A copper-based low-temperature catalyst and its preparation method and application

Using citric acid and valine to construct a copper-based catalyst carrier solves the problem of agglomeration of active components in copper-based catalysts, achieves stable dispersion of copper and efficiently catalyzes hydrogen production from methanol reforming, significantly increasing the hydrogen production rate and maintaining high selectivity. sex.

CN116618047BActive Publication Date: 2024-10-18GUANGDONG UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310428098.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-18
Estimated Expiration
2043-04-19

AI Technical Summary

Technical Problem

The active component copper of existing copper-based low-temperature catalysts is prone to agglomeration during use, resulting in reduced dispersion and low hydrogen production rate, making it difficult to achieve efficient catalytic hydrogen production by methanol reforming at low temperatures.

Method used

A combination of citric acid and valine is used to construct a carrier for a copper-based catalyst, and stable dispersion of copper is achieved through coordination. The preparation method includes mixing a copper salt solution, citric acid and valine at a specific molar ratio, and calcining to form a solid carrier. And it is reduced in a hydrogen atmosphere to form monovalent copper ions as the active component.

Benefits of technology

The hydrogen production rate of the catalyst is improved. The copper particles have excellent dispersion on the catalyst. When catalyzing methanol reforming for hydrogen production, the hydrogen production rate reaches 72.68 μmol·gcat-1·s-1, and the hydrogen selectivity is higher than 99.86%. Maintain high catalytic activity at lower temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116618047B_ABST
    Figure CN116618047B_ABST
Patent Text Reader

Abstract

The present invention discloses a copper-based low-temperature catalyst and a preparation method and application thereof. The preparation method of the copper-based low-temperature catalyst provided by the present invention uses valine and citric acid to jointly construct an organic carbon carrier in the catalyst. Specifically, the present invention uses a solution system to construct a catalyst with highly dispersed active components, so that it can catalyze methanol to produce hydrogen at a low temperature of 210°C or below, and the three carboxyl groups in citric acid and the one amino group in valine can form a stable ligand structure with copper, so that the copper on the catalyst has excellent dispersibility and the copper can be prevented from migrating and dispersing in the catalyst, thereby maintaining its excellent dispersibility, and finally enabling the catalyst to have excellent catalytic activity during the reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalyst preparation, and in particular to a copper-based low-temperature catalyst and a preparation method and application thereof. Background Art

[0002] Energy is the foundation of human production and life. Hydrogen energy is clean, efficient, safe and sustainable. It is regarded as the cleanest energy with the greatest development potential in the 21st century. It can be seen that the development of hydrogen energy has important energy value and strategic significance. High-temperature proton exchange membrane fuel cell (HT-PEMFC), also known as high-temperature polymer electrolyte membrane fuel cell, is a PEM fuel cell that mainly uses methanol as fuel and operates at a cell temperature of 150 to 180°C. The reaction temperature of methanol liquid phase reforming to produce hydrogen (APRM) is mostly between 210°C and 350°C. Therefore, if heat exchange between APRM reaction and HT-PEMFC is to be realized, it is particularly important to develop a catalyst for low-temperature and efficient hydrogen production.

[0003] The prior art discloses a highly dispersed copper-based catalyst and its preparation method and application. The catalyst provided by the prior art can also catalyze methanol reforming to produce hydrogen at a low temperature below 210°C. The principle is that ZnO and CeO2 are used as the catalyst carrier, and the agglomeration of the active component copper is avoided through the synergistic effect between the two metal oxides. However, in the catalyst prepared by the prior art, copper is loaded on the carrier by physical adsorption. The active component is still prone to agglomeration during the use of the catalyst, so the maximum hydrogen production rate can only reach 58.39μmol·g cat -1 ·s -1 . Summary of the invention

[0004] In order to solve the problem in the prior art that the active component copper on the copper-based low-temperature catalyst used for catalytic methanol reforming to produce hydrogen is easily agglomerated during use to cause a decrease in dispersibility, the present invention provides a method for preparing a copper-based low-temperature catalyst, a carrier of the copper-based catalyst is constructed by combining citric acid and valine, and stable dispersion of copper is achieved through the coordination effect between citric acid, valine and copper, thereby improving the catalytic hydrogen production rate of the catalyst.

[0005] Another object of the present invention is to provide a copper-based low-temperature catalyst.

[0006] Another object of the present invention is to provide an application of a copper-based low-temperature catalyst in catalytic methanol reforming to produce hydrogen.

[0007] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0008] A method for preparing a copper-based low-temperature catalyst comprises the following steps:

[0009] S1. Mixing a copper salt solution, citric acid and valine in a molar ratio of copper in the copper salt solution: citric acid: valine = 1.4: (0.8-1.2): (0.1-0.5) and reacting them sufficiently to obtain a Cu-CA-Val complex;

[0010] S2. calcining the Cu-CA-Val complex obtained in step S1 in an inert gas atmosphere at 250°C to 450°C for 1 to 4 hours to obtain a copper-based low-temperature catalyst precursor;

[0011] S3. The copper-based low-temperature catalyst precursor obtained in step S2 is placed in a hydrogen atmosphere for reduction to obtain a copper-based low-temperature catalyst.

[0012] The purpose of step S1 is to construct the structural framework of a copper-based low-temperature catalyst in a solution, wherein CA represents citric acid and Val represents valine; the purpose of step S2 is to carbonize citric acid and valine to form a solid catalyst carrier; and in step S3, after hydrogen reduction, the copper ions loaded on the carrier can be reduced to monovalent copper ions and metallic copper as active components acting on the catalyst.

[0013] In step S1, since the liquid is a good dispersant, the catalyst is constructed in the solution, so that the active component copper has excellent high dispersibility on the final catalyst carrier; citric acid and valine are used to construct the catalyst carrier because citric acid and valine have three carboxyl groups and one amino group respectively, and the carboxyl group can be bonded and coordinated with copper to form a stable coordination tetrahedral structure, while the amino group can be used as an additional anchor point to further coordinate with copper, wrapping the copper ion inside, so that it is not easy to migrate and agglomerate during the use of the catalyst, and maintain excellent dispersibility. The molar ratio of copper, citric acid and valine in the copper salt solution is controlled to 1.4: (0.8-1.2): (0.1-0.5), the purpose of which is to make the three reactants form a stable ligand structure.

[0014] The calcination temperature, time and gas atmosphere in step S2 are limited in order to simultaneously carbonize valine and citric acid to form an organic carbon carrier to provide attachment sites for copper. When the calcination temperature in S2 is lower than 250°C, the carrier is difficult to form, and when the temperature is higher than 450°C, the particles of the active component copper tend to agglomerate; when the calcination time is lower than 1h, the organic carbon carrier is also difficult to form, and if the calcination time is higher than 4h, it is not conducive to the dispersion of copper on the catalyst because the components on the carrier are easily lost.

[0015] Preferably, the molar ratio of copper to citric acid and valine in the copper salt solution in step S1 is 1.4:(0.9-1.1):(0.2-0.4).

[0016] More preferably, the molar ratio of copper to citric acid and valine in the copper salt solution in step S1 is 1.4:1:0.3.

[0017] When the molar ratio of copper to citric acid and valine in the copper salt solution in step S1 is 1.4:1:0.3, copper has the highest loading on the catalyst and the catalyst has the best effect in catalyzing hydrogen production. This is because at the molar ratio of 1.4:1:0.3, the coordination of the active component copper with citric acid and valine is the most complete and there are no excess bonding electrons.

[0018] Preferably, the calcination temperature in step S2 is 270-350°C.

[0019] Preferably, the calcination time in step S2 is 2 to 3.5 hours.

[0020] The most important role of calcination temperature and time is to decompose and interact with each component. If the calcination time is shorter or the temperature is lower, the organic carbon carrier is not fully calcined, it is difficult to form a stable carrier structure, and the bonding between the active component and the carrier is also insufficient. If the calcination temperature is higher or the calcination time is longer, the active components are easy to sinter and agglomerate, and valine itself is easy to undergo dehydration polymerization reaction, resulting in the breaking of the coordination bond formed with copper. In this case, copper is easy to form large metal particles, the active sites are reduced, and the hydrogen production effect is poor.

[0021] In a specific embodiment of the present invention, the reduction in step S3 can be performed at a temperature of 250 to 550°C.

[0022] Preferably, the reduction temperature in step S3 is 350°C.

[0023] The present invention also protects a copper-based low-temperature catalyst prepared by the above-mentioned method for preparing the copper-based low-temperature catalyst.

[0024] Preferably, the copper loading in the copper-based low-temperature catalyst is 48-60%.

[0025] In a specific embodiment of the present invention, the copper loading on the copper-based catalyst is the proportion of the mass of copper in the total mass of the catalyst. The preparation method of the copper-based low-temperature catalyst provided by the present invention can achieve an excellent copper loading, and the more active component copper on the catalyst, the better the catalytic performance of the catalyst, but when the mass of copper on the catalyst accounts for more than 60% of the total mass of the catalyst, copper is prone to agglomeration during the use of the catalyst, reducing the catalytic activity of the catalyst.

[0026] More preferably, the copper loading in the copper-based low-temperature catalyst is 55-58%.

[0027] More preferably, in the copper-based low-temperature catalyst, copper particles with a particle size of 8 to 13 nm account for 82 to 90% of all copper particles.

[0028] The particle size of the active component copper particles on the catalyst can indicate the dispersibility of the copper nanoparticles. When the copper particles with a particle size of 8 to 13 nm account for 82 to 90% of all copper particles, it means that the copper on the copper-based catalyst has a relatively consistent particle size, and the particle size is only 8 to 13 nm, indicating that the copper has excellent dispersibility on the catalyst carrier. At this time, the probability of the active component agglomerating during the use of the catalyst is lower, and the active component can have a larger contact area with the substrates of the reaction catalyzed by it, namely methanol and water, so it has a higher catalytic activity when catalyzing methanol reforming to produce hydrogen.

[0029] More preferably, copper particles with a particle size of 9 to 12 nm in the copper-based low-temperature catalyst account for 89 to 90% of all copper particles.

[0030] The present invention also protects an application of the copper-based low-temperature catalyst in catalyzing methanol reforming to produce hydrogen.

[0031] In a specific embodiment of the present invention, the specific method for applying the above-mentioned copper-based low-temperature catalyst to catalytic methanol reforming to produce hydrogen is: adding the copper-based low-temperature catalyst to a reaction solution of water and methanol, using argon as a protective gas, and conducting a hydrogen production reaction in an intermittent reactor.

[0032] Preferably, the reaction temperature of the copper-based low-temperature catalyst when catalyzing methanol reforming to produce hydrogen is 180-210°C.

[0033] The existing methanol liquid phase reforming to produce hydrogen is mostly carried out at a temperature of 210 to 350°C. The copper in the copper-based catalyst provided by the present invention has excellent dispersibility and the copper particles will not agglomerate during use, so it also has excellent catalytic activity at a lower temperature (180 to 210°C).

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] The present invention uses valine and citric acid to construct a carrier of a copper-based catalyst, wherein the carrier and the active component copper can be connected to each other through coordination. Therefore, the preparation method provided by the present invention can make the copper on the copper-based catalyst maintain excellent dispersibility and will not agglomerate during the use of the catalyst. The copper-based low-temperature catalyst prepared by the preparation method of the copper-based low-temperature catalyst provided by the present invention has a low temperature of 72.68 μmol·g cat -1 ·s-1 The hydrogen production rate is 2.5 times that of conventional conventional methods, and the selectivity of hydrogen in the produced gas is higher than 99.86%. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a comparison chart of the catalytic performance of the copper-based low-temperature catalyst prepared in Example 1 of the present invention, the commercial CuZnAl catalyst, and the commercial Raney Cu catalyst in catalyzing the hydrogen production reaction of methanol liquid phase reforming at 180°C.

[0037] Figure 2 XRD spectrum of the copper-based low-temperature catalyst obtained by adjusting the molar ratio of copper salt to citric acid.

[0038] Figure 3 HRTEM image of the copper-based low-temperature catalyst prepared in Example 1 of the present invention and the corresponding mapping element analysis image.

[0039] Figure 4 This is a transmission electron microscope image of copper particles in the copper-based low-temperature catalyst prepared in Example 1 of the present invention.

[0040] Figure 5 This is a statistical diagram of the particle size of copper particles in the copper-based low-temperature catalyst prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0041] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.

[0042] Example 1

[0043] A method for preparing a copper-based low-temperature catalyst comprises the following steps:

[0044] S1. mixing a copper salt solution, citric acid and valine in a molar ratio of copper in the copper salt solution: citric acid: valine = 1.4:1:0.3 and reacting them sufficiently to obtain a Cu-CA-Val complex;

[0045] S2. The Cu-CA-Val complex obtained in step S1 is calcined in an inert gas atmosphere at 300° C. for 3 h to obtain a copper-based low-temperature catalyst precursor;

[0046] S3. The copper-based low-temperature catalyst precursor obtained in step S2 is placed in a hydrogen atmosphere for reduction to obtain a copper-based low-temperature catalyst.

[0047] The copper-based low-temperature catalyst prepared by the method for preparing the copper-based low-temperature catalyst in the above Example 1 has a copper loading of 58.00%, and copper particles with a particle size of 11.5 nm account for 90% of all copper particles.

[0048] Example 2

[0049] A method for preparing a copper-based low-temperature catalyst, which differs from Example 1 in that:

[0050] S1. Mixing a copper salt solution, citric acid and valine in a molar ratio of copper in the copper salt solution: citric acid: valine = 1.4:1.1:0.2;

[0051] S2. The Cu-CA-Val complex obtained in step S1 was calcined in an inert gas atmosphere at 350° C. for 2 h.

[0052] The copper-based low-temperature catalyst prepared by the method for preparing the copper-based low-temperature catalyst in Example 2 has a copper loading of 56.14%, and copper particles with a particle size of 10.5 nm account for 89% of all copper particles.

[0053] Example 3

[0054] A method for preparing a copper-based low-temperature catalyst, which differs from Example 1 in that:

[0055] S1. Mixing a copper salt solution, citric acid and valine in a molar ratio of copper in the copper salt solution: citric acid: valine = 1.4:0.9:0.4;

[0056] S2. The Cu-CA-Val complex obtained in step S1 was calcined in an inert gas atmosphere at 270° C. for 3.5 h.

[0057] The copper-based low-temperature catalyst prepared by the preparation method of the copper-based low-temperature catalyst in the above Example 3 has a copper loading of 55.05%, and copper particles with a particle size of 9.5 nm account for 90% of all copper particles.

[0058] Example 4

[0059] A method for preparing a copper-based low-temperature catalyst, which differs from Example 1 in that:

[0060] S1. Mix a copper salt solution, citric acid and valine in a molar ratio of copper in the copper salt solution: citric acid: valine = 1.4:1.2:0.1.

[0061] The copper-based low-temperature catalyst prepared by the method for preparing the copper-based low-temperature catalyst in Example 4 has a copper loading of 51.17%, and copper particles with a particle size of 9 nm account for 87% of all copper particles.

[0062] Example 5

[0063] A method for preparing a copper-based low-temperature catalyst, which differs from Example 1 in that:

[0064] S1. Mix a copper salt solution, citric acid and valine in a molar ratio of copper in the copper salt solution: citric acid: valine = 1.4:0.8:0.5.

[0065] The copper-based low-temperature catalyst prepared by the method for preparing the copper-based low-temperature catalyst in Example 5 has a copper loading of 50.76%, and copper particles with a particle size of 12 nm account for 88% of all copper particles.

[0066] Example 6

[0067] A method for preparing a copper-based low-temperature catalyst, which differs from Example 1 in that:

[0068] S2. calcining the Cu-CA-Val complex obtained in step S1 at 450° C. in an inert gas atmosphere.

[0069] The copper-based low-temperature catalyst prepared by the method for preparing the copper-based low-temperature catalyst in Example 6 above has a copper loading of 49.49%, and copper particles with a particle size of 12.5 nm account for 90% of all copper particles.

[0070] Example 7

[0071] A method for preparing a copper-based low-temperature catalyst, which differs from Example 1 in that:

[0072] S2. calcining the Cu-CA-Val complex obtained in step S1 in an inert gas atmosphere at 250°C.

[0073] The copper-based low-temperature catalyst prepared by the method for preparing the copper-based low-temperature catalyst in Example 7 above has a copper loading of 50.01%, and copper particles with a particle size of 8 nm account for 85% of all copper particles.

[0074] Example 8

[0075] A method for preparing a copper-based catalyst, which differs from Example 1 in that:

[0076] S2. Calcine the Cu-CA-Val complex obtained in step S1 for 1 h.

[0077] The copper-based low-temperature catalyst prepared by the method for preparing the copper-based low-temperature catalyst in Example 8 has a copper loading of 49.75%, and copper particles with a particle size of 8 nm account for 82% of all copper particles.

[0078] Example 9

[0079] A method for preparing a copper-based catalyst, which differs from Example 1 in that:

[0080] S2. Calcine the Cu-CA-Val complex obtained in step S1 for 4 h.

[0081] The copper-based low-temperature catalyst prepared by the method for preparing the copper-based low-temperature catalyst in Example 9 above has a copper loading of 39.25%, and copper particles with a particle size of 12 nm account for 84% of all copper particles.

[0082] Comparative Example 1

[0083] A method for preparing a copper-based low-temperature catalyst, which differs from Example 1 in that:

[0084] S1. Mix a copper salt solution, citric acid and valine in a molar ratio of copper in the copper salt solution: citric acid: valine = 1.4:1.5:0.01.

[0085] The copper-based low-temperature catalyst prepared by the preparation method of the copper-based low-temperature catalyst in Comparative Example 1 has a copper loading of 43.73%, and copper particles with a particle size of 10 nm account for 80% of all copper particles.

[0086] Comparative Example 2

[0087] A method for preparing a copper-based low-temperature catalyst, which differs from Example 1 in that:

[0088] S1. Mix a copper salt solution, citric acid and valine in a molar ratio of copper in the copper salt solution: citric acid: valine = 1.4:0.5:1.0.

[0089] The copper-based low-temperature catalyst prepared by the preparation method of the copper-based low-temperature catalyst in Comparative Example 2 has a copper loading of 37.95%, and copper particles with a particle size of 9 nm account for 85% of all copper particles.

[0090] Comparative Example 3

[0091] A method for preparing a copper-based low-temperature catalyst, which differs from Example 1 in that:

[0092] S2. calcining the Cu-CA-Val complex obtained in step S1 in an inert gas atmosphere at 500°C.

[0093] The copper-based low-temperature catalyst prepared by the preparation method of the copper-based low-temperature catalyst in Comparative Example 3 has a copper loading of 33.54%, and copper particles with a particle size of 12.5 nm account for 90% of all copper particles.

[0094] Comparative Example 4

[0095] A method for preparing a copper-based low-temperature catalyst, which differs from Example 1 in that:

[0096] S2. Calcine the Cu-CA-Val complex obtained in step S1 for 6 hours.

[0097] The copper-based low-temperature catalyst prepared by the preparation method of the copper-based low-temperature catalyst in Comparative Example 4 has a copper loading of 31.73%, and copper particles with a particle size of 12.5 nm account for 85% of all copper particles.

[0098] Comparative Example 5

[0099] A method for preparing a copper-based low-temperature catalyst, which differs from Example 1 in that:

[0100] S1. Mix the copper salt solution, citric acid and glycine.

[0101] The copper-based low-temperature catalyst prepared by the preparation method of the copper-based low-temperature catalyst in Comparative Example 5 has a copper loading of 26.17%, and copper particles with a particle size of 15 nm account for 85% of all copper particles.

[0102] Performance Testing

[0103] Catalytic performance test: 50 mg of the copper-based low-temperature catalyst prepared in the embodiment and the comparative example was added to 20 mL of a reaction solution of water and methanol in a molar ratio of 1:1, and 2 MPa argon was used as a protective gas to conduct a hydrogen production performance test in an intermittent reactor. After reacting for 1 hour at 210°C, the gas phase product was quantitatively analyzed using gas chromatography after cooling to room temperature. The hydrogen production rate is obtained by calculating the gas production volume using the water displacement method, and the hydrogen production rate is the μmol hydrogen content produced per gram of catalyst per second; the selectivity is calculated by the amount of H2, CO, and CH4 in the product, for example, hydrogen selectivity H2 (%) = nH2*100% / (nH2+nCO+nCH4).

[0104] Catalytic performance test at different temperatures: The copper-based low-temperature catalyst provided in Example 1 was used for the test. The specific operating steps were the same as those for the catalytic performance test, except that the reaction temperatures were 210° C. and 350° C., respectively.

[0105] The specific test data are as follows Table 1-2 Figures 1 to 5 As shown:

[0106]

[0107] Table 2. Catalytic performance of the copper-based low-temperature catalyst provided in Example 1 at different temperatures

[0108]

[0109] From the data of Examples 1 to 3 in Table 1, it can be seen that in the method for preparing the copper-based low-temperature catalyst provided by the present invention, when the molar ratio of copper to citric acid and valine in the copper salt solution is 1.4, which is preferred in the present invention:

[0110] When the calcination time and temperature are in the preferred range of 270-350°C and 2-3.5h, respectively, the obtained copper-based low-temperature catalyst has a better hydrogen production rate, and the specific hydrogen production rate can reach 70 μmol·g cat -1 ·s -1 Above. It can be seen from the data of Examples 4 to 5 that when the amount of citric acid or valine is more, it means that the amount of valine or citric acid is less. In this case, the bonding and coordination between copper and the organic carbon carrier of the catalyst is not sufficient, so the hydrogen production rate of the catalyst is poor. It can be seen from the data of Examples 6 to 9 that when the calcination temperature in step S2 is low or the time is short, which is not within the preferred range of the present invention, the organic carbon carrier of the catalyst cannot be more fully calcined and it is difficult to form a stable carrier structure, and the bonding between the carrier and copper is not sufficient, so the hydrogen production rate of the catalyst is poor; but when the calcination temperature is too high or the time is too long, copper is easy to sinter and agglomerate to form large particles, so the hydrogen production rate of the catalyst is also reduced. It can be seen from the data of Comparative Examples 1 to 2 that when the amount of valine and citric acid in step S1 is too small, the organic carbon carrier formed by calcination is not sufficiently bonded to copper, and a stable ligand structure cannot be formed. Therefore, the hydrogen production rate of the obtained copper-based low-temperature catalyst can only reach a maximum of 56.93μmol·g cat -1 ·s -1 . From the data of Comparative Examples 3 to 4, it can be seen that when the calcination temperature in step S2 is too high or the time is too long, copper itself will sinter and then agglomerate, and valine will undergo self-dehydration polymerization reaction, and the coordination bond formed with copper will break, which will further cause the active component copper to migrate and agglomerate to form large particles of copper, and the effective specific surface area of ​​the catalyst is reduced, so the catalytic hydrogen production rate is low. From the data of Comparative Example 5, it can be seen that valine is an indispensable necessary condition for the present invention to prepare an organic carbon carrier that bonds well with copper. Compared with valine, glycine has a shorter carbon chain. Although glycine also has only one amino group and can form a saturated coordination with copper and citric acid, it is precisely because of the shorter carbon chain that the organic carbon carrier formed by high-temperature calcination of glycine is not stable. The carrier is easily decomposed during the catalytic hydrogen production reaction, so the catalytic hydrogen production rate is low.

[0111] As can be seen from Table 2, although the copper-based low-temperature catalyst provided by the present invention can catalyze the reaction of methanol reforming to produce hydrogen at a relatively low temperature of 210°C, it can also be used at the general reaction temperature (350°C) of catalyzing methanol reforming to produce hydrogen.

[0112] Figure 1 The catalytic performance comparison chart of the copper-based low-temperature catalyst prepared in Example 1 of the present invention and the commercial CuZnAl catalyst and the commercial Raney Cu catalyst in the hydrogen production reaction of methanol liquid phase reforming at 180°C is shown. Figure 1 It can be seen that when catalyzing the hydrogen production reaction at 180°C, the copper-based low-temperature catalyst prepared in Example 1 of the present invention has a catalyst capacity of 14.46 μmol·g cat -1 ·s -1 The hydrogen production rate and hydrogen selectivity of up to 99.91% are both higher than those of commercial CuZnAl catalysts and Raney Cu catalysts. The hydrogen production rate is 2.19 times that of the commercial CuZnAl catalyst and 11.76 times that of the commercial Raney Cu catalyst under the same conditions. In addition, the raw materials of the copper-based catalyst provided by the present invention are widely available and inexpensive, which can greatly reduce the cost of commercialization.

[0113] Figure 2 XRD spectrum of copper-based low-temperature catalyst obtained by adjusting the molar ratio of copper salt to citric acid. Figure 2 It can be seen that when only the molar ratio of copper salt to citric acid is adjusted in step S1, as Cu 2+ As the ratio of carbon to CA increases from 0.8 to 1.8, the characteristic peak of copper in the XRD spectrum gradually becomes sharper, and the particle size of the copper nanoparticles increases from 9.1 nm to 37.8 nm. This indicates that with the increase of the active component copper, the organic carbon carrier obtained by calcination in the present invention is difficult to form sufficient coordination with copper, so its ability to coat the active component is relatively weakened, and the copper ions partially migrate and agglomerate during calcination, and the particle size becomes larger.

[0114] Figure 3 The HRTEM image and the corresponding mapping element analysis image of the copper-based low-temperature catalyst prepared in Example 1 of the present invention are shown. As can be seen from the HRTEM image (F), the copper-based low-temperature catalyst prepared in Example 1 of the present invention presents a loose and porous sheet structure, which has a large specific surface area and can provide a large amount of reaction area, and the active metal copper particles can be highly dispersed on the organic carbon carrier, which is consistent with its high hydrogen production rate effect. Figure 3(B), (C), (D), and (E) correspond to the distribution diagrams of Cu, N, O, and C. These elements are evenly distributed on the catalyst, especially metallic copper, which is highly dispersed on the catalyst.

[0115] Figure 4 This is a transmission electron microscope image of copper particles in the copper-based low-temperature catalyst prepared in Example 1 of the present invention. Figure 5 This is a statistical diagram of the particle size of copper particles in the copper-based low-temperature catalyst prepared in Example 1 of the present invention. Figures 4-5 It can be seen that in the copper-based low-temperature catalyst provided in Example 1, copper nanoparticles with a particle size of 11-12 nm are the main active components. The distribution of active metal copper nanoparticles in this particle size range is the most uniform and is not easy to precipitate or sinter.

[0116] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing a copper-based low-temperature catalyst, characterized in that: The specific steps include: S1. mixing a copper salt solution, citric acid and valine in a molar ratio of copper in the copper salt solution: citric acid: valine = 1.4: (0.8-1.2): (0.1-0.5) and reacting them sufficiently to obtain a Cu-CA-Val complex; S2. calcining the Cu-CA-Val complex obtained in step S1 in an inert gas atmosphere at 270°C to 350°C for 1 to 4 hours to obtain a copper-based low-temperature catalyst precursor; S3. The copper-based low-temperature catalyst precursor obtained in step S2 is placed in a hydrogen atmosphere for reduction to obtain a copper-based low-temperature catalyst.

2. The method for preparing a copper-based low-temperature catalyst according to claim 1, characterized in that: In the step S1, the molar ratio of copper in the copper salt solution to citric acid and valine is 1.4:(0.9-1.1):(0.2-0.4).

3. The method for preparing a copper-based low-temperature catalyst according to claim 1, characterized in that: The calcination time in step S2 is 2 to 3.5 hours.

4. A copper-based low-temperature catalyst prepared by the method for preparing a copper-based low-temperature catalyst according to any one of claims 1 to 3.

5. The copper-based low-temperature catalyst according to claim 4, characterized in that: The mass loading of copper in the copper-based low-temperature catalyst is 48-60%.

6. The copper-based low-temperature catalyst according to claim 5, characterized in that: The mass loading amount of copper in the copper-based low-temperature catalyst is 55-58%.

7. The copper-based low-temperature catalyst according to claim 5, characterized in that: In the copper-based low-temperature catalyst, copper particles with a particle size of 8 to 13 nm account for 82 to 90% of all copper particles.

8. Use of the copper-based low-temperature catalyst according to any one of claims 4 to 7 in catalytic methanol reforming to produce hydrogen at 180°C.

Citation Information

Patent Citations

  • Preparation method of mesoporous carbon loaded nano platinum catalyst

    CN113659160A

  • Nitrogen-doped carbon-coated copper catalyst as well as preparation method and application thereof