A method for preparing alumina slurry and application of the prepared alumina slurry in preparing green porcelain sheets
Through three ball milling processes and appropriate organic solvent treatment, the problems of long time preparation of alumina slurry and uneven particle dispersion are solved, the uniform dispersion of alumina particles and the stability of sintering shrinkage are achieved, and the production of electronic ceramics is improved. efficiency and product quality.
Patent Information
- Application Number
- CN202310567677.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-04-21
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-04-21
AI Technical Summary
The existing alumina slurry preparation process is time-consuming and the alumina particles are unevenly dispersed, resulting in unstable shrinkage of green ceramic tiles after sintering, affecting the performance and production efficiency of electronic ceramics.
Using three ball milling processes, alumina powder, additive powder, molybdenum powder solution and acrylic adhesive are added respectively. By monitoring the particle size, the alumina particles are evenly dispersed, the ball milling time is reduced, and the water content of the organic solvent is controlled to avoid gelation. phenomenon.
Alumina particles are uniformly dispersed in a short period of time, stable particle size distribution and sintering shrinkage are obtained, and production efficiency and product quality are improved.
Smart Images

Figure BDA0004237245210000081
Abstract
Description
[0001] The present invention is a divisional application of a Chinese invention patent application with an application date of April 21, 2022, application number 2022104231512, and name “A method for preparing alumina slurry and the prepared alumina slurry”. Technical Field
[0002] The invention relates to the field of electronic ceramics, in particular to raw materials for preparing green ceramic sheets used in electronic ceramics, and specifically to a method for preparing alumina slurry and application of the prepared alumina slurry in preparing green ceramic sheets. Background Art
[0003] Electronic ceramics refer to ceramics that can use electrical and magnetic properties in the electronics industry. Electronic ceramics are ceramics with new functions that are obtained through precise control of the surface, grain boundaries and size structure. They can be widely used in energy, household appliances, automobiles, etc.
[0004] Electronic ceramics can usually be made by sintering raw ceramic sheets after a series of treatments. At present, the raw material used for the preparation of raw ceramic sheets used in electronic ceramics is mostly alumina slurry. The alumina slurry is mixed evenly and then vacuum degassed. After the bubbles in the slurry are removed, it enters a tape casting machine to cast raw ceramics, and is cut into sheets according to a certain size. Among them, the difficulty, time consumption, and performance of the alumina slurry preparation determine the performance and cost-effectiveness of the raw ceramics and even the subsequent electronic ceramics to a certain extent. Since alumina particles are easy to agglomerate or soft to agglomerate, a ball mill is generally used for ball milling dispersion. However, the current alumina slurry preparation process basically requires a long time of ball milling to make the alumina particles evenly dispersed, resulting in a long production process and is not conducive to large-scale production. At the same time, the current raw ceramic sheets cast from the alumina slurry still have large shrinkage changes and unstable shrinkage after sintering into electronic ceramics. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a new method for preparing alumina slurry, which can achieve uniform dispersion of alumina slurry in a relatively short time, effectively disperse the particle aggregates in the system that are in a state of agglomeration or soft agglomeration, and obtain an ideal particle size distribution state, which is beneficial to the sintering shrinkage of electronic ceramics that is stable and controllable.
[0006] To achieve the above object, a technical solution adopted by the present invention is: a method for preparing alumina slurry, the preparation method comprising the following steps:
[0007] (1) adding aluminum oxide powder, auxiliary agent powder, molybdenum powder solution and a first organic solvent into a ball mill respectively to perform a first ball milling;
[0008] (2) adding a portion of the acrylic binder to the ball mill for a second ball milling, and monitoring the particle size of the particles in the slurry during the ball milling process;
[0009] (3) when it is monitored that the particle size reaches a preset value, the second ball milling is stopped, the remaining acrylic binder and plasticizer are added, and the third ball milling is performed to obtain an alumina slurry;
[0010] Wherein, in terms of mass percentage, the portion of acrylic adhesive in step (2) accounts for 0.5%-5% of the total amount of acrylic adhesive added, and the portion of acrylic adhesive in step (2) accounts for 0.05%-2% of the amount of aluminum oxide powder added, and the time used for the second ball milling accounts for more than 75% of the total ball milling time of the first ball milling, the second ball milling and the third ball milling.
[0011] According to some preferred aspects of the present invention, the part of the acrylic adhesive in step (2) accounts for 1%-4% of the total amount of acrylic adhesive added, by mass percentage. In some embodiments of the present invention, the part of the acrylic adhesive in step (2) accounts for 1%-2% of the total amount of acrylic adhesive added, by mass percentage. In some embodiments of the present invention, the part of the acrylic adhesive in step (2) accounts for 2%-3% of the total amount of acrylic adhesive added, by mass percentage. In some embodiments of the present invention, the part of the acrylic adhesive in step (2) accounts for 3%-4% of the total amount of acrylic adhesive added, by mass percentage.
[0012] According to some preferred aspects of the present invention, the portion of the acrylic adhesive in step (2) accounts for 0.1%-1.5% of the amount of the aluminum oxide powder added, by mass percentage. In some embodiments of the present invention, the portion of the acrylic adhesive in step (2) accounts for 0.1%-0.5% of the amount of the aluminum oxide powder added, by mass percentage. In some embodiments of the present invention, the portion of the acrylic adhesive in step (2) accounts for 0.5%-1% of the amount of the aluminum oxide powder added, by mass percentage. In some embodiments of the present invention, the portion of the acrylic adhesive in step (2) accounts for 1%-1.5% of the amount of the aluminum oxide powder added, by mass percentage.
[0013] According to some preferred aspects of the present invention, the weight average molecular weight of the acrylic adhesive is 400,000-600,000, and the glass transition temperature is -10 to 30° C. More preferably, the weight average molecular weight of the acrylic adhesive is 450,000-550,000, and the glass transition temperature is 0-20° C.
[0014] According to a specific aspect of the present invention, the acrylic adhesive is KFA-440 of the corresponding chemistry.
[0015] According to some preferred aspects of the present invention, in the alumina slurry, by mass percentage, alumina powder accounts for 45%-60%, auxiliary powder accounts for 2%-8%, molybdenum powder solution accounts for 0.5%-5%, acrylic adhesive accounts for 8%-20%, plasticizer accounts for 0.05%-3%, and the first organic solvent accounts for 15%-40%.
[0016] Furthermore, in terms of mass percentage, in the alumina slurry, alumina powder accounts for 47%-58%, auxiliary powder accounts for 2%-7%, molybdenum powder solution accounts for 0.8%-3.5%, acrylic adhesive accounts for 10%-18%, plasticizer accounts for 0.1%-1.5%, and the first organic solvent accounts for 15%-38%.
[0017] The auxiliary powder in the present invention does not contain metal molybdenum powder.
[0018] According to some preferred aspects of the present invention, the auxiliary powder includes silicon dioxide, talc and chromium oxide.
[0019] According to some preferred aspects of the present invention, the mass ratio of the silicon dioxide, the talc and the chromium oxide is 4-5.5:1.5-3.5:1.
[0020] In some embodiments of the present invention, the auxiliary powder consists of silicon dioxide, talc and chromium oxide.
[0021] According to some preferred aspects of the present invention, the molybdenum powder solution is obtained by dispersing metallic molybdenum powder in a second organic solvent, with a mass fraction of 20-40%, and the second organic solvent may be isopropanol.
[0022] According to some preferred aspects of the present invention, the plasticizer may be dibutyl phthalate.
[0023] According to some preferred aspects of the present invention, the first organic solvent is an organic solvent that is incompatible with or insoluble in water. According to a specific and preferred aspect of the present invention, the first organic solvent may be toluene.
[0024] According to the present invention, the preset value is: D 50 1.9-2.5μm.
[0025] According to some preferred aspects of the present invention, the time used for the first ball milling accounts for 1%-5% of the total ball milling time of the first ball milling, the second ball milling and the third ball milling.
[0026] In some embodiments of the present invention, the time used for the first ball milling accounts for 2%-4% of the total ball milling time of the first ball milling, the second ball milling and the third ball milling.
[0027] Furthermore, the time used for the second ball milling accounts for more than 80% of the total ball milling time of the first ball milling, the second ball milling and the third ball milling.
[0028] In the present invention, in a large number of experimental practices, alumina slurry is very likely to gel in the initial mixing stage or during ball milling, causing difficulty in ball milling, and once formed, it is difficult to continue to be used as a slurry for the casting system, and raw porcelain cannot be prepared, resulting in a great increase in production costs. After the inventor combined experiments with production practices, it was analyzed that the gelation phenomenon may be caused by the presence of water in the system, but in practice, even if the powder raw materials such as alumina powder are subjected to a certain drying treatment, gelation still occurs to varying degrees in different batches. Later, the inventor unexpectedly discovered that when the organic solvent-based casting system uses other types of adhesives such as PVB (polyvinyl butyral), the occurrence of gelation is basically avoided when the powder raw materials such as alumina powder are subjected to a certain drying treatment. After comparison, it is analyzed that it may be that the present invention uses an acrylic adhesive, and the functional group carboxyl group contained therein should be able to form multiple hydrogen bonds with water, resulting in the system gelation phenomenon can occur and be more obvious when the moisture content is very low, but if the moisture needs to be completely removed, the dehydration operation will be time-consuming and energy-consuming, which is not conducive to reducing costs and improving production efficiency.
[0029] After continuous experiments and summaries, according to some preferred aspects of the present invention, in step (1), the water content of the alumina powder and the auxiliary agent powder is controlled to be lower than 0.75% before being added to the ball mill, which can basically control the occurrence of gelation, and the dehydration time and energy consumption are within a reasonable range.
[0030] Furthermore, in step (1), the water content of the alumina powder and the auxiliary agent powder is controlled to be less than 0.5% before being added into the ball mill.
[0031] In some embodiments of the present invention, the alumina powder and the auxiliary agent powder may be dried at a certain temperature (eg, 50-100° C.) until the water content meets the requirements.
[0032] In the present invention, the method of monitoring the particle size of particles in the slurry includes but is not limited to: stopping the operation of the equipment, sampling for particle size measurement, or real-time monitoring through online equipment; no specific details are given here.
[0033] Another technical solution provided by the present invention is: an alumina slurry prepared by the preparation method described above.
[0034] Another technical solution provided by the present invention is the use of the alumina slurry prepared by the above-mentioned preparation method in the preparation of green porcelain sheets.
[0035] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0036] The present invention is based on the problems that the existing alumina slurry preparation process is time-consuming and the shrinkage rate of the raw ceramic sheets cast from the alumina slurry varies greatly after being sintered into electronic ceramics. Based on a large number of experiments, the inventors found in practice that only a small amount of suitable acrylic adhesive is added to participate in the main ball milling process of alumina slurry preparation, and most of the acrylic adhesive and all the plasticizers are added last. This method not only successfully achieves uniform dispersion of the various components in the alumina slurry in a relatively short time, so that each particle including the alumina particles is separated from agglomeration or soft agglomeration, greatly saving time cost and being conducive to large-scale production and application, but also the processing ball milling method enables the particles to obtain a suitable and narrow particle size distribution state in a relatively short time, so that after the raw ceramic sheets made of the alumina slurry are sintered into electronic ceramics, the electronic ceramics can have a stable and controllable shrinkage rate, thereby ensuring stable product quality. DETAILED DESCRIPTION
[0037] The above scheme is further described below in conjunction with specific embodiments; it should be understood that these embodiments are used to illustrate the basic principles, main features and advantages of the present invention, and the present invention is not limited to the scope of the following embodiments; the implementation conditions adopted in the embodiments can be further adjusted according to specific requirements, and the implementation conditions not specified are usually the conditions in conventional experiments.
[0038] Unless otherwise specified in the following examples, all raw materials are commercially available or prepared by conventional methods in the art.
[0039] Alumina powder was purchased from Aluminium, brand AMB. 50 60-70μm;
[0040] Metallic molybdenum powder, silicon dioxide, talc, and chromium oxide are all commercially available, with a Fisher particle size between 1 and 2.3 microns;
[0041] Dibutyl phthalate was purchased from Dapeng Chemical with a purity of 99%;
[0042] The acrylic adhesive is KFA-440 from Huying Chemical;
[0043] D 50 Measured by Malvern 3000 laser particle size analyzer;
[0044] The ball mill is a commercially available 100kg (300L) ball mill lined with an alumina sleeve, and the operating parameters are: a rotation speed of 40±5r / min, alumina balls with a particle size of about 30mm, and a material-to-ball ratio (specifically, the mass ratio of the amount of alumina powder added to the total amount of alumina balls) controlled to be 1:1.
[0045] Example 1
[0046] This example provides an alumina slurry and a preparation method thereof. In terms of mass percentage, the alumina slurry includes the following components: 47% alumina powder, 4% auxiliary powder, 3% molybdenum powder solution, 12% acrylic adhesive, 0.3% plasticizer, and 33.7% toluene; wherein the auxiliary powder is composed of silicon dioxide, talcum powder, and chromium oxide, and the mass ratio of silicon dioxide, talcum powder, and chromium oxide is 5:3:1; the molybdenum powder solution is obtained by dispersing metal molybdenum powder in isopropanol, and its mass fraction is 30%.
[0047] The alumina powder and auxiliary agent powder weighed in proportion are dried in a drying room at a temperature of 80±10° C. until the water content is reduced to 0.75% and set aside.
[0048] The preparation method of the alumina slurry comprises the following steps:
[0049] Step 1: Put the dried alumina powder into the ball mill;
[0050] Step 2: Put the dried additive powder into the ball mill;
[0051] Step 3: Put isopropanol into a stainless steel barrel, then put metal molybdenum powder into the stainless steel barrel containing isopropanol, and stir evenly to obtain a molybdenum powder solution, and finally put the molybdenum powder solution into a ball mill;
[0052] Step 4: Put toluene into the ball mill;
[0053] Step 5: Cover the ball mill lid for the first ball milling. After running for 2 hours, stop, open the lid, put part of the acrylic adhesive into the ball mill, then cover the lid and start running the ball mill for the second ball milling. During the ball milling process, the particle size D 50 Monitoring was performed; wherein, some acrylic adhesives accounted for 1.5% of the total amount of acrylic adhesives added;
[0054] Step 6: When the particle size reaches the preset particle size value D 50 When the particle size is 1.9-2.5 μm, the second ball milling time is about 50 hours;
[0055] At the same time, when the particle size reaches the requirement, open the cover of the ball mill and put the remaining acrylic adhesive into the ball mill; then put dibutyl phthalate into the ball mill and run it for 5 hours to obtain alumina slurry.
[0056] No gelation occurs during the preparation process.
[0057] Example 2
[0058] This example provides an alumina slurry and a preparation method thereof. In terms of mass percentage, the alumina slurry includes the following components: 56% alumina powder, 5% auxiliary powder, 3% molybdenum powder solution, 15% acrylic adhesive, 0.8% plasticizer, and 20.2% toluene; wherein the auxiliary powder is composed of silicon dioxide, talcum powder, and chromium oxide, and the mass ratio of silicon dioxide, talcum powder, and chromium oxide is 5:3:1; the molybdenum powder solution is obtained by dispersing metal molybdenum powder in isopropanol, and its mass fraction is 30%.
[0059] The alumina powder and auxiliary agent powder weighed in proportion are dried in a drying room at a temperature of 80±10° C. until the water content is reduced to 0.75% and set aside.
[0060] The preparation method of the alumina slurry comprises the following steps:
[0061] Step 1: Put the dried alumina powder into the ball mill;
[0062] Step 2: Put the dried additive powder into the ball mill;
[0063] Step 3: Put isopropanol into a stainless steel barrel, then put metal molybdenum powder into the stainless steel barrel containing isopropanol, and stir evenly to obtain a molybdenum powder solution, and finally put the molybdenum powder solution into a ball mill;
[0064] Step 4: Put toluene into the ball mill;
[0065] Step 5: Cover the ball mill lid for the first ball milling. After running for 2 hours, stop, open the lid, put part of the acrylic adhesive into the ball mill, then cover the lid and start running the ball mill for the second ball milling. During the ball milling process, the particle size D 50 Monitoring was performed; among them, some acrylic adhesives accounted for 3% of the total amount of acrylic adhesives added;
[0066] Step 6: When the particle size reaches the preset particle size value D 50 When the particle size is 1.9-2.5 μm, the second ball milling time is about 60 hours;
[0067] At the same time, when the particle size reaches the requirement, open the cover of the ball mill and put the remaining acrylic adhesive into the ball mill; then put dibutyl phthalate into the ball mill and run it for 5 hours to obtain alumina slurry.
[0068] No gelation occurs during the preparation process.
[0069] Example 3
[0070] This example provides an alumina slurry and a preparation method thereof. In terms of mass percentage, the alumina slurry includes the following components: 51% alumina powder, 4.5% auxiliary powder, 3% molybdenum powder solution, 12% acrylic adhesive, 1% plasticizer, and 28.5% toluene; wherein the auxiliary powder is composed of silicon dioxide, talcum powder, and chromium oxide, and the mass ratio of silicon dioxide, talcum powder, and chromium oxide is 5:3:1; the molybdenum powder solution is obtained by dispersing metal molybdenum powder in isopropanol, and its mass fraction is 30%.
[0071] The alumina powder and auxiliary agent powder weighed in proportion are dried in a drying room at a temperature of 80±10° C. until the water content is reduced to 0.75% and set aside.
[0072] The preparation method of the alumina slurry comprises the following steps:
[0073] Step 1: Put the dried alumina powder into the ball mill;
[0074] Step 2: Put the dried additive powder into the ball mill;
[0075] Step 3: Put isopropanol into a stainless steel barrel, then put metal molybdenum powder into the stainless steel barrel containing isopropanol, and stir evenly to obtain a molybdenum powder solution, and finally put the molybdenum powder solution into a ball mill;
[0076] Step 4: Put toluene into the ball mill;
[0077] Step 5: Cover the ball mill lid for the first ball milling. After running for 2 hours, stop, open the lid, put part of the acrylic adhesive into the ball mill, then cover the lid and start running the ball mill for the second ball milling. During the ball milling process, the particle size D 50 Monitoring was performed; among them, some acrylic adhesives accounted for 4% of the total amount of acrylic adhesives added;
[0078] Step 6: When the particle size reaches the preset particle size value D 50 When the particle size is 1.9-2.5 μm, the second ball milling time is about 65 hours;
[0079] At the same time, when the particle size reaches the requirement, open the cover of the ball mill and put the remaining acrylic adhesive into the ball mill; then put dibutyl phthalate into the ball mill and run it for 5 hours to obtain alumina slurry.
[0080] No gelation occurs during the preparation process.
[0081] Comparative Example 1
[0082] The method is basically the same as Example 1, except that the preparation process is different. The specific preparation process is as follows:
[0083] All the components of the alumina slurry are mixed at once, and then added to the ball mill for ball milling. During the ball milling process, the particle size of the particles in the slurry is adjusted. 50 Monitor and when the particle size reaches the preset value D 50 When the particle size was 1.9 to 2.5 μm, alumina slurry was obtained and the ball milling time was about 150 hours.
[0084] Comparative Example 2
[0085] The method is basically the same as Example 1, except that the preparation process is different. The specific preparation process is as follows:
[0086] All components in the alumina slurry are mixed at one time, and then added into a ball mill for ball milling. The ball milling time is the same as the total ball milling time in Example 1 to obtain alumina slurry.
[0087] Comparative Example 3
[0088] The same as Example 1, except that the preparation process is different, specifically, in the fifth step, no acrylic adhesive is added, and other components except acrylic adhesive and dibutyl phthalate are directly mixed and milled. After 200 hours of ball milling, it is still difficult to reach the preset particle size D 50 The particle size is 1.9-2.5 μm, and at this time, the alumina powder in the ball mill presents relatively large agglomerates, making it difficult to measure the particle size.
[0089] Performance Testing
[0090] The alumina slurries obtained in the above Examples 1-3 and Comparative Examples 1-2 are first made into green ceramic sheets, which are then sintered into electronic ceramics, and some performance tests are performed on them. See Table 1 for specific results.
[0091] 1. Mix the alumina slurry evenly and then perform vacuum degassing to remove the bubbles in the slurry. Then, the slurry is fed into a tape casting machine to cast green porcelain. The green porcelain sheets are cut into sheets according to a certain size.
[0092] The four temperature zones of the casting machine are: 75±10℃, 95±10℃, 120±10℃, 130±10℃;
[0093] A green porcelain with a thickness of 0.4 mm was cast and cut into a 60 mm*80 mm (Y*X) test piece.
[0094] X direction: refers to the casting direction; Y direction: refers to the direction perpendicular to the casting direction.
[0095] 2. The green ceramic pieces obtained above were sintered at 1600°C for 20 hours to form ceramics and then the shrinkage rate was measured. The shrinkage rate was measured using a tool microscope produced by Guangdong Wanhao Precision Instrument Co., Ltd., model: VTM-4030F:
[0096] Shrinkage rate = 1-(size after sintering / size before sintering);
[0097] The required shrinkage specifications are as follows:
[0098] Shrinkage in X direction: 15.9%, tolerance 0.2%; Shrinkage in Y direction: 16.3%, tolerance 0.2%;
[0099] The shrinkage rate difference (shrinkage rate in the Y direction - shrinkage rate in the X direction) is 0.4%, and the tolerance is 0.15%. Note: Controlling the appropriate shrinkage rate difference can facilitate the size adjustment of the device during sintering. If it is too close, it is difficult to effectively adjust the size.
[0100] Table 1
[0101]
[0102] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
[0103] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A method for preparing alumina slurry, characterized in that: The method includes: (1) adding aluminum oxide powder, auxiliary agent powder, molybdenum powder solution and a first organic solvent into a ball mill respectively to perform a first ball milling; the auxiliary agent powder comprises silicon dioxide, talcum powder and chromium oxide, and the water content of the aluminum oxide powder and the auxiliary agent powder before adding into the ball mill is controlled to be less than 0.75% respectively; (2) adding a portion of the acrylic binder to the ball mill for a second ball milling, and monitoring the particle size of the particles in the slurry during the ball milling process; (3) when it is monitored that the particle size reaches a preset value, the second ball milling is stopped, the remaining acrylic binder and plasticizer are added, and the third ball milling is performed to obtain an alumina slurry; Wherein, in terms of mass percentage, the portion of acrylic adhesive in step (2) accounts for 0.5%-5% of the total amount of acrylic adhesive added, and the portion of acrylic adhesive in step (2) accounts for 0.05%-2% of the amount of aluminum oxide powder added, the time used for the second ball milling accounts for more than 75% of the total ball milling time of the first ball milling, the second ball milling and the third ball milling, and the time used for the first ball milling accounts for 1%-5% of the total ball milling time of the first ball milling, the second ball milling and the third ball milling.
2. The method for preparing alumina slurry according to claim 1, characterized in that: The water contents of the alumina powder and the auxiliary powder are controlled to be lower than 0.5% before being added into the ball mill; the time used for the second ball milling accounts for more than 80% of the total ball milling time of the first ball milling, the second ball milling and the third ball milling.
3. The method for preparing alumina slurry according to claim 1, characterized in that: Before adding the alumina powder and the auxiliary powder into the ball mill, the alumina powder and the auxiliary powder are dried at 50-100° C. until the water content meets the requirement.
4. The method for preparing alumina slurry according to claim 1, characterized in that: In terms of mass percentage, the portion of acrylic adhesive in step (2) accounts for 1%-4% of the total amount of acrylic adhesive added; the weight average molecular weight of the acrylic adhesive is 400,000-600,000, and the glass transition temperature is -10 to 30°C; in terms of mass percentage, the portion of acrylic adhesive in step (2) accounts for 0.1%-1.5% of the amount of aluminum oxide powder added.
5. The method for preparing alumina slurry according to claim 4, characterized in that: In terms of mass percentage, the acrylic adhesive in step (2) accounts for 1.5%-4% of the total amount of acrylic adhesive added; the weight average molecular weight of the acrylic adhesive is 450,000-550,000, and the glass transition temperature is 0-20°C; in terms of mass percentage, the acrylic adhesive in step (2) accounts for 0.1%-1% of the amount of aluminum oxide powder added.
6. The method for preparing alumina slurry according to claim 1, characterized in that: In terms of mass percentage, in the alumina slurry, alumina powder accounts for 45%-60%, auxiliary powder accounts for 2%-8%, molybdenum powder solution accounts for 0.5%-5%, acrylic adhesive accounts for 8%-20%, plasticizer accounts for 0.05%-3%, and the first organic solvent accounts for 15%-40%; The plasticizer is dibutyl phthalate, and the first organic solvent is toluene; the mass ratio of the silicon dioxide, the talc and the chromium oxide is 4-5.5:1.5-3.5:1; the molybdenum powder solution is obtained by dispersing metallic molybdenum powder in a second organic solvent, and its mass fraction is 20%-40%, and the second organic solvent is isopropanol.
7. The method for preparing alumina slurry according to claim 6, characterized in that: In terms of mass percentage, in the alumina slurry, alumina powder accounts for 47%-58%, auxiliary powder accounts for 2%-7%, molybdenum powder solution accounts for 0.8%-3.5%, acrylic adhesive accounts for 10%-18%, plasticizer accounts for 0.1%-1.5%, and the first organic solvent accounts for 15%-38%. The acrylic adhesive is KFA-440 of Mutual Chemical, and the auxiliary powder is composed of silicon dioxide, talc and chromium oxide, and the Fisher particle size is between 1-2.3μm.
8. The method for preparing alumina slurry according to claim 1, 6 or 7, characterized in that: The D of the alumina powder 50 is 60-70μm, and the preset value is: D 50 1.9-2.5μm.
9. The method for preparing alumina slurry according to claim 1, characterized in that: The implementation method of step (1) and step (2) includes: Put the dried alumina powder into the ball mill; Put the dried additive powder into the ball mill; Put isopropanol into a stainless steel barrel, then put metal molybdenum powder into the stainless steel barrel containing isopropanol, and stir evenly to obtain a molybdenum powder solution, and finally put the molybdenum powder solution into a ball mill; The first organic solvent is toluene, and toluene is put into a ball mill; The ball mill was covered with a lid for the first ball milling. After the ball milling stopped, the lid was opened and part of the acrylic adhesive was put into the ball mill. Then the lid was covered and the ball mill was started for the second ball milling. During the ball milling process, the particle size of the particles in the slurry was adjusted. 50 Conduct monitoring.
10. Use of alumina slurry prepared by the method according to any one of claims 1 to 9 in preparing green ceramic sheets.