Preparation method of nylon-polyester sheath-core composite fiber and super black fabric made therefrom

Through the composite spinning technology of cationic modified polyester and PA6, combined with special dyeing and finishing processes, the problem of difficult dyeing of nylon-polyester-skin-core composite fiber fabrics into deep black has been solved, the preparation of super black fabrics has been achieved, and the wear resistance of the fabrics has been improved. Sexy and cooling properties, suitable for high-end clothing.

CN116623313BActive Publication Date: 2024-10-11HAIXI NEW TEXTILE MATERIAL OF JINJIANG IND TECH ACAD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310526747.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-10-11
Estimated Expiration
2043-05-11

AI Technical Summary

Technical Problem

Conventional nylon-polyester sheath-core composite fiber fabrics are difficult to achieve a deep black effect when dyed in super black, and there are problems with electrostatic dust sticking and poor abrasion resistance.

Method used

Cationic modified polyester chips are mixed with black pigments and dispersing additives and then extruded by a single screw to form a cationic modified polyester black masterbatch, which is mixed with white cationic modified polyester chips and then compounded with PA6 chips. Spinning to form polyester, nylon, sheath and core composite fibers, super black fabrics are produced through special dyeing and finishing processes.

Benefits of technology

It achieves the super black appearance of the fabric, improves the wear resistance and cooling performance, solves the problem of electrostatic dust absorption, and has the characteristics of softness, skin-friendly, stiffness and dust-proofing, and is suitable for mid-to-high-end clothing fields.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of textile fabrics, and specifically discloses a method for preparing a nylon-polyester core-skin composite fiber and a super black fabric made thereof. The nylon-polyester core-skin composite fiber adopts a deep black core material of cationic polyester, and is spun with the original white PA6 of the epidermis for core-skin structure composite spinning, which greatly reduces the direct penetration of light on the fiber, and superimposes a special process of masterbatch and slice mixing method and nylon dyeing combination, which greatly improves the black depth of the fabric, overcomes the technical difficulty of the core-skin structure fiber fabric being difficult to dye deep black, and realizes the super black appearance of the fabric, which has broad application prospects in the fields of mid-to-high-end school uniforms, sports brand clothing, men's business casual trousers, women's fashion, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textile fabrics, and in particular to a method for preparing a nylon-polyester sheath-core composite fiber and a super black fabric prepared thereby. Background Art

[0002] Nylon-polyester skin-core composite fiber fabric has a wide range of application prospects in the fields of men's trousers, women's fashion, etc. because of its good appearance, touch and cool feeling, soft and delicate, good skin-friendly feeling, bright colors, excellent wear resistance, good heat setting, crisp and flat, good rebound and other advantages. Among them, super black nylon-polyester skin-core composite fiber fabric is favored by market consumers. However, the conventional nylon-polyester skin-core composite fiber has a white nylon fiber surface layer and a white polyester fiber core layer. When the fabric is super black dyed, it is difficult for the black dye to penetrate into the core layer, and the fabric can only achieve the effect of medium black. The general treatment method is to use a super black dyeing material with a high dyeing rate and increase the use of super black dyeing materials. However, the super black nylon-polyester skin-core composite fiber fabric obtained by this method has the disadvantages of electrostatic dust adhesion, poor wear resistance and poor cool effect, which is difficult to be recognized by the market. Therefore, it is particularly important to study and develop a nylon-polyester skin-core composite fiber that can be used to prepare super black fabrics. Summary of the invention

[0003] In view of the deficiencies in the prior art, the technical problem to be solved by the present invention is to provide a method for preparing a nylon-polyester sheath-core composite fiber and a super black fabric made therefrom, which overcomes the technical difficulty that conventional nylon-polyester sheath-core structure fiber fabrics are difficult to dye dark black and can achieve a super black appearance of the fabric.

[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0005] The preparation method of nylon-polyester sheath-core composite fiber specifically comprises the following steps:

[0006] Step 1: After drying, the white cationic modified polyester chips are added into a mixer together with black pigment and dispersing aid to be completely mixed, and then enter a single screw extruder to melt blend and granulate to obtain a cationic modified polyester black masterbatch;

[0007] Step 2: Add the white cationic modified polyester chips and the cationic modified polyester black masterbatch obtained in step 1 into a mixer and mix them completely to obtain black and white cationic modified polyester mixture chips;

[0008] Step 3: Dry the matt white PA6 slices and the black and white cationic modified polyester mixture slices obtained in step 2 separately, use them as the sheath and core layers respectively, and obtain polyester-nylon sheath-core composite fiber filaments through a composite spinning process.

[0009] Preferably, in the step 1, the mass percentage of the white cationic modified polyester chips, the black pigment and the dispersing aid is in the range of 7-9:0.7-2:0.3-1, and the total of the three is 100%.

[0010] Preferably, the black pigment in step 1 is carbon black, and the average particle size of the carbon black is 10nm-70nm.

[0011] Preferably, the dispersing aid in step 1 is one or more of polyethylene wax, ethylene bisstearamide, oleamide, erucamide, stearic acid and zinc stearate.

[0012] Preferably, in the step 2, the mass percentage range of the white cationic modified polyester chips and the cationic modified polyester black masterbatch is 4-6:6-4, and the sum of the two is 100%.

[0013] Preferably, the mass percentage of the fully matte white PA6 slices obtained in step 3 and the black and white cationic modified polyester mixture slices obtained in step 2 is in the range of 4-6:6-4, and the sum of the two is 100%.

[0014] The present invention also provides a super black fabric, which is woven and dyed into a super pure black fabric by knitting technology using nylon-polyester sheath-core composite fiber filaments and nylon-spandex core-wrapped original white filaments, wherein: the nylon-polyester sheath-core composite fiber filaments are the nylon-polyester sheath-core composite fiber filaments as claimed in claim 1, and the dyeing in the dyeing and finishing process uses black acid dye to dye the nylon material of the nylon-polyester sheath-core composite fiber surface and the nylon material of the nylon-spandex core-wrapped filaments.

[0015] Preferably, the nylon-spandex core-spun filament is a 33dtex / 25f-55dtex / 37f fully matte core-spun filament, and the nylon-polyester sheath-core composite fiber filament is a 55dtex / 36f-110dtex / 72f fully matte DTY heavy mesh filament.

[0016] Preferably, the structure of the super pure black fabric is a double-sided variable structure and an imitation woven twill texture fabric structure.

[0017] Preferably, the dyeing and finishing process includes softening, moisture absorption, quick drying and antistatic one-bath finishing.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The fabric of the present invention utilizes nylon-polyester sheath-core fiber, which has both the excellent wearing properties of PA6 material and the good heat setting and crispness of modified polyester material, as well as the unique functional elements of medium elasticity and electrostatic comprehensive effect of composite fiber and the cool feeling performance of nylon material, forming an optimized combination of "nylon + polyester" dual wearing properties; in addition, by utilizing the principle of opposite polarity of friction electrostatic charge between nylon and polyester materials and combining with the addition of post-finishing antistatic additives, the technical problem of electrostatic dust absorption of the fabric is effectively solved, and the fabric as a whole meets the technical requirements of twill texture, antistatic, cool feeling, wear resistance and the like, and meets the functional label mark requirements for ready-made clothing.

[0020] The super black effect of the fabric of the present invention is achieved by developing and producing a deep black core material of cationic polyester with added masterbatch, and spinning the core-skin structure with the original white full-dull PA6 of the skin layer into a fiber, which can greatly reduce the direct penetration ability of light on the fiber; when the composite fiber is dyed super black, the demand for acid dyes and the technical requirements for high dyeing rate are greatly reduced, and the color fastness of the fabric is also improved.

[0021] The present invention combines a special process of superimposing masterbatch with a slice mixing method and nylon dyeing to greatly improve the black depth of the fabric, overcome the technical difficulty of skin-core structure fiber fabric being difficult to dye dark black, and achieve a super black appearance effect of the fabric.

[0022] The fabric of the invention has the advantages of being soft and skin-friendly, wear-resistant, crisp, good in shaping, low in static electricity, dust-resistant, cool, etc., and has broad application prospects in the fields of mid- to high-end school uniforms, sports brand clothing, men's business casual trousers, women's fashion, etc. DETAILED DESCRIPTION

[0023] Example 1

[0024] This embodiment provides a method for preparing a nylon-polyester sheath-core composite fiber, which specifically includes the following steps:

[0025] Step 1: After drying the white cationic modified polyester chips, add them into a mixer together with carbon black, polyethylene wax and zinc stearate with an average particle size of 10nm-70nm, and mix them thoroughly. The mass percentage of the three is 9:0.7:0.3. Enter the single-screw extruder, melt-blend and granulate at 260℃-280℃ to obtain a cationic modified polyester black masterbatch.

[0026] Step 2: Add the white cationic modified polyester chips and the cationic modified polyester black masterbatch obtained in step 1 into a mixer and mix them completely, with the mass percentage of the two being 6:4, to obtain black and white cationic modified polyester mixture chips.

[0027] Step three: Dry the matt white PA6 slices and the black and white cationic modified polyester mixture slices obtained in step two separately, with the mass percentage of the two being 6:4, and use them as the sheath and core layers respectively, and obtain polyester-nylon sheath-core composite fiber filaments through the same-circular sheath-core composite spinning process.

[0028] Example 2

[0029] This embodiment provides a method for preparing a nylon-polyester sheath-core composite fiber, which specifically includes the following steps:

[0030] Step 1: After drying the white cationic modified polyester chips, add them into a mixer together with carbon black, ethylene bisstearamide and stearic acid with an average particle size of 10nm-70nm and mix them thoroughly. The mass percentage of the three is 8:1.5:0.5. Enter the single-screw extruder, melt-blend and granulate at 260℃-280℃ to obtain a cationic modified polyester black masterbatch.

[0031] Step 2: Add the white cationic modified polyester chips and the cationic modified polyester black masterbatch obtained in step 1 into a mixer and mix them completely, with the mass percentage of the two being 4:6, to obtain black and white cationic modified polyester mixture chips.

[0032] Step three: Dry the white PA6 slices and the black and white cationic modified polyester mixture slices obtained in step two separately, with the mass percentage of the two being 5:5, and use them as the sheath and core layers respectively, and obtain polyester-nylon sheath-core composite fiber filaments through the same-circular sheath-core composite spinning process.

[0033] Example 3

[0034] This embodiment provides a method for preparing a nylon-polyester sheath-core composite fiber, which specifically includes the following steps:

[0035] Step 1: After drying the white cationic modified polyester chips, add them into a mixer together with carbon black, polyethylene wax, stearic acid and zinc stearate with an average particle size of 10nm-70nm, and mix them thoroughly. The mass percentage of the three is 7:2:1. Enter the single-screw extruder, melt-blend and granulate at 260℃-280℃ to obtain a cationic modified polyester black masterbatch.

[0036] Step 2: Add the white cationic modified polyester chips and the cationic modified polyester black masterbatch obtained in step 1 into a mixer and mix them completely in a mass percentage range of 5:5 to obtain black and white cationic modified polyester mixture chips.

[0037] Step three: Dry the white PA6 slices and the black and white cationic modified polyester mixture slices obtained in step two separately, with the mass percentage of the two being 4:6, and use them as the sheath and core layers respectively. Through the same-circular sheath-core composite spinning process, polyester-nylon sheath-core composite fiber filaments are obtained.

[0038] Example 4

[0039] The present embodiment provides a super black fabric, which is made of nylon-polyester sheath-core composite fiber filaments and nylon-spandex core-covered original white filaments, which are woven by weft-knitted large circular machines to form double-sided jacquard structure and imitation woven twill texture fabric, and are processed into pure black fabric through dyeing and finishing, wherein: the nylon-polyester sheath-core composite fiber filaments are the nylon-polyester sheath-core composite fiber filaments prepared in Example 1, with a specification of 55dtex / 36f; the nylon-spandex core-covered original white filaments have a specification of 55dtex / 37f.

[0040] Weaving adopts weft knitting circular machine, 34 ” , double needle cylinder, needle number 36G, total number of needles 3840, jacquard twill structure, the designed weight of the grey fabric is 260 g / m2, and the lower width is 135 cm.

[0041] The dyeing and finishing process includes open-width washing, high-temperature initial shaping of grey cloth, single dyeing of nylon with acid dyes, and functional finishing. The functional finishing adopts soft, moisture-absorbing, quick-drying, and antistatic one-bath shaping finishing.

[0042] Specifically: the initial high-temperature setting temperature of the grey cloth is 195°C, the machine speed is 23 meters / minute, the initial weight is 210 grams / meter, and the width is 160 centimeters; PA6 is dyed with black acid dye, the dyeing temperature is 98°C, and the dyeing time is 50 minutes; the post-finishing adopts soft + moisture absorption and quick drying + antistatic one-bath setting finishing, of which the amount of R-3 type moisture absorption finishing agent is 15 grams / liter, the hydrophilic softener is 10 grams / liter, and the KB-1 type antistatic finishing agent is 20 grams / liter. The setting temperature is 135°C, the machine speed is 26 meters / minute, and the weight of the finished fabric off the machine is 200 grams / square meter and the width is 162 centimeters.

[0043] Example 5

[0044] The present embodiment provides a super black fabric, which is made of nylon-polyester sheath-core composite fiber filaments and nylon-spandex core-covered original white filaments, which are woven by weft-knitted large circular machines to form double-sided jacquard structure and imitation woven twill texture fabric, and are processed into pure black fabric through dyeing and finishing, wherein: the nylon-polyester sheath-core composite fiber filaments are the nylon-polyester sheath-core composite fiber filaments prepared by Example 3, with a specification of 55dtex / 36f; the nylon-spandex core-covered original white filaments have a specification of 55dtex / 37f.

[0045] Weaving adopts weft knitting circular machine, 34 ”, double needle cylinder, needle number 36G, total number of needles 3840, jacquard twill structure, the designed weight of the grey fabric is 260 g / m2, and the lower width is 135 cm.

[0046] The dyeing and finishing process includes open-width washing, high-temperature initial shaping of grey cloth, single dyeing of nylon with acid dyes, and functional finishing. The functional finishing adopts soft, moisture-absorbing, quick-drying, and antistatic one-bath shaping finishing.

[0047] Specifically: the initial high-temperature setting temperature of the grey cloth is 195°C, the machine speed is 23 meters / minute, the initial weight is 210 grams / meter, and the width is 160 centimeters; PA6 is dyed with black acid dye, the dyeing temperature is 98°C, and the dyeing time is 50 minutes; the post-finishing adopts soft + moisture absorption and quick drying + antistatic one-bath setting finishing, of which the amount of R-3 type moisture absorption finishing agent is 15 grams / liter, the hydrophilic softener is 10 grams / liter, and the KB-1 type antistatic finishing agent is 20 grams / liter. The setting temperature is 135°C, the machine speed is 26 meters / minute, and the weight of the finished fabric off the machine is 200 grams / square meter and the width is 162 centimeters.

[0048] Comparative Example 1

[0049] The difference between this comparative example and the above-mentioned Example 5 is that the core layer of the nylon-polyester core-skin composite fiber is the original white cationic modified polyester fiber. The dyes used in Examples 4 and 5 and Comparative Example 1 are the same.

[0050] The super black fabrics prepared in the above-mentioned Examples 4-5 and Comparative Example 1 were tested for moisture absorption and quick drying, antistatic, cool feeling and blackness. According to GB / T 21655.1-2008, the moisture absorption and quick drying performance of the three fabrics were comparable, the water absorption rate was greater than 200%, and the moisture permeability was 10000 g / (m 2 •d) and above, the diffusion time of dripping water is within 3s; the antistatic performance level of the three fabrics is equivalent to that of GB / T12703.3-2009, and the charge is not more than 0.5μC / piece; the contact coolness coefficient q of the three fabrics is measured according to GB / T35263-2017 -max Both are between 0.18-0.21 J / (cm 2 ·s).

[0051] However, according to the Pantone color card, the black color number of Example 4 is 19-0303 TCX Super Black, the black color number of Example 5 is 19-4203TCX Super Black, and the black color number of Comparative Example 1 is 19-3907 TCX Medium Black. The blackness of Comparative Example 1 is obviously inferior to that of Examples 4 and 5.

[0052] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which shall fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing super black brocade polyester core-skin composite fiber filament, characterized in that: The specific steps include: Step 1: After drying, the white cationic modified polyester chips are added into a mixer together with black pigment and dispersing aid to be completely mixed, and then enter a single screw extruder to melt blend and granulate to obtain a cationic modified polyester black masterbatch; Step 2: Add the white cationic modified polyester chips and the cationic modified polyester black masterbatch obtained in step 1 into a mixer and mix them completely to obtain black and white cationic modified polyester mixture chips; Step 3: Dry the matt white PA6 slices and the black and white cationic modified polyester mixture slices obtained in step 2, respectively, and use them as the skin layer and the core layer, respectively, and obtain the polyamide-polyester skin-core composite fiber filament through a composite spinning process; The nylon material of the nylon-polyester skin-core composite fiber surface is dyed with black acid dye to obtain super black nylon-polyester skin-core composite fiber filament; In the step 1, the mass percentage of the white cationic modified polyester chips, the black pigment and the dispersing aid is in the range of 7-9:0.7-2:0.3-1; The black pigment in step 1 is carbon black, and the average particle size of the carbon black is 10nm-70nm; In the step 2, the mass percentage range of the white cationic modified polyester chips and the cationic modified polyester black masterbatch is 4-6:6-4; The mass percentage range of the fully matte white PA6 slices obtained in step 3 and the black and white cationic modified polyester mixture slices obtained in step 2 is 4-6:6-4.

2. The method for preparing super black nylon-polyester core-skin composite fiber filament according to claim 1, characterized in that: The dispersing aid in step 1 is one or more of polyethylene wax, ethylene bis stearamide, oleamide, erucamide, stearic acid and zinc stearate. 3.Super black fabric, characterized by: The super pure black fabric is made of nylon-polyester core-skin composite fiber filament and nylon-spandex core-skinned original white filament through knitting process and dyeing and finishing. The dyeing in the dyeing and finishing process uses black acid dye to dye the nylon material of the nylon-polyester core-skin composite fiber surface and the nylon material of the nylon-spandex core-skinned filament; The method for preparing the nylon-polyester sheath-core composite fiber filament specifically comprises the following steps: Step 1: After drying, the white cationic modified polyester chips are added into a mixer together with black pigment and dispersing aid to be completely mixed, and then enter a single screw extruder to melt blend and granulate to obtain a cationic modified polyester black masterbatch; Step 2: Add the white cationic modified polyester chips and the cationic modified polyester black masterbatch obtained in step 1 into a mixer and mix them completely to obtain black and white cationic modified polyester mixture chips; Step 3: Dry the matt white PA6 slices and the black and white cationic modified polyester mixture slices obtained in step 2, respectively, and use them as the skin layer and the core layer, respectively, and obtain the polyamide-polyester skin-core composite fiber filament through a composite spinning process; In the step 1, the mass percentage of the white cationic modified polyester chips, the black pigment and the dispersing aid is in the range of 7-9:0.7-2:0.3-1; The black pigment in step 1 is carbon black, and the average particle size of the carbon black is 10nm-70nm; In the step 2, the mass percentage range of the white cationic modified polyester chips and the cationic modified polyester black masterbatch is 4-6:6-4; The mass percentage range of the fully matte white PA6 slices obtained in step 3 and the black and white cationic modified polyester mixture slices obtained in step 2 is 4-6:6-4.

4. The super black fabric according to claim 3, characterized in that: The nylon-spandex core-spun filament is a fully matte core-spun filament.

5. The super black fabric according to claim 3, characterized in that: The structure of the super pure black fabric is a double-sided variable structure and an imitation woven twill texture fabric structure.

6. The super black fabric according to claim 3, characterized in that: The dyeing and finishing process includes soft, moisture-absorbing, quick-drying and antistatic one-bath finishing.