A γ-TiAl alloy for precision casting and preparation method thereof

By adjusting the Al content and adding B element, and combining vacuum arc consumable melting and vacuum arc solidification melting processes, a TiAl alloy with fine full-lamellar structure was prepared, which solved the problems of coarse grains and unstable mechanical properties of TiAl-4822 alloy, and achieved the improvement of high-temperature mechanical properties and the reduction of preparation cost.

CN116607048BActive Publication Date: 2024-11-22INST OF METAL RESEARCH - CHINESE ACAD OF SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210121410.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-09
Publication Date
2024-11-22
Estimated Expiration
2042-02-09

AI Technical Summary

Technical Problem

The existing TiAl-4822 alloy composition results in coarse grains, leading to unstable mechanical properties, especially in areas of varying blade thickness. Furthermore, it requires a cumbersome four-step heat treatment process, increasing manufacturing costs and affecting quality stability.

Method used

By adjusting the Al content and adding a large amount of B, the solidification route of the alloy was optimized. A combination of vacuum arc consumable melting and vacuum arc shell melting was adopted to prepare a fine and uniform full lamellar TiAl alloy, avoiding the formation of coarse columnar crystals.

Benefits of technology

This method enables the production of fine and uniform grain structures without heat treatment, improving the high-temperature mechanical properties and crack propagation resistance of the alloy, reducing manufacturing costs, and meeting the requirements of high thrust-to-weight ratio for aero-engines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003498365600000051
    Figure BDA0003498365600000051
  • Figure HDA0003498365610000011
    Figure HDA0003498365610000011
  • Figure HDA0003498365610000021
    Figure HDA0003498365610000021
Patent Text Reader

Abstract

The present invention belongs to the field of lightweight and high temperature resistant Ti-Al intermetallic compounds, specifically a γ-TiAl alloy for precision casting and a preparation method thereof, which is suitable for equiaxed and fine grained TiAl alloys formed by investment casting. The preparation process route adopts vacuum arc consumable melting VAR+vacuum arc condensation shell melting VSM or secondary vacuum arc consumable melting, and the specific range of alloy composition is: Ti-(42-44)Al-(1.7-2.3)Mo-(1.7-2.3)Nb–(0.6-1.0)B-(0.1-0.2)C (at%) or Ti-(28.5-29.8)Al-(2.3-3.3)Mo-(4.0-5.2)Nb-(0.20-0.28)B-(0.03-0.06)C (wt%). The present invention optimizes the Al element content, adjusts the alloy solidification route and adds a large amount of TiB2 nucleating agent, thereby avoiding the coarse columnar crystals formed by the solidification of traditional TiAl alloys, making the cast matrix have fine and uniform equiaxed grains, and realizing stable control of the microstructure and mechanical behavior of the cast TiAl alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of lightweight and high temperature resistant Ti-Al intermetallic compounds, specifically a γ-TiAl alloy for precision casting and a preparation method thereof, which is suitable for equiaxed and fine grained TiAl alloy components formed by investment casting. Background Art

[0002] GE, an internationally renowned engine company, designed the TiAl-4822 alloy, which had the best plasticity at the time (elongation 2%). In 2006, the TiAl alloy blades were used in the low-pressure turbine 6th and 7th stage blades of the GEnx engine powered by the Boeing 787 passenger aircraft, as well as the Genx-2B engine of the B747 passenger aircraft and the GE9X engine of the B777X passenger aircraft. The European Snecma company also applied TiAl-4822 alloy low-pressure turbine blades to the Leap-1A / Leap-1B engines of the 320 / 737 passenger aircraft, established a supply chain for TiAl-4822 alloy blades, and achieved stable batch production of blades. However, the composition of the TiAl-4822 alloy is a coarse full-lamellar structure in the cast state, with grains in the range of 500 to 1500μm ( Figure 1 ), the coarse grains often result in only a few grains in the blade body, and the grain boundary or grain orientation is the weak link in mechanical properties. The stability of mechanical properties of the blade's tenon, blade body, and sealing teeth, which are of different thicknesses, cannot be well guaranteed. In addition, the macroscopic columnar crystal structure of the thicker parts of the blade will also lead to strong anisotropy. For this reason, the alloy requires a cumbersome four-step heat treatment method to refine the microstructure ( Figure 2 ), the blade preparation cost is high, and the result of grain refinement is significantly affected by the process conditions and the thickness of the casting, which seriously affects the stability of the blade preparation quality. Summary of the invention

[0003] The purpose of the present invention is to provide a γ-TiAl alloy for precision casting and a preparation method thereof, wherein a TiAl alloy with a fine full-lamellar structure containing titanium, aluminum, niobium, molybdenum, boron and carbon elements is directly obtained by alloy solidification without heat treatment. The structure has good high-temperature comprehensive mechanical properties and is suitable for complex structure aviation parts such as low-pressure turbine blades and swirlers.

[0004] The technical solution of the present invention is:

[0005] A γ-TiAl alloy for precision casting has the following components in atomic percentage: Al 42-44%, Mo 1.7-2.3%, Nb 1.7-2.3%, B 0.6-1.0%, C 0.1-0.2% and Ti balance.

[0006] A γ-TiAl alloy for precision casting has the following components by mass percentage: Al 28.5-29.8%, Mo 2.3-3.3%, Nb 4.0-5.2%, B 0.20-0.28%, C 0.03-0.06% and Ti balance.

[0007] The preparation method of the γ-TiAl alloy for precision casting adopts a combined melting method of vacuum arc consumable melting VAR and vacuum arc shell melting VSM or secondary vacuum arc consumable melting to obtain the alloy.

[0008] The preparation method of the γ-TiAl alloy for precision casting comprises the following steps: adding sponge titanium, AlMo master alloy, AlNb master alloy, TiB2 or AlB master alloy, TiC master alloy and Al beans as raw materials, uniformly mixing and pressing into a dense electrode according to the required percentage of components, and then performing vacuum arc melting.

[0009] The design idea of ​​the present invention is:

[0010] The present invention adjusts the Al content in the range of 42-44 at%, so that the γ solidification route of the alloy is transformed into the β solidification route, avoiding the formation of α phase peritectic reaction when the Al content is between 45% and 49 at%, and the anisotropy caused by the γ{111} or {202} lamellae being perpendicular to the heat flow direction. The alloy adjusts the alloy solidification route by optimizing the Al element content and adding a large amount of TiB2 nucleating agent, avoiding the coarse columnar crystals formed by the solidification of the traditional TiAl alloy, so that the cast matrix has fine and uniform equiaxed grains, and ensures that the organization has good and stable mechanical properties.

[0011] The present invention combines the combined effects of low Al content components and Mo and Nb elements, breaks through the theoretical concept of 0.15at% upper limit of B element addition in TiAl alloy, creatively adds a large amount of 0.6-1.0at% B refining elements to form TiB2 to significantly refine the grains and improve the fluidity of the alloy, thereby achieving stable control of the microstructure and mechanical behavior of the cast TiAl alloy.

[0012] The advantages and beneficial effects of the present invention are:

[0013] 1. The characteristics of the TiAl-NMB alloy material of the present invention are that it adopts the preparation process route of vacuum arc consumable melting VAR + vacuum arc shell melting VSM or secondary vacuum arc consumable melting. Under working conditions, β solidification forms a full-lamellar microstructure with an average grain size of less than 100μm. Its fine full-lamellar structure is insensitive to the wall thickness of the casting, and the grain size will not change significantly with the increase of wall thickness; the full-lamellar structure has a good ability to contain crack propagation for brittle TiAl alloys, and has a good guarantee for improving the high-cycle fatigue performance of the material; the fine-grained cast equiaxed structure enables the matrix to maintain a relatively high strength and stable mechanical behavior, and the isotropy and mechanical convergence are very good.

[0014] 2. The density of TiAl alloy is only half of that of nickel-based high-temperature alloy. Due to its good specific strength and specific modulus, TiAl alloy can replace high-temperature alloy materials in the temperature range of 600-700°C to prepare key load-bearing components of the hot end of high thrust-to-weight ratio aircraft engines. The cast TiAl alloy of the present invention is optimized in composition on the basis of traditional γ-TiAl alloy, so that the coarse cast TiAl alloy grain size can be prepared without heat treatment and other measures. Through composition optimization design, the solidified cast structure directly has a fine grain structure, and the full lamellar structure has good crack propagation resistance and fatigue performance, which meets the comprehensive mechanical performance requirements of TiAl alloy precision castings in high thrust-to-weight ratio aircraft engines.

[0015] 3. The TiAl-NMB alloy of the present invention replaces the nickel-based high-temperature alloy to make the last two-stage blades of the low-pressure turbine of a large bypass ratio aircraft engine, which can greatly reduce the static and dynamic load weight of the engine, and has a very significant contribution to improving the thrust-to-weight ratio and fuel efficiency of the engine. Using TiAl-NMB alloy to replace the nickel-based K417G high-temperature alloy to make the last-stage blades of the low-pressure turbine of the engine can achieve a 50% weight reduction of the working blade itself, and a blade static load weight reduction of about 5 to 10 kg. After the blade weight is reduced, the centrifugal load on the turbine disk will be significantly reduced, which is of great significance to the realization of the weight reduction goal of the aircraft engine. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is the cast structure of traditional TiAl-4822 alloy.

[0017] Figure 2 It is a near-γ cast structure of traditional TiAl-4822 alloy after four-step grain refinement heat treatment.

[0018] Figure 3 It is the fine full lamellar cast structure of the TiAl-NMB alloy of the present invention.

[0019] Figure 4 The grain size distribution statistics of various parts of the TiAl-NMB alloy aero-engine combustion chamber swirler of the present invention are shown. DETAILED DESCRIPTION

[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example 1

[0022] In this embodiment, the composition of TiAl-NMB alloy is Ti-44Al-2.0Nb-2.0Mo-0.8B-0.1C (at%) or Ti-29.8Al-4.6Nb-2.8Mo-0.26B-0.03C (wt%). After being uniformly mixed with raw materials according to the required composition, 10kg electrodes are pressed. After six electrodes are assembled and vacuum welded, a primary pre-alloyed ingot with a diameter of 170mm and a length of 700mm is prepared by a vacuum consumable arc melting VAR (Vacuum Arc Remelting). The materials used to press the electrode are sponge titanium, pure aluminum, AlMo, AlNb, TiC and TiB2 intermediate alloy particles configured according to the above composition. The particle size of the raw materials is: sponge titanium 3-12.7mm, pure aluminum (Al beans) 6-12mm, AlMo intermediate alloy 1-4mm, AlNb intermediate alloy 1-3mm, TiC intermediate alloy and TiB2 intermediate alloy less than 100 mesh.

[0023] The two primary pre-alloyed ingots are welded together in a vacuum or argon atmosphere, and then melted again by secondary vacuum consumable arc melting (VAR) into a 120 kg ingot with a diameter of 220 mm.

[0024] In this embodiment, after the TiAl-NMB alloy is obtained by a combination of vacuum arc consumable melting VAR and secondary vacuum arc consumable melting VAR, the secondary smelted ingot is sawn into four parts, and each 30 kg part is placed in a vacuum induction water-cooled copper crucible ISM (induction skull melting) to melt and cast TiAl alloy low-pressure turbine blades, which have a fine and uniform full-lamellar structure. The grain size of the exhaust edge / inlet edge at the thinnest part of the blade is close to that of the tenon at the thickest part (30-70 μm), see Figure 4 At 650℃, the blade material has a yield strength σ 0.2 ≥400MPa, breaking strengthσ b ≥500MPa, elongation ≥5%, fatigue limit strength ≥350MPa, which are significantly better than the traditional TiAl-4822 alloy performance of 100~120MPa.

[0025] Example 2

[0026] In this embodiment, the composition of the TiAl-NMB alloy is Ti-42Al-2.0Nb-2.0Mo-1.0B-0.2C (at%) or Ti-28.5Al-4.6Nb-2.8Mo-0.28B-0.06C (wt%). After being uniformly mixed with the raw materials according to the required composition, 22kg electrodes are pressed. After the six electrodes are assembled and vacuum welded, a primary pre-alloyed ingot with a diameter of 220mm and a length of 1000mm is prepared by a vacuum consumable arc melting VAR (Vacuum Arc Remelting). The materials used to press the electrode are sponge titanium, pure aluminum, AlMo, AlNb, TiC and AlB intermediate alloy particles configured according to the above composition. The particle size of the raw materials is: sponge titanium 8-12.7mm, pure aluminum (Al beans) 6-9mm, AlMo intermediate alloy 1-3mm, AlNb intermediate alloy 1-2mm, TiC intermediate alloy and AlB intermediate alloy less than 80 mesh.

[0027] The primary pre-alloyed ingot is welded with auxiliary guide rods under vacuum or argon atmosphere conditions, and is melted and cast again by vacuum skull melting (VSM) to form 22 5-7 kg split mold ingots with a diameter of 80 mm. This eliminates the need for sawing, facilitating accurate weight feeding in the next step of precision casting.

[0028] In this embodiment, after the TiAl-NMB alloy is obtained by vacuum arc consumable melting VAR + vacuum arc condensation shell melting VSM combined melting method, the ingot of secondary condensation shell melting is divided into corresponding portions according to the required weight, such as 30kg placed in a water-cooled copper crucible to melt and cast the TiAl alloy booster impeller. The impeller has a full lamellar structure regardless of the central axis or the peripheral thin-walled blades, and the grain size is in the range of 50 to 150 μm, showing good microstructural uniformity. At a temperature of 700°C, the impeller material has a yield strength σ 0.2 ≥350MPa, breaking strengthσ b ≥480MPa, elongation ≥8%, fatigue limit strength ≥320MPa, which is 50-100MPa better than the traditional TiAl-4822 alloy performance.

[0029] Example 3

[0030] In this embodiment, the composition of the TiAl-NMB alloy is Ti-43Al-2.0Nb-2.0Mo-0.6B-0.15C (at%) or Ti-29.2Al-4.6Nb-2.8Mo-0.20B-0.045C (wt%). After being uniformly mixed with the raw materials according to the required composition, a 4kg electrode is pressed. After the four electrodes are assembled and vacuum welded, a vacuum consumable arc melting VAR (Vacuum Arc Remelting) is used to prepare a primary pre-alloyed ingot with a diameter of 120mm and a length of 500mm. The materials used to press the electrode are sponge titanium, pure aluminum, AlMo, AlNb, TiC and TiB2 intermediate alloy particles configured according to the above composition. The particle size of the raw materials is: sponge titanium 3-6mm, pure aluminum (Al beans) 3-8mm, AlMo intermediate alloy 2-4mm, AlNb intermediate alloy 2-3mm, TiC intermediate alloy and TiB2 intermediate alloy less than 60 mesh.

[0031] Four primary pre-alloyed ingots are welded together in a vacuum or argon atmosphere, and auxiliary guide rods are welded on, and then melted again by secondary vacuum consumable arc melting (VAR) into a 64 kg ingot with a diameter of 170 mm.

[0032] In this embodiment, after the TiAl-NMB alloy is obtained by a combined smelting method of primary vacuum arc consumable melting VAR + secondary vacuum arc consumable melting VAR, the secondary smelted ingot is sawn into four parts, each part weighing 16 kg is placed in a vacuum induction water-cooled copper crucible ISM (induction skull melting) to melt and cast a TiAl alloy vortex finder. The thinnest thickness of the vortex finder impeller is only 0.7 mm. The TiAl-4822 alloy is extremely difficult to form, and the number of local grains in the thin wall is small. By optimizing the alloy composition, the mold can be well filled and fine grains can be formed, so that the comprehensive mechanical properties of the impeller are greatly improved.

[0033] Table 1 Comparison of cast properties of two TiAl alloys

[0034]

[0035] From Table 1 and Figure 3 It can be seen that the present invention aims at the drawbacks of TiAl-4822 and proposes an optimized composition of TiAl alloy for precision casting. The optimal fine full-lamellar structure of TiAl alloy in the cast state can be achieved only by the composition, so that the castability is improved and good high temperature performance and fatigue performance are obtained.

Claims

1. A γ-TiAl alloy for precision casting, characterized in that: The composition of the γ-TiAl alloy is as follows in terms of atomic percentage: Al42~44%, Mo1.7~2.3%, Nb1.7~2.3%, B0.6~1.0%, C 0.1~0.2%, and Ti balance; the TiAl alloy has a full lamellar microstructure in the cast state, and β solidification forms a full lamellar microstructure with an average grain size of less than 100μm, showing microstructural uniformity.

2. A method for preparing a γ-TiAl alloy for precision casting according to claim 1, characterized in that: It is obtained by vacuum arc consumable melting (VAR), vacuum arc shell melting (VSM) or secondary vacuum arc consumable melting.

3. The method for preparing a γ-TiAl alloy for precision casting according to claim 2, characterized in that: The raw materials are titanium sponge, AlMo master alloy, AlNb master alloy, TiB2 or AlB master alloy, TiC master alloy and Al beans, which are uniformly mixed and pressed into dense electrodes according to the required composition percentages, and then vacuum arc melting is carried out.