam, ε-caprolactam, hexamethylphosphoramide, tetramethylurea, N-dimethylpropyleneurea, and 1,3-dimethyl-2-imidazolidinone acid; and lactams; sulfolanes such as sulfolane and dimethylsulfolane; nitriles such as benzonitrile; ketones such as methyl phenyl ketone, and mixtures thereof.
[0034] In the presence of these organic polar solvents, the polymerization conditions of the above-mentioned thioetherification agent and the polyhalogenated aromatic compound are usually as follows: the temperature is 200-330°C, and the pressure is in the range of substantially keeping the polymerization solvent and the polyhalogenated aromatic compound as the polymerization monomer in the liquid phase, usually selected from the range of 0.1-20 MPa, preferably 0.1-2 MPa. The reaction time varies depending on the temperature and pressure, but is usually in the range of 10 minutes or 72 hours, preferably in the range of 1 hour or 48 hours.
[0035] The granular uncrosslinked PAS used in the present invention also includes the following methods: a method in which a polyhalogenated aromatic compound and an organic polar solvent are reacted while being continuously or intermittently added in the presence of a thioetherifying agent and an organic polar solvent; a method in which a polyhalogenated aromatic compound and an organic polar solvent are reacted while being continuously or intermittently added in the presence of a thioetherifying agent.
[0036] The particulate uncrosslinked PAS used in the present invention can be produced, for example, by further post-treating the PAS obtained by the above-mentioned polymerization method or a reaction mixture containing the PAS.
[0037] There are no particular restrictions on the post-treatment method of the reaction mixture containing PAS obtained by the above-mentioned polymerization method. For example, as a step for washing the by-products (inevitable components derived from the polymerization reaction of PAS) contained in the polymerization reaction product after polymerizing PAS (hereinafter also referred to as "washing step"), the following methods (1) to (6) can be exemplified.
[0038] Method (1): after the polymerization reaction is completed, first, the reaction mixture is directly or after adding an acid or a base, the solvent is distilled off under reduced pressure or normal pressure, then the solid matter after the solvent is distilled off is washed once or twice or more with water, a reaction solvent (or an organic solvent having an equivalent solubility for the low molecular weight polymer), acetone, methyl ethyl ketone, an alcohol or the like, further neutralized, washed with water and filtered, and a dispersion medium is added as needed to form a dispersion.
[0039] Method (2), after the polymerization reaction is completed, water, acetone, methyl ethyl ketone, alcohols, ethers, halogenated hydrocarbons, aromatic hydrocarbons, aliphatic hydrocarbons and other solvents (soluble in the polymerization solvent used and at least a poor solvent for PAS) are added to the reaction mixture as a precipitant to precipitate solid products such as PAS and inorganic salts, which are then washed and filtered, and a dispersion medium is added as needed to form a dispersion.
[0040] Method (3), after the polymerization reaction is completed, a reaction solvent (or an organic solvent having an equivalent solubility to the low molecular weight polymer) is added to the reaction mixture, stirred, and then filtered to remove the low molecular weight polymer, and then washed with water, acetone, methyl ethyl ketone, alcohol or other solvents once or twice or more, then neutralized, washed with water and filtered, and a dispersion medium is added as needed to form a dispersion.
[0041] Method (4): After the polymerization reaction is completed, water is added to the reaction mixture for washing and filtering. If necessary, an acid is added during the washing for acid treatment. Furthermore, if necessary, a dispersion medium is added to form a dispersion.
[0042] Method (5), after the polymerization reaction is completed, the reaction mixture is filtered, washed with a reaction solvent once or twice or more as needed, further washed with water and filtered, and a dispersion medium is added as needed to form a dispersion liquid.
[0043] Method (6), after the polymerization reaction is completed, the reaction mixture is desolvated to obtain a slurry containing PAS, the slurry containing PAS is further contacted with water and a solvent containing oxygen atoms having 1 to 10 carbon atoms, the PAS is formed into porous particles, the obtained porous particles are washed and filtered with carbon dioxide water, and a dispersion medium is added as needed to form a dispersion. The solvent containing oxygen atoms having 1 to 10 carbon atoms may be, for example, at least one selected from the group consisting of alcohols and ketones. It should be noted that alcohols (also referred to as alcohol solvents or alcohol solvents) include alcohols having 10 or less carbon atoms, such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, tert-butanol, ethylene glycol, propylene glycol, trimethylolpropane, benzyl alcohol, etc.; alcohols having 10 or less carbon atoms and containing an ether bond, such as 2-methoxyethanol, 2-ethoxyethanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, 3-methoxy-1-butanol, 2-isopropoxyethanol, etc.; alcohols having 10 or less carbon atoms and containing a ketone group, such as 3-hydroxy-2-butanone; and alcohols having 10 or less carbon atoms and containing an ester group, such as methyl hydroxyisobutyrate. In addition, ketones (also referred to as ketone solvents or ketone solvents) include acetone, methyl ethyl ketone, cyclohexanone, γ-butyl lactone, or N-methylpyrrolidone. In the present invention, the use of a monohydric alcohol having 10 or less carbon atoms is preferred because the residual carboxyl group-containing alkylamino compound can be effectively removed, and a monohydric alcohol having 3 or less carbon atoms is more preferred.
[0044] After the above post-treatments (1) to (6), the product may be dried to form a powder.
[0045] The melt viscosity of the powdered uncrosslinked PAS used in the present invention is not particularly limited. The melt viscosity (V6) measured at 300°C is preferably 1 [Pa·s] or more, more preferably 3 [Pa·s] or more, further preferably 5 [Pa·s] or more and preferably 800 [Pa·s] or less, more preferably 500 [Pa·s] or less, further preferably 200 [Pa·s] or less.
[0046] The non-Newtonian index of the powdery uncrosslinked PAS used in the present invention is not particularly limited, but is preferably within the range of 0.90 or more, more preferably 0.95 or more, and preferably 1.25 or less, more preferably 1.20 or less.
[0047] The melt viscosity (V6) measured at 300°C refers to the melt viscosity after holding the sample for 6 minutes at a temperature of 300°C and a load of 1.96 MPa using an orifice with an orifice length / orifice diameter ratio of 10 / 1. The non-Newtonian index (N value) is a value calculated by measuring the shear rate and shear stress using a capillary rheometer at 300°C and an orifice length (L) / orifice diameter (D) ratio of L / D=40, and using the following formula.
[0048] SR=K.SS N
[0049] [SR represents the shear rate (seconds) -1 ), SS represents shear stress (dyne / cm 2 ), and K represents a constant. ] The closer the N value is to 1, the closer the PAS structure is to a linear structure, and the higher the N value is, the more developed the cross-linking structure is.
[0050] The particle size of the powdered uncrosslinked PAS used in the present invention is not particularly limited, but the average particle size based on SEM observation is preferably in the range of 1 [μm] or more, more preferably 5 [μm] or more, further preferably 20 [μm] to preferably 500 [μm] or less, more preferably 400 [μm] or less, further preferably 300 [μm] or less.
[0051] The present invention comprises the steps of: a step of compression-molding the thus obtained powdery uncrosslinked polyarylene sulfide to obtain a compression-molded product; and a step of measuring the porosity of the compression-molded product.
[0052] Compression molding can include a method of mechanically compressing powdered uncrosslinked PAS in a non-molten state. Various methods can be used in the compression molding process without particular limitation. Specifically, from the perspective of the stability of the production of the compressed product, a method in which the powdered uncrosslinked PAS is pushed between two rollers rotating in a manner intermeshing with each other is particularly desirable, whereby the powdered uncrosslinked PAS is sandwiched therebetween, fed out and compressed at a high density to form a plate.
[0053] The method for measuring the porosity of the obtained compression molded product is not particularly limited, and for example, the method described in Examples can be used.
[0054] The present invention comprises the following step: a step of crushing the compression molded product within a specific porosity range to obtain a crushed product. That is, this step is a step of selecting the compression molded product within a specific porosity range measured in the previous step and crushing it to obtain a crushed product.
[0055] The range of specific porosity is not particularly limited. For example, from the viewpoint of suppressing the amount of fine powder, and from the viewpoint of efficiently promoting the cross-linking reaction and excellent productivity, the porosity can be selected to be preferably 0.10〔%〕or more, more preferably 0.30〔%〕or more, further preferably 0.50〔%〕or more, particularly preferably 0.60 or more, and most preferably 0.62 or more. The porosity can be selected to be preferably 10.00〔%〕or less, more preferably 5.00〔%〕or less, and further preferably 4.95〔%〕or less.
[0056] The step of obtaining the compression molded product, the step of measuring the porosity, and the step of obtaining the crushed product may be performed continuously. In this case, the steps may be performed while adjusting the porosity of the compression molded product.
[0057] The porosity of the compression molded product can be adjusted by adjusting the compression pressure during compression molding. As described in the above specific example, the porosity of the plate-shaped compression molded product can be adjusted by adjusting the interval between the two press rolls.
[0058] Specifically, various methods can be used in the method of crushing the compression molded product, and there are no particular limitations. Examples include the following methods: a roller crusher method in which at least two rollers are rotated in a manner that they interlock with each other, and the compression molded product is crushed mainly by compression force and partly by shear force; a shredder method in which a compression molded product is crushed while a rotor equipped with a cutter or the like is rotated; a pounding method in which a mortar-shaped impact rod is dropped and the compression molded product is crushed by its impact; a stone mortar method in which the compression molded product is crushed by the shear force generated when passing through the gap between the upper and lower grinding stones; etc. The shape of the crushed product is not particularly limited, and examples include amorphous scales, flakes, etc.
[0059] The present invention comprises a step of sizing the crushed product obtained in this way to obtain a granulated product.
[0060] Specifically, various methods can be used to size the crushed product without particular limitation, and examples thereof include a method of adjusting the crushed product to have physical pores of a suitable size and shape by passing the crushed product through a sieve, a filter, a punching metal, or the like.
[0061] When the powdered uncrosslinked PAS is compression-molded, pulverized, and sized, it is also possible to mix a partially crosslinked PAS as necessary.
[0062] The porosity of the granulated product thus obtained is the same as the porosity of the compression molded product before crushing.
[0063] As described above, in the present invention, by adjusting the porosity of the compression-molded product of uncrosslinked PAS for oxidative crosslinking, a crosslinked PAS having uniform voids and suppressed batch-to-batch variation and excellent quality stability is obtained regardless of the particle shape of the granulated product.
[0064] In addition, the shape of the granules may be amorphous from the viewpoint of being suitable for oxidative crosslinking and subsequent melt extrusion molding. The amorphous shape may be any shape such as granules, plates, pillows, needles, etc., and 20 granules are randomly selected from the two-dimensional images captured in the electronic photograph (magnification 10 times), and when the shortest dimension of each granule is regarded as the minor diameter and the equivalent circle diameter is regarded as the diameter, it is preferred that the minor diameter / diameter=0.5 or more.
[0065] The present invention includes a step of oxidatively crosslinking the granulated material thus obtained. Oxidative crosslinking is not particularly limited as long as it is a known method, and for example, the following method can be cited: the granulated material is heat-treated in an oxidative atmosphere such as air or oxygen-enriched air. The heating conditions are preferably in a temperature range of 180°C or more to 20°C lower than the melting point of PAS, from the viewpoint of the time required for the heat treatment and the good thermal stability of the PAS melted after the heat treatment. Among them, the melting point here refers to: the melting point measured using a differential scanning calorimeter (DSC device Pyris Diamond manufactured by PerkinElmer) in accordance with JIS K7121.
[0066] Regarding the oxygen concentration during heat treatment in an oxidizing atmosphere such as air or oxygen-enriched air, from the viewpoint of fast oxidation rate and ability to perform treatment in a short time, it can be preferably in the range of 5 volume % or more, more preferably in the range of 10 mass % or more, and from the viewpoint of suppressing the increase in the amount of free radical generation, suppressing the thickening during heat treatment, and achieving a good color tone, it can be preferably in the range of 30 volume % or less, more preferably in the range of 25 volume % or less.
[0067] The non-Newtonian index of the crosslinked PAS of the present invention obtained in this way is not particularly limited. For example, the non-Newtonian index may be preferably in the range of 1.26 or more, more preferably 1.30 or more, and further preferably 1.35 or more, and may be preferably in the range of 2.00 or less, more preferably 1.95 or less, and further preferably 1.90 or less.
[0068] In addition, the melt viscosity of the cross-linked PAS of the present invention is not particularly limited. For example, the melt viscosity (V6) measured at 300°C can be preferably in the range of 20 [Pa·s] or more, more preferably 100 [Pa·s] or more, and can be preferably in the range of 5000 [Pa·s] or less, more preferably 2000 [Pa·s] or less.
[0069] When the uncrosslinked PAS granules are oxidatively crosslinked, the shape thereof does not change much, and therefore the porosity, maximum particle size, and circularity are the same as those described above.
[0070] The crosslinked PAS of the present invention described in detail above can be processed into a molded product having excellent heat resistance, molding processability, dimensional stability, etc. by various melt processing methods such as injection molding, extrusion molding, compression molding, and blow molding.
[0071] In addition, the cross-linked PAS of the present invention can be used as a PAS resin composition containing various filling materials in order to further improve the performances such as strength, heat resistance and dimensional stability. As filling materials, there is no particular limitation, for example, fibrous filling materials, inorganic filling materials, etc. can be cited. As fibrous filling materials, fibers such as glass fiber, carbon fiber, silane glass fiber, ceramic fiber, aramid fiber, metal fiber, potassium titanate, silicon carbide, calcium sulfate, calcium silicate, natural fibers such as wollastonite, etc. can be used. Moreover, as inorganic filling materials, barium sulfate, calcium sulfate, clay, pyrophyllite, bentonite, sericite, zeolite, mica, mica, talc, attapulgite, ferrite, calcium silicate, calcium carbonate, magnesium carbonate, glass beads, etc. can be used. In addition, various additives such as mold release agent, colorant, heat stabilizer, ultraviolet stabilizer, foaming agent, rust inhibitor, flame retardant, lubricant, etc. can be contained as additives during molding.
[0072] Furthermore, the crosslinked PAS obtained according to the present invention can be used as a PAS resin composition appropriately blended with a synthetic resin such as polyester, polyamide, polyimide, polyetherimide, polycarbonate, polyphenylene ether, polysulfone, polyethersulfone, polyetheretherketone, polyetherketone, polyarylate, polyethylene, polypropylene, polytetrafluoroethylene, polyvinylidene fluoride, polystyrene, ABS resin, epoxy resin, silicone resin, phenolic resin, polyurethane resin, liquid crystal polymer, or an elastomer such as polyolefin rubber, fluororubber, silicone rubber, etc., depending on the application.
[0073] The cross-linked PAS obtained by the production method of the present invention also has the properties of heat resistance and dimensional stability that PAS resin originally has, and therefore, it is widely useful as a material for various molding processes such as injection molding or compression molding, or extrusion molding of composites, sheets, tubes, etc., or stretch molding, or as a material for fibers or films, such as electrical / electronic parts such as connectors, printed circuit boards, and encapsulated molded products, automotive parts such as lamp reflectors and various electrical equipment parts, interior materials for various buildings, aircrafts, and automobiles, or precision parts such as OA equipment parts, camera parts, and clock parts, etc., or as a material for fibers or films. In particular, the cross-linked PAS resin of the present invention has a short crystallization time, which is useful when used as a material for injection molding, and can improve demolding properties and further shorten molding cycles, thereby achieving improvements in molding processability and molding efficiency.
[0074] Example
[0075] The present invention will be described in detail below with reference to Examples, which are merely illustrative and not limiting.
[0076] [Synthesis Example] Preparation of uncrosslinked polyphenylene sulfide resin
[0077] Into a 150 L autoclave with stirring blades equipped with a pressure gauge, a thermometer, a condenser, a decanter, and a rectifying column, 33.222 kg (226 mol) of p-dichlorobenzene (hereinafter referred to as DCB), 2.280 kg (23 mol) of NMP, 27.300 kg (230 mol) of 47.23 mass % sodium hydrosulfide, and 18.533 kg (228 mol) of 49.21 mass % caustic soda were charged. Then, the valve of the pipe from the autoclave to the distillation apparatus was opened to start dehydration, and the valve of the pipe to the pressure reducing apparatus was opened. As the pressure was reduced from atmospheric pressure to 47 [kPa abs] at a rate of -6.6 [kPa abs] / min, the liquid temperature was gradually raised from 128°C to 147°C at a rate of 0.1°C / min, and finally dehydration was carried out at 47 [kPa abs] and a liquid temperature of 147°C for 4 hours. The mixed vapor of water and DCB discharged from the distillation tower is condensed in the condenser, and the water and p-DCB are separated in the decanter. Water is distilled out of the system at any time, and p-DCB is returned to the autoclave. The DCB distilled by post-azeotropy during dehydration is separated in the decanter and returned to the kettle at any time. After the dehydration is completed, the kettle is in a state where the anhydrous sodium sulfide composition is dispersed in DCB. Furthermore, the internal temperature is cooled to 160°C, 47.492kg (479mol) of NMP is added, and the temperature is raised to 185°C. At the moment when the pressure reaches 0.00MPa, the valve connected to the distillation tower is opened, and the temperature is raised to 200°C in 1 hour. At this time, cooling and valve opening are controlled in such a way that the outlet temperature of the distillation tower becomes below 110°C. The mixed vapor of DCB and water distilled is condensed in the condenser, separated in the decanter, and DCB is returned to the kettle. The amount of distilled water is 179G. Next, the internal temperature was raised from 200°C to 230°C over 3 hours, stirred for 1 hour, then raised to 250°C and stirred for 1 hour. After the reaction was completed, the internal temperature of the autoclave was cooled from 250°C to 235°C. After reaching the temperature, the bottom valve of the autoclave was opened, and the autoclave was directly rinsed in a 150-liter vacuum stirring dryer (desolventizer jacket temperature 120°C) with stirring blades under reduced pressure, N-methyl-2-pyrrolidone was extracted, cooled to room temperature and sampled, and a PPS mixture with an NV of 55% was obtained.
[0078] [Examples / Manufacturing Examples]
[0079] (Compression process)
[0080] The molding, pulverization and granulation were performed using a roller compression granulator (roller compactor). That is, the PPS mixture obtained in the synthesis example was put into the hopper with a screw feeder of the roller compactor, the screw feeder speed was set to 63.5 rpm, the roller compression pressure was adjusted in 5 stages of 1.0, 1.2, 1.5, 1.8, and 2.0 ton / cm, the roller speed was set to 15 rpm, and 30 kg of each plate-shaped compression molding was manufactured.
[0081] (Porosity Measurement Process)
[0082] Next, the porosity of each of the obtained compression-molded products was measured.
[0083] (Crushing and granulation process)
[0084] Then, the compression molded products were crushed by a coarse crusher while adjusting the processing amount to 848.4, 732.3, and 654.7 kg / hour, respectively, to produce 10 kg of crushed products.
[0085] Then, the crushed product was sized by a granulator and then sieved by a wire mesh (adjusted to 5.0 mm) of the granulator to obtain granulated products.
[0086] (Bulk density measurement process)
[0087] Then, 10 kg of each of the obtained granulated products was weighed, and the bulk density was measured for each.
[0088] [Table 1]
[0089] Porosity Bulk density % <![CDATA[g / cm 3 ]]> Granulated material 1 4.94 0.482 Granules 2 4.94 0.575 Granules 3 4.94 0.503 Granules 4 1.52 0.485 Granules 5 1.52 0.573 Granules 6 1.52 0.507 Granules 7 0.62 0.488 Granules 8 0.62 0.573 Granules 9 0.62 0.501 Granules 10 0.35 0.498 Granules 11 0.35 0.593 Granules 12 0.35 0.523 Granules 13 0.10 0.509 Granules 14 0.10 0.603 Granules 15 0.10 0.534
[0090] (Example 1)
[0091] (Oxidative cross-linking process)
[0092] From the granules thus obtained, 5 kg was weighed arbitrarily from each of the granules 1, 2, and 3 so that the porosity was constant, and the granules were placed in a box-type plate dryer preheated to 150° C., respectively, and heat-treated while blowing 2 L / min of air. The temperature was controlled so that the internal temperature of the heat treatment machine became 250° C. After maintaining for 0, 2, 4, and 6 hours, each granule that had completed oxidative crosslinking was obtained. The melt viscosity of each of these granules that had completed oxidative crosslinking was measured, and the results are shown in Table 2.
[0093] (Example 2)
[0094] Granulated materials that had undergone oxidation crosslinking were obtained in the same manner as in Example 1 except that "Granulated materials 4, 5, 6" were used instead of "Granulated materials 1, 2, 3" in Example 1. The melt viscosity of each granulated material that had undergone oxidation crosslinking was measured. The results are shown in Table 2.
[0095] (Example 3)
[0096] Granulated materials that had undergone oxidation crosslinking were obtained in the same manner as in Example 1 except that "Granulated materials 7, 8, 9" were used instead of "Granulated materials 1, 2, 3" in Example 1. The melt viscosity of each granulated material that had undergone oxidation crosslinking was measured. The results are shown in Table 2.
[0097] (Example 4)
[0098] Granulated materials 10, 11, 12 were used instead of Granulated materials 1, 2, 3 in Example 1. Granulated materials 10, 11, 12 were used instead of Granulated materials 1, 2, 3 in Example 1. The melt viscosity of the granulated materials 10, 11, 12 was measured.
[0099] (Example 5)
[0100] Granulated materials 13, 14, 15 were used instead of Granulated materials 1, 2, 3 in Example 1. Granulated materials 13, 14, 15 were used instead of Granulated materials 1, 2, 3 in Example 1. The melt viscosity of the granulated materials 13, 14, 15 was measured.
[0101] [Table 2]
[0102]
[0103] (Comparative Example 1)
[0104] (Oxidative cross-linking process)
[0105] From the granules thus obtained, 5 kg of each of the granules 1, 4, and 7 was weighed so that the bulk density was constant, and the mixture was placed in a box-type plate dryer preheated to 150° C., and heat-treated while blowing 2 L / min of air. The temperature was controlled so that the internal temperature of the heat treatment machine became 250° C. After being kept for 0, 2, 4, and 6 hours, each granule that had completed oxidative crosslinking was obtained. The melt viscosity of each of these granules that had completed oxidative crosslinking was measured, and the results are shown in Table 3.
[0106] (Comparative Example 2)
[0107] Granulated materials that had undergone oxidation crosslinking were obtained in the same manner as in Example 1 except that "Granulated materials 2, 5, 8" were used instead of "Granulated materials 1, 4, 7" in Comparative Example 1. The melt viscosity of each granulated material that had undergone oxidation crosslinking was measured. The results are shown in Table 3.
[0108] (Comparative Example 3)
[0109] Granulated materials that had undergone oxidation crosslinking were obtained in the same manner as in Example 1 except that "Granulated materials 3, 6, 9" were used instead of "Granulated materials 1, 4, 7" in Comparative Example 1. The melt viscosity of each granulated material that had undergone oxidation crosslinking was measured. The results are shown in Table 3.
[0110] [Table 3]
[0111]
[0112] The above results show that, compared with the case of using a granulated product with a constant bulk density, when a plate-shaped compression molded product with a constant porosity is used, a cross-linked PPS with less melt viscosity deviation at any heat treatment time tends to be obtained. Therefore, it is shown that, compared with the bulk density that varies depending on the particle size of the granulated product and the ratio of the voids between the granulated products, the progress of the cross-linking reaction and the melt viscosity can be managed with high accuracy.
[0113] In addition, the above results show that when the porosity of the plate-like compression molded product is in the range of 0.10 to 4.94, there is a tendency to obtain a cross-linked PPS with less melt viscosity deviation and high melt viscosity. It further shows that if the porosity of the plate-like compression molded product is in the range of 0.62 to 4.94, the cross-linking reaction can be promoted more efficiently and the melt viscosity can be increased in a short time.
[0114] In addition, each measurement was performed as follows.
[0115] (Measurement Example) Measurement of Porosity
[0116] The porosity (%) of the compression molded product is measured as follows: Using a plate-shaped compression molded product, the ratio of the volume of pores contained in a unit constant volume of the plate-shaped compression molded product is taken as the porosity (%), and the measurement is performed by the following X-ray CT scanning method.
[0117] (X-ray CT scan)
[0118] CT scanning conditions
[0119] X-ray CT scanning: “TDM1000H-II (2K)” manufactured by Yamato Scientific co., ltd. was used.
[0120] As current conditions, scanner: 2 inches, magnification axis position: 15 mm, tube voltage: 50 kV tube current: 0.085 mA, as pore scanning conditions, matrix size: 512×512×512 (pixcel), constructed field of view size: 1.08×1.08×1.08 (mm), reconstructed pixel size: 0.002123 (mm) × 3-directional binary threshold, porosity analysis was carried out, and the numbers of 10 times were recorded in the table.
[0121] (Measurement Example) Measurement of Bulk Density
[0122] The granulated material is scraped and filled into a cup in a container with a constant volume. After the lid is closed, the weight is measured with an electronic meter and divided by the volume to calculate the bulk density [g / cm 3 〕.
[0123] (Measurement Example) Measurement of Melt Viscosity
[0124] The oxidatively crosslinked granulated PPS was tested using a flow tester CFT-500D (manufactured by Shimadzu Corporation) at a temperature of 300°C and a load of 1.96 × 10 6 Under the conditions of Pa and L / D=10 (mm) / 1 (mm), the melt viscosity at 300° C. was measured after maintaining for 6 minutes.
Claims
1. A method for producing a cross-linked polyarylene sulfide, characterized in that: The invention comprises the following steps: a step of compressing powdered uncrosslinked polyarylene sulfide to obtain a compression molded product; a step of measuring the porosity of the compression molded product; a step of crushing the compression molded product within a specific porosity range to obtain a crushed product; a step of granulating the crushed product to obtain a granulated product; and a step of oxidatively crosslinking the granulated product obtained in the previous step, wherein the specific porosity range is a porosity range of 0.10 to 10.00%.
2. The method for producing a cross-linked polyarylene sulfide according to claim 1, wherein: The shape of the granulated material is amorphous.
3. A method for producing a resin composition, comprising: a step of producing a cross-linked polyarylene sulfide by the production method according to claim 1 or 2; and a step of melt-kneading the obtained cross-linked polyarylene sulfide with other components.
4. A method for producing a molded article, comprising: a step of producing a resin composition by the production method according to claim 3; and a step of melt-molding the obtained resin composition.