Ceramic matrix composite material and method for making the same
By adding sintering inhibitors with specific particle size and distribution to ceramic matrix composites, the problem of strength reduction in oxide-based CMCs at high temperatures was solved, achieving high strength and strength retention rate under high-temperature conditions.
Patent Information
- Application Number
- CN202180085142.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-12-25
- Filing Date
- 2021-12-21
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-12-21
AI Technical Summary
Existing oxide-based ceramic matrix composites are prone to ceramic particle growth at high temperatures, leading to reduced matrix porosity and strength. This phenomenon is particularly difficult to suppress under high-temperature conditions above 1000℃.
By adding sintering inhibitors with an average particle size of less than 0.28 μm, such as silica, zirconium oxide, yttrium oxide, magnesium oxide, or mullite, to the ceramic matrix, the average particle size and the distance between the centers of gravity in the matrix can be adjusted to suppress the growth of ceramic particles and improve the tensile strength and strength retention rate of the material after heat exposure treatment.
It achieves high tensile strength (above 150MPa) and strength retention rate (above 80%) of ceramic composite materials at a high temperature of 1200℃, effectively suppressing the strength reduction caused by heat exposure.
Smart Images

Figure CN116670096B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a ceramic matrix composite material and a method for making the same. Background Art
[0002] Compared with ordinary ceramics, ceramic matrix composite materials (hereinafter also referred to as "CMC") formed by combining ceramic continuous fibers with a ceramic matrix have higher resistance (damage tolerance) to the destruction of the entire material caused by the progress of damage. Therefore, CMC is being studied as a substitute material for heat-resistant metals such as Ni-based alloys.
[0003] CMC (hereinafter also referred to as "oxide-based CMC") formed by forming alumina or mullite-based oxide into ceramic continuous fibers and composite the ceramic continuous fibers with a ceramic matrix has a heat resistance of 1200° C. Therefore, the application of oxide-based CMC as a component for aircraft jet engines is expected (see Non-Patent Document 1).
[0004] As a method for producing oxide-based CMC, the following method is known: a slurry obtained by dispersing raw material powder of a ceramic matrix in a solvent such as water (hereinafter also referred to as "matrix slurry") is impregnated into ceramic continuous fibers and dried to obtain a molded body, and the obtained molded body is sintered at above 1000° C. to obtain an oxide-based CMC (see non-patent document 2).
[0005] Prior art literature
[0006] Non-patent literature
[0007] Non-patent document 1: J. Aerospace Lab, Issue 3, (2011) 1-12.
[0008] Non-patent document 2: J.Am.Ceram.Soc.,81[8],(1998)2077-86.
[0009] Non-patent document 3: Acta Mater., 47
[12] , (1999) 3411-3422
[0010] Non-patent document 4: J. Euro. Ceram. Soc., 32, (2012) 1965-1970 Summary of the invention
[0011] Problems to be solved by the invention
[0012] Generally, for oxide-based CMCs exposed to high temperatures of more than 1000°C for a long time, the ceramic particles in the ceramic matrix (i.e., the ceramic particles constituting the ceramic matrix) undergo grain growth due to heat. As a result, the porosity of the ceramic matrix decreases and the ceramic matrix and the ceramic continuous fibers are consolidated. As a result, the strength of the CMC decreases. Therefore, attempts have been made to suppress the grain growth of ceramic particles by adding magnesium oxide and zirconium oxide as sintering inhibitors to the ceramic matrix (see non-patent documents 3 and 4). However, the oxide-based CMCs obtained in these non-patent documents all have low tensile strength, and the strength decreases significantly when exposed to high temperature environments.
[0013] An object of the present invention is to provide at least one of a ceramic composite material having high tensile strength and in which a decrease in strength after a heat exposure treatment is suppressed, and a method for producing the same.
[0014] Means for solving problems
[0015] The inventors of the present application attempted to make a ceramic matrix raw material contain a sintering inhibitor, and produced a CMC including a ceramic matrix, a ceramic continuous fiber, and a sintering inhibitor. As a result, they discovered a CMC that inhibits the grain growth of ceramic particles in the ceramic matrix and is not easily reduced in strength even when exposed to a high temperature environment of 1200°C. Furthermore, focusing on the average particle size of the sintering inhibitor, they discovered a CMC that maintains high strength by adjusting the average particle size of the sintering inhibitor, thereby completing the present invention.
[0016] That is, the present invention is as described in the claims, and the gist of the present invention is as follows.
[0017] [1] A ceramic matrix composite material comprising a ceramic matrix and ceramic continuous fibers, wherein the ceramic matrix contains a sintering inhibitor having an average particle size of not more than 0.28 μm.
[0018] [2] The ceramic matrix composite material according to [1] above, wherein the average distance between centers of gravity of the sintering inhibitor is 4.5 μm or less.
[0019] [3] The ceramic matrix composite material according to [1] or [2] above, wherein the sintering inhibitor is one or more selected from the group consisting of silica, zirconia, yttrium oxide, magnesium oxide, mullite and strontium oxide.
[0020] [4] The ceramic matrix composite material as described in any one of [1] to [3] above, wherein the ceramic continuous fibers are continuous fibers of one or more oxide ceramics selected from the group consisting of alumina, silica, mullite, and zirconia.
[0021] [5] The ceramic matrix composite material according to any one of [1] to [4] above, wherein the ceramic matrix is one or more oxides selected from the group consisting of alumina, mullite, and zirconia.
[0022] [6] A ceramic matrix composite material as described in any one of [1] to [5] above, characterized in that the ceramic matrix composite material has a tensile strength of 150 MPa or more and a strength retention rate of 80% or more after heat exposure treatment at 1200°C for 100 hours.
[0023] [7] A method for producing a ceramic matrix composite material as described in any one of [1] to [6] above, wherein a molded body obtained by impregnating ceramic continuous fibers into a ceramic matrix slurry obtained by adding a sintering inhibitor having a purity of 99% or more to a ceramic matrix raw material powder and drying the impregnated ceramic continuous fibers is sintered.
[0024] [8] The method for producing a ceramic matrix composite material according to [7] above, wherein the average particle size of the sintering inhibitor exceeds 0.05 μm and is not more than 30 μm.
[0025] Effects of the Invention
[0026] The ceramic matrix composite material of the present invention achieves the following objectives: providing a ceramic composite material having a high strength of more than 150 MPa in which the reduction in strength after heat exposure treatment is suppressed (for example, a ceramic composite material having a strength retention rate of more than 80% after heat exposure treatment at 1200°C for 100 hours and suppressed reduction in strength), and at least one of its manufacturing methods. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] [ Figure 1 ] Figure 1 Graph showing the relationship between the tensile strength of the ceramic matrix composite materials of Examples 1 to 3 and Comparative Examples 1 and 2 and the average particle size of silica in the ceramic matrix.
[0028] [ Figure 2 ] Figure 2 Graph showing the relationship between the tensile strength of the ceramic matrix composite materials of Examples 1 to 3 and Comparative Examples 1 and 2 and the average center-of-gravity distance of silica in the ceramic matrix.
[0029] [ Figure 3 ] Figure 3 This is a silicon mapping image obtained by photographing the sample of Example 1 at 5000 times magnification.
[0030] [ Figure 4 ] Figure 4 This is a silicon mapping image obtained by photographing the sample of Comparative Example 1 at 5000 times magnification. DETAILED DESCRIPTION
[0031] Hereinafter, the present invention will be described.
[0032] In this specification, a "ceramic matrix composite" (CMC) is a material formed by a composite of ceramic continuous fibers and a ceramic matrix, and is a so-called ceramic fiber-reinforced ceramic.
[0033] In this specification, the so-called "ceramic fiber" refers to polycrystalline ceramics formed by spinning, and filamentary polycrystalline ceramics. Ceramic fibers can be divided into "ceramic short fibers" and "ceramic continuous fibers" according to their fiber length. In this embodiment, "ceramic short fibers" refer to ceramic fibers with a fiber length of less than 500μm, and "ceramic continuous fibers" are ceramic fibers other than ceramic short fibers (ceramic fibers with a fiber length of 500μm or more). In addition, the ceramic fiber can be an independent single fiber, a ceramic fiber in a state of a plurality of fibers being aggregated, or a fiber bundle. In this specification, a "fiber bundle" is a fiber in a state of agglomeration of two or more ceramic fibers, or a fiber in a state of agglomeration of hundreds of units of ceramic fibers. The so-called "ceramic fiber cloth" is a fabric of ceramic fibers, especially a fabric of ceramic continuous fibers. It can also be a fabric of ceramic continuous fibers in a fiber bundle.
[0034] In this specification, the "ceramic matrix" refers to the matrix (parent phase) of CMC composed of ceramic crystal grains, and may also contain a sintering inhibitor.
[0035] In this specification, the "sintering inhibitor" is a substance having a function of inhibiting the grain growth of ceramic crystal grains during heat treatment.
[0036] The present invention relates to CMC, characterized in that it includes a ceramic matrix (hereinafter also referred to as "matrix") and ceramic continuous fibers (hereinafter also referred to as "continuous fibers"), and the matrix contains a sintering inhibitor (hereinafter also referred to as "inhibitor") having an average particle size of 0.28 μm or less. That is, the CMC of the present invention is essentially a CMC formed by a matrix, continuous fibers and an inhibitor, and the inhibitor is contained in the matrix. In addition, it is characterized in that an inhibitor having a specific average particle size is contained in the matrix. When the average particle size of the inhibitor is higher than this value, the inhibitor becomes coarse particles in the matrix. As a result, the inhibitor may become a source of destruction of the CMC.
[0037] The average particle size of the inhibitor of the CMC of the present invention (hereinafter also referred to as "average inhibitor particle size") is 0.28 μm or less. If the average inhibitor particle size exceeds 0.28 μm, the tensile strength of the CMC is likely to decrease. The average inhibitor particle size is 0.05 μm or more, 0.08 μm or more, or 0.10 μm or more, and preferably 0.28 μm or less or 0.26 μm or less. If the average inhibitor particle size is 0.05 μm or more, the grain growth of the matrix (i.e., the grain growth of the ceramic grains constituting the matrix) is easily suppressed.
[0038] The average inhibitor particle size is the average particle size of the inhibitor. In the CMC of the present invention, the inhibitor exists in the matrix. Therefore, in the cross section of the CMC, the matrix is observed using a field emission scanning microscope (hereinafter also referred to as "FE-SEM") equipped with an energy dispersive X-ray analyzer to obtain EDS mapping data of elements corresponding to the inhibitor, and the data is converted into a two-dimensional EDS mapping image. The average inhibitor particle size is obtained by image analysis of the obtained two-dimensional EDS mapping image.
[0039] FE-SEM observation is performed using a field emission scanning microscope (for example, JSM-7600F, manufactured by JEOL Ltd.) that is a common energy dispersive X-ray analyzer. The following conditions can be cited as conditions for FE-SEM observation.
[0040] Accelerating voltage: 7kV
[0041] Observation magnification: 5000 times
[0042] The measurement sample may be cut into pieces by using a diamond blade and an observation surface may be prepared using an Ar ion beam cross-section polisher.
[0043] The conversion of EDS mapping data into a two-dimensional EDS mapping image can be performed using image analysis software (e.g., ImageJ, manufactured by the National Institutes of Health, USA). Specifically, the EDS mapping data is input into the image analysis software and converted into a two-dimensional EDS mapping image of 256×192 pixels.
[0044] As for the image analysis of the two-dimensional EDS mapping image, it can be performed using image analysis software (for example, ImageJ, manufactured by the National Institute of Health). The two-dimensional EDS mapping image is input into the image analysis software in grayscale. The grayscale image is binarized with 8 bits and a threshold of 50 to obtain a processed image. In the processed image, the white area corresponds to the inhibitor, so the equivalent diameter of each area is calculated based on the area of each white area in the processed image, and the average particle size of the inhibitor is calculated using the average value. It should be noted that the number of inhibitors (white areas) used for calculation can be set to 150 ± 50.
[0045] The CMC of the present invention preferably has an average center-of-gravity distance of 4.5 μm or less of the inhibitor. It is more preferably 0.01 to 4.0 μm, and even more preferably 0.03 to 3.5 μm. If the average center-of-gravity distance is 4.5 μm or less, the inhibitor is easily dispersed and present in the matrix. In addition, when the CMC is subjected to heat exposure treatment, defects originating from the inhibitor are less likely to occur.
[0046] The average distance between centers of gravity is obtained by analyzing the center of gravity of the inhibitor based on a mapping image of the substrate (a two-dimensional EDS mapping image obtained by converting EDS mapping data using image analysis software (e.g., ImageJ, manufactured by the National Institutes of Health)) and connecting the center of gravity points with a straight line according to the following (a) and (b) standards.
[0047] (a) Connect the obtained centroids with a straight line that does not pass through other particles.
[0048] (b) When a line segment connecting the centroids intersects another line segment, the shorter one is used.
[0049] The average distance between centers of gravity obtained by this analysis means the extent to which the inhibitors are separated and exist in the matrix. The larger the average distance between centers of gravity, the weaker the effect of inhibiting the sintering of the matrix.
[0050] The average center-of-gravity distance can be derived using image analysis software Nanohunter (product name: NS2K-PRO, manufactured by NANOSYSTEM).
[0051] Specifically, the average center-of-gravity distance in the present invention can be obtained by the following method: That is, by observing the matrix in the cross section of CMC with FE-SEM to obtain an EDS mapping image of the element corresponding to the inhibitor, and performing image analysis on the image.
[0052] Using the processed image obtained in the same manner as for the average inhibitor particle size, the coordinates of the center of gravity of each white region in the processed image were determined by the following method.
[0053] The coordinates of the center of gravity of the white area are set as (Xg, Yg), and the coordinates of the center of gravity of each white area are calculated using the following formula: The long side of the processing image is set as the X axis, and the short side is set as the Y axis.
[0054] Xg = (the sum of the x-coordinate values of each unit pixel when the white area is divided) / the sum of the number of unit pixels constituting the white area
[0055] Yg = (the sum of the y coordinate values of each unit pixel when the white area is divided) / the sum of the number of unit pixels constituting the white area
[0056] According to the criteria of (a) and (b) above, the centroids of different white areas are connected with straight lines, and the average value of the lengths of the obtained line segments is calculated, and the average value is used as the average centroid distance.
[0057] The coordinates of the centroid, the length of the line segment, and the average value can be calculated using image analysis software (eg, NS2K-PRO, manufactured by NANOSYSTEM). The number of inhibitors used for calculation can be 150±50.
[0058] The inhibitor may be of a composition different from that of the matrix, and for example, may be one or more selected from the group consisting of silica, zirconia, yttrium oxide, magnesium oxide, mullite and strontium oxide, preferably one or more selected from the group consisting of silica, zirconia, yttrium oxide, magnesium oxide and mullite, and particularly preferably silica.
[0059] The content of the inhibitor (hereinafter also referred to as "substrate inhibitor amount") is preferably 1 mass % to 10 mass % relative to the total mass of the substrate and the inhibitor, more preferably 1.1 mass % to 9 mass %, and further preferably 1.5 mass % to 6.5 mass %. On the other hand, defects derived from the inhibitor tend to be reduced, so the substrate inhibitor amount is preferably 0.3 mass % to 0.4 mass % or more, and less than 5.0 mass % or less than 4.0 mass %.
[0060] In the CMC of the present invention, the mass ratio of the inhibitor relative to the mass of the CMC (hereinafter also referred to as "CMC inhibitor amount") can be exemplified as 0.4 mass% or more or 0.6 mass% or more and 4.3 mass% or less or 2.8 mass% or less. On the other hand, the CMC inhibitor amount is preferably 0.1 mass% or more or 0.2 mass% or more and 3.0 mass% or less or 2.5 mass% or less, because defects derived from the inhibitor are likely to be reduced.
[0061] In the present invention, the mass of CMC is the total mass of the matrix, the inhibitor, and the continuous fibers.
[0062] For example, in a CMC containing silica as an inhibitor and having a matrix of alumina, the CMC inhibitor amount can be calculated by {(mass of silica [g]) / (mass of silica + mass of alumina + mass of continuous fibers) [g]}×100. In addition, the matrix inhibitor amount can be calculated by {(mass of silica [g]) / (mass of silica + mass of alumina) [g]}×100.
[0063] The CMC of the present invention preferably contains at least silicon dioxide (SiO2) as an inhibitor. If silicon dioxide is contained as an inhibitor, the particle growth of the matrix is easily suppressed, and a CMC with higher heat resistance is easily obtained. In particular, when the matrix is alumina, the effect of suppressing the particle growth of the matrix is more easily obtained.
[0064] The content of silica (hereinafter also referred to as "CMC silica content") is preferably 0.4% by mass or more or 0.6% by mass or more, and preferably 4.3% by mass or less or 2.8% by mass or less, relative to the mass of CMC. On the other hand, it is preferably 0.1% by mass or more or 0.2% by mass, and 3.0% by mass or less or 2.5% by mass, because the defects derived from silica tend to decrease. If the CMC silica content is 0.1% by mass or more, the particle growth of the matrix is more easily suppressed. On the other hand, if the CMC silica content is 4.3% by mass or less, the ceramic continuous fibers and the matrix are less likely to consolidate, and even if heat exposure treatment is performed, defects caused by the dissolution of silica are less likely to occur in the CMC.
[0065] The substrate is at least one of oxide ceramics and non-oxide ceramics, preferably oxide ceramics, more preferably at least one selected from the group consisting of alumina, mullite and zirconia, and further preferably at least one of alumina and mullite.
[0066] Considering high heat resistance and the like, the matrix is, for example, one or more oxides selected from the group consisting of alumina, mullite, and zirconia. Alumina is preferred from the viewpoint of having higher heat resistance and strength.
[0067] As long as the continuous fiber is a continuous fiber composed of ceramic, there is no particular restriction, preferably oxide ceramics, more preferably one or more of the group consisting of alumina, silica, mullite and zirconia, further preferably at least any one of the oxide ceramics of alumina and mullite, and further preferably a continuous fiber of oxide ceramics of alumina and / or mullite. Ceramic continuous fiber can be a continuous fiber formed by the same type of ceramic as the matrix, or a continuous fiber formed by a ceramic of a different type from the matrix. The so-called continuous fiber here is a fiber that can use any length and can be woven into a two-dimensional or three-dimensional structure. Usually, when making CMC, a fiber in a state where hundreds of units of fibers are gathered is used as a ceramic continuous fiber. With regard to the ceramic continuous fiber of the present embodiment, it is preferably a fiber bundle state and a fiber bundle is woven state. The ceramic continuous fiber (hereinafter also referred to as "ceramic fiber cloth") is preferably a fiber bundle woven state. The oxide ceramic continuous fiber can be, for example, an alumina continuous fiber, a mullite continuous fiber, etc., more preferably a mullite continuous fiber. From the viewpoint of strength, the continuous fiber is preferably an alumina continuous fiber. On the other hand, from the viewpoint of heat resistance, the continuous fiber is preferably a mullite continuous fiber. It should be noted that the mullite continuous fiber can be a continuous fiber formed of mullite and alumina, and can also contain alumina. The continuous fiber formed of mullite and alumina can be exemplified by a continuous fiber in which the mass ratio of mullite (3Al2O3·2SiO2): alumina (Al2O3) is 70 mass %: 30 mass % to 45 mass %: 55 mass %.
[0068] The CMC of the present invention has high strength, and the tensile strength (especially the tensile strength of the CMC in a state where no heat exposure treatment is performed) is preferably 150 MPa or more, more preferably 150 or more and 700 MPa or less, and particularly preferably 150 or more and 650 MPa or less. In addition, the CMC of the present invention is characterized in that the strength does not decrease even when exposed to a high temperature environment of 1200°C. Therefore, the strength retention rate of the CMC of the present invention after 100 hours of heat exposure treatment at 1200°C (hereinafter also referred to as "strength retention rate") is preferably 80% or more, more preferably 85% or more, and further preferably 90% or more. The strength retention rate of the CMC of the present invention can be exemplified as less than 120%, less than 115%, or less than 105%. For the CMC of this embodiment, the tensile strength after heat exposure treatment can also be higher than the tensile strength before heat exposure treatment.
[0069] The tensile strength is a value obtained by using a strength tester (e.g., AG-XPlus, manufactured by Shimadzu Corporation) and a tensile test fixture according to the method of JIS R 1656. For the test sample, CMC is processed into a width of 10±1mm×length of 110±10mm×thickness of 2±1mm, and aluminum pull tabs are installed at both ends to make a tensile test piece. For the measurement of tensile strength, the average value obtained by measuring twice with a load speed of 0.5mm / min can be used as the tensile strength of CMC.
[0070] The heat exposure treatment may be exemplified by a method of heat treating CMC in an air atmosphere at 1200° C. for 100 hours.
[0071] The fiber volume fraction of the CMC of the present invention is 30 vol% to 60 vol%. When the fiber volume fraction satisfies this range, the ceramic continuous fibers are appropriately present in the CMC, and the shape of the CMC is easily maintained, so that a CMC with high strength is easily obtained.
[0072] The fiber volume fraction is the volume ratio [vol %] of the continuous fibers in the CMC. The fiber volume fraction is calculated by the following formula.
[0073] Fiber volume ratio [vol %] = (V f / V CMC )×100
[0074] In the above formula, V f is the volume of continuous fiber, V CMC is the volume of CMC. In addition, V f and V CMC Each can be calculated using the following formula.
[0075] V f =m / ρ f
[0076] V cmc =A×B×t
[0077] In the above formula, m is the mass of the continuous fiber [g], and ρ f is the density of continuous fibers [g / cm 3 ], in addition, A is the length of CMC [cm], B is the width of CMC [cm], and t is the thickness of CMC [cm].
[0078] The density of the CMC of the present invention varies depending on the type of substrate, and is, for example, 2.40 g / cm 3 Above 3.20g / cm 3 the following.
[0079] Density is the measured density of CMC [g / cm 3] is the ratio of volume measured by the Archimedean method to mass measured using an electronic balance according to JIS R 1634 [g / cm 3 ]The value obtained.
[0080] The CMC of this embodiment can be used for known CMC applications, and can be used for components including the CMC, particularly applications requiring heat resistance, and one or more selected from the group consisting of heat-resistant filters, turbine components, and nuclear power-related components.
[0081] Next, the method for producing the CMC of the present invention will be described.
[0082] As long as a CMC having the above characteristics can be obtained, any method for producing the CMC of the present invention can be used. The CMC of the present invention can be produced by sintering a molded body obtained by impregnating ceramic continuous fibers into a ceramic matrix slurry obtained by adding a sintering inhibitor having a purity of 99% or more to a ceramic matrix raw material powder and drying the resultant.
[0083] As a specific method for producing CMC of the present invention, there can be cited a method for producing a ceramic matrix composite material comprising the following steps: a step of impregnating ceramic continuous fibers with a slurry comprising a ceramic matrix raw material powder, a sintering inhibitor having an average particle size of more than 0.05 μm and less than 30 μm, and a solvent to obtain a mixture; a step of solidifying the mixture to obtain a molded body; and a step of sintering the molded body. As a specific method for producing CMC of the present invention, there can be cited a method for producing a ceramic matrix composite material comprising the following steps: a step of impregnating ceramic continuous fibers with a slurry comprising a ceramic matrix raw material powder, a sintering inhibitor having an average particle size of more than 0.05 μm and less than 30 μm and a purity of more than 99%, and a solvent to obtain a mixture; a step of solidifying the mixture to obtain a molded body; and a step of sintering the molded body.
[0084] By impregnating ceramic continuous fibers with a slurry comprising ceramic matrix raw material powder, a sintering inhibitor having an average particle size greater than 0.05 μm and less than 30 μm, and a solvent (hereinafter also referred to as the "impregnation process"), a composition in which the precursors of the matrix and the inhibitor are diffused and infiltrated in the ceramic continuous fibers (continuous fibers), i.e., a mixture of the matrix slurry and the continuous fibers, can be obtained.
[0085] The slurry containing a ceramic matrix raw material powder, a sintering inhibitor having an average particle size of more than 0.05 μm and less than 30 μm, and a solvent (hereinafter also referred to as "matrix slurry", and for convenience, the sintering inhibitor contained in the matrix slurry is also referred to as "inhibitor source") only needs to have fluidity that can be impregnated into continuous fibers. The viscosity of the matrix slurry can be, for example, greater than 1 mPa·s or greater than 5 mPa·s and less than 500 mPa·s or less than 400 mPa·s. The viscosity of the matrix slurry is easily affected by the average particle size of the ceramic matrix raw material powder, the average particle size of the inhibitor source, and the content of the inhibitor source. Occasionally, it is also affected by the content of adsorbed water in the ceramic matrix raw material powder and the inhibitor source.
[0086] Ceramic matrix raw material powder (hereinafter also referred to as "raw material powder") is a powder of the raw material of the matrix of CMC, that is, a precursor of the matrix. The raw material powder can be arbitrarily selected according to the type of the matrix of the target CMC, for example, oxide powder, and one or more selected from the group consisting of alumina powder, mullite powder, zirconia powder and silica powder, and at least one of alumina powder and mullite powder, and alumina powder. In addition, the raw material powder can include α-alumina powder, mullite powder, zirconia powder, and composite powders thereof, preferably at least α-alumina powder, preferably α-alumina powder.
[0087] The average particle size of the raw material powder (hereinafter also referred to as "raw material particle size") is preferably 0.1 μm to 5 μm, more preferably 0.1 μm to 2.0 μm, and further 0.1 μm to 0.5 μm. By making the raw material particle size satisfy this range, the raw material powder can be easily dispersed uniformly around the continuous fiber.
[0088] The raw material particle size is the median particle size (D50) in the volume particle size distribution of the raw material powder measured by a wet method, which can be measured using a conventional device (e.g., MT3300EX-II, manufactured by Macrotrac BEL). As the measurement sample, a slurry obtained by dispersing the raw material powder in pure water and subjecting it to a dispersion treatment such as ultrasonic treatment to remove slow aggregates can be used.
[0089] The content of the raw material powder in the matrix slurry (hereinafter also referred to as "solid content concentration") is preferably 50 mass % to 80 mass %, and more preferably 60 mass % to 80 mass %.
[0090] The solid content concentration is a mass concentration obtained by the ratio [mass %] of the total mass of the raw material powder and the inhibitor source relative to the total mass of the raw material powder, the inhibitor source and the solvent.
[0091] The volume ratio of the raw material powder to the volume of the matrix slurry at 25°C and atmospheric pressure (hereinafter also referred to as "volume solid content concentration") is preferably 20 vol% to 55 vol%, more preferably 28 vol% to 55 vol%.
[0092] For example, in the case of a matrix slurry in which the raw material powder is alumina powder, the inhibitor source is silica, and the solvent is water, the solid content concentration is {(mass of alumina powder [g] + mass of silica [g]) / (mass of silica + mass of alumina powder + mass of water) [g]}×100. In addition, the volume solid content concentration is given by {(volume of alumina [cm 3 ] + volume of silicon dioxide [cm 3 ]) / (volume of silicon dioxide + volume of aluminum oxide + volume of water) [cm 3 ]}×100. In addition, in calculating the volume solid content concentration, the density at 25°C and atmospheric pressure may be used.
[0093] In addition, the solid content concentration can also be obtained as the mass ratio of the residual part after the solvent of the base slurry is dried relative to the mass of the base slurry.
[0094] The inhibitor source may be the same compound as the inhibitor contained in CMC and at least one of its precursors, or may be a precursor of the inhibitor contained in CMC. The inhibitor source may be a compound having a composition different from that of the raw material powder, and examples thereof include one or more selected from the group consisting of silica, zirconia, yttrium oxide, magnesium oxide, and mullite, and further one or more selected from the group consisting of silica, zirconia, yttrium oxide, magnesium oxide, and mullite, and further at least one of silica and zirconia. In addition, it is preferred that at least silica is included, and further, silica is more preferred.
[0095] The inhibitor source may be in a state that can be mixed with the raw material powder, and is preferably at least one of a powder and colloidal particles, and more preferably a powder.
[0096] The average particle size of the inhibitor source (hereinafter also referred to as the "average inhibitor source particle size") is preferably greater than 0.05 μm and less than 30 μm. The average inhibitor source particle size is less than 30 μm, preferably less than 10 μm, less than 5 μm, less than 1 μm, less than 0.8 μm or less than 0.5 μm. If the average inhibitor source particle size exceeds 30 μm, coarse particles of the inhibitor are easily generated in the obtained CMC. The average inhibitor source particle size is greater than 0.01 μm, preferably greater than 0.05 μm, greater than 0.08 μm, greater than 0.1 μm or greater than 0.2 μm. The preferred range of the average inhibitor source particle size can be exemplified by 0.06 μm to 10 μm, 0.06 to 1 μm, and further 0.08 μm to 0.5 μm. By making the average inhibitor source particle size satisfy this range, the inhibitor source is not easy to aggregate in the matrix slurry. In addition, in the obtained CMC, the inhibitor is easily dispersed uniformly in the matrix. As a result, it is considered that the average inhibitor particle size of CMC of the present invention is likely to be satisfied after sintering.
[0097] The average inhibitor source particle size may be measured in the same manner as the raw material particle size.
[0098] The inhibitor source preferably has a high purity, preferably 99% or more, but may have a purity of 100% or less.
[0099] The content of the inhibitor source in the matrix slurry may be the same as the content of the inhibitor in the target CMC. The content of the inhibitor source in the matrix slurry is preferably 0.3% by mass to 10% by mass, more preferably 0.4% by mass to 9% by mass, and even more preferably 0.5% by mass to 7% by mass, for example, in terms of the ratio of the mass of the inhibitor source to the total mass of the raw material powder and the inhibitor source (hereinafter also referred to as "the amount of the inhibitor source" and, when the inhibitor is silica, etc., also referred to as "the amount of the silica source", etc.).
[0100] In addition, the mass ratio of the inhibitor source relative to the mass of the matrix slurry (i.e., the total mass of the raw material powder, the inhibitor source and the solvent) (hereinafter also referred to as "inhibitor source amount (slurry)") can be exemplified as greater than 0.2 mass % or greater than 0.3 mass % and less than 8 mass % or less than 7 mass %.
[0101] For example, in a matrix slurry in which the matrix powder is alumina, the inhibitor source is silica, and the solvent is water, the amount of the inhibitor source is calculated by {(mass of silica [g]) / (mass of silica + mass of alumina) [g]}×100, and the amount of the inhibitor source (slurry) is calculated by {(mass of silica [g]) / (mass of silica + mass of alumina + mass of water) [g]}×100, respectively.
[0102] In addition, the mass ratio of the raw material powder relative to the mass of the matrix slurry (i.e., the total mass of the raw material powder, the inhibitor source and the solvent) (hereinafter also referred to as "raw material powder amount (slurry)") can be exemplified as greater than 45 mass % or greater than 55 mass % and less than 80 mass % or less than 75 mass %.
[0103] For example, in a matrix slurry in which the matrix powder is alumina, the inhibitor source is silica, and the solvent is water, the amount of raw powder (slurry) is calculated by {(mass of alumina [g]) / (mass of silica + mass of alumina + mass of water) [g]}×100.
[0104] The solvent contained in the matrix slurry can be, for example, one or more alcohols selected from the group consisting of water, methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, butyl alcohol and isobutyl alcohol; one or more ketones selected from the group consisting of acetone, methyl ethyl ketone, methyl isobutyl ketone, diisobutyl ketone, cyclohexanone and diacetone alcohol; one or more aromatic hydrocarbons selected from the group consisting of benzene, toluene and xylene; one or more hydrocarbons selected from the group consisting of ethyl acetate, methyl acetate, butyl acetate, ethyl acetate, At least one ester selected from the group consisting of methoxybutyl acetate and isobutyl acetate; at least one aliphatic hydrocarbon selected from the group consisting of n-hexane, heptane, cyclohexane and methylcyclohexane; at least one glycol ether selected from the group consisting of ethylene glycol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether and propylene glycol monomethyl ether; at least one selected from the group consisting of N,N-dimethylformamide, tetrahydrofuran, N-methyl-2-pyrrolidone, 1,4-dioxane and styrene. The solvent is preferably at least one of water and alcohol, and more preferably water.
[0105] In the manufacturing method of the present invention, any method for manufacturing the matrix slurry provided for the impregnation process is any as long as it is a slurry in a state in which the raw material powder and the inhibitor source are dispersed. The manufacturing method of the matrix slurry is any as long as the raw material powder, the inhibitor source and the solvent are mixed. It is preferably obtained by crushing and mixing. Specifically, the raw material powder, the inhibitor source and the solvent are mixed and crushed in a ball mill. The balls used in the ball mill only need to remove the slow agglomerates of the raw material powder, and can be ceramic balls with a larger average particle size than the raw material powder. As such balls, ceramic balls with a diameter of 0.5 mm to 20 mm, and 1 mm to 15 mm can be exemplified. The ceramic ball can be at least any one of an alumina ball and a zirconia ball, and can further be an alumina ball.
[0106] In order to make the raw material powder and the inhibitor source disperse more uniformly by using the solvent, the matrix slurry may also contain a dispersant. The dispersant may be exemplified by at least one of a dispersant having high affinity with the raw material powder and a dispersant having high solubility in the solvent, and may be one or more selected from the group consisting of anionic polymer dispersants, cationic polymer dispersants, nonionic polymer dispersants, anionic low molecular weight dispersants, cationic low molecular weight dispersants, nonionic low molecular weight dispersants, inorganic acids, and inorganic salts. As a specific dispersant, preferably at least one selected from the group consisting of ammonium polyacrylate, ammonium polymethacrylate, sodium polyacrylate, sodium polymethacrylate, polyethylene imine, polyethylene glycol, sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, benzalkonium chloride, distearyl dimethyl ammonium chloride, polyoxyethylene alkyl ether, pentaethylene glycol monododecyl ether, octaethylene glycol monododecyl ether, polyoxyethylene alkylphenyl ether, dilute nitric acid, dilute hydrochloric acid, dilute sulfuric acid, phosphoric acid and sodium tripolyphosphate, more preferably at least one selected from the group consisting of ammonium polyacrylate, ammonium polymethacrylate, sodium polyacrylate, sodium polymethacrylate, polyethylene imine, dilute nitric acid, dilute hydrochloric acid, dilute sulfuric acid and phosphoric acid, further preferably at least one selected from the group consisting of ammonium polyacrylate, ammonium polymethacrylate, dilute nitric acid and dilute hydrochloric acid, and still more preferably at least one of dilute nitric acid and dilute hydrochloric acid.
[0107] The content of the dispersant can be exemplified by 0.01% or more or 0.05% by mass and 10% or less or 8% by mass relative to the mass of the matrix slurry (ie, the total mass of the raw material powder, the inhibitor source, the solvent, and the dispersant).
[0108] Examples of the ceramic continuous fibers impregnated in the matrix slurry include alumina continuous fibers, mullite continuous fibers, etc. Alumina·mullite continuous fibers, that is, continuous fibers composed of alumina and mullite are preferred.
[0109] The ceramic continuous fibers used in the impregnation step may be the same as those contained in the CMC, and are preferably continuous fibers of one or more selected from the group consisting of alumina, silica, mullite, and zirconia, and more preferably at least one of alumina and mullite.
[0110] The impregnation step can obtain a mixture of the matrix slurry and the continuous fibers. The impregnation method may be any method that allows the matrix slurry to diffuse and impregnate the continuous fibers, and examples thereof include at least one of a vacuum impregnation treatment and a pressure impregnation treatment.
[0111] Examples of the vacuum impregnation treatment include treatment performed under the following conditions.
[0112] Impregnation atmosphere: Vacuum degree is 85% or more, or 90% or more, and 100% or less; Vacuum degree is less than 100%, or 99% or less
[0113] Impregnation temperature: above 0℃ or above 10℃, and
[0114] Below 40℃ or below 35℃
[0115] As the pressure impregnation treatment, there can be mentioned treatment performed under the following conditions.
[0116] Impregnation pressure: 0.11MPa or more or 0.15MPa or more, and
[0117] 2.0MPa or less or 1.8MPa or less
[0118] Impregnation temperature: above 0℃ or above 10℃, and
[0119] Below 40℃ or below 35℃
[0120] Specifically, as an impregnation method, there can be exemplified a method of impregnating the continuous fibers with the matrix slurry at 25° C. and under a vacuum degree of 95% or more and less than 100%.
[0121] The manufacturing method of the present embodiment includes a step of solidifying the mixture to obtain a molded body (hereinafter also referred to as a "molding step"). Thus, a molded body as a precursor of the CMC of the present embodiment can be obtained. The molding method can be any method in which the mixture is solidified to obtain a mixture (molded body) having a certain shape, and one or more selected from the group consisting of heat treatment, freezing treatment and additive treatment can be exemplified. It should be noted that the molding step can be a combination of the above methods, and the same treatment can also be performed multiple times.
[0122] Examples of the heat treatment include treatment under the following conditions.
[0123] Heat treatment temperature: above 50℃, above 60℃ or above 80℃, and
[0124] Below 160℃ or below 140℃
[0125] Heat treatment times: more than 1 time but less than 5 times
[0126] The heat treatment time may be arbitrarily adjusted according to the amount of the mixture to be treated and the heat treatment temperature, and examples thereof include 1 hour to 10 hours, and 2 hours to 8 hours.
[0127] As the freezing treatment, there can be mentioned treatment under the following conditions.
[0128] Freezing temperature: above -200℃ or above -180℃, and
[0129] Below -20℃ or below -30℃
[0130] Sublimation pressure: 0.001MPa or more or 0.002MPa or more, and
[0131] 0.05MPa or less or 0.03MPa or less
[0132] Number of treatments: more than 1 time but less than 5 times
[0133] When the freezing treatment is performed a plurality of times, the freezing temperature and the sublimation pressure may be set to arbitrary conditions.
[0134] As an additive treatment, a treatment in which the mixture is molded by mixing additives such as a curing agent and a binder with the mixture can be cited. As long as the additive is a known additive used in the manufacture of CMC, for example, agar, gelatin, methylcellulose, camphene, sodium alginate, 2-hydroxyethyl acrylate, 4-hydroxybutyl acrylate, 6-hydroxyhexyl acrylate, acrylic acid, methacrylic acid, acrylamide, N,N'-methylenebisacrylamide, N,N'-ethylenebisacrylamide, methacrylamide, polyethylene glycol diacrylate, methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, urea, boron nitride (BN), aluminum nitride (AlN), silicon nitride (Si3N4), gallium nitride (GaN), zirconium nitride (ZrN), polyaluminum chloride ([Al2(OH) n Cl 6-n ] m , 1≤n≤5, m≤10), trimethoxyaluminum, triethoxyaluminum, tri-n-propoxyaluminum, tri-isopropoxyaluminum, tri-n-butoxyaluminum, tri-isobutoxyaluminum, tri-sec-butoxyaluminum, tri-tert-butoxyaluminum, trimethoxyboron, triethoxyboron, tri-n-propoxyboron, tri-isopropoxyboron, tetramethoxysilane, tetraethoxysilane, tetra-n-propoxysilane, tetra-isopropoxysilane, tetra-n-butoxysilane, tetra-isobutoxysilane, tetra-n-butoxysilane, tetra-sec-butoxysilane, tetra-tert-butoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, propyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, propyltrimethoxysilane, propyltriethoxysilane, paraffin and polyvinyl alcohol. One or more of the group.
[0135] The additive treatment is preferably one or more selected from the group consisting of a method of mixing a curing agent and a binder with a mixture, a method of mixing a curing agent with a mixture, and a method of mixing a binder with a mixture, and more preferably a method of mixing a curing agent and a binder with a mixture.
[0136] In the manufacturing method of this embodiment, the mixing step and the molding step may be repeated, or the mixing step may be performed under the same conditions except that the molded body obtained in the molding step is used instead of the ceramic continuous fiber. For example, the manufacturing method of this embodiment may include the mixing step and the molding step for 1 or more times but 5 or less times.
[0137] The method for producing CMC of the present invention includes a step of sintering the molded body (hereinafter also referred to as "sintering step"). Thus, the CMC of the present invention can be obtained. The sintering may be carried out under any conditions as long as the raw material powder can be sintered, and sintering under the following conditions can be mentioned.
[0138] Sintering atmosphere: oxidizing atmosphere or inactive atmosphere, preferably air atmosphere
[0139] Sintering temperature: above 800℃, above 900℃ or above 1000℃, and
[0140] Below 1600℃ or below 1500℃
[0141] Firing times: more than 1 time but less than 5 times
[0142] The firing time may be arbitrarily changed according to the size of the molded body (or calcined body) and the characteristics of the firing furnace used, and may be, for example, 30 minutes to 120 hours. When firing is performed multiple times, the firing atmosphere and firing temperature may be set to arbitrary conditions.
[0143] The sintering is preferably pressureless sintering because of its simplicity. In the present invention, "pressureless sintering" refers to a method of sintering by heating a sintered object (a molded body, a calcined body, etc.) without applying an external force.
[0144] The sintering step is preferably: sintering the molded body at 800°C or higher, preferably 800°C or higher and lower than 1000°C in an atmospheric atmosphere and atmospheric pressure to make a pre-calcined body, and sintering the pre-calcined body at 900°C or higher and 1600°C or lower, preferably 1000°C or higher and 1600°C or lower, and more preferably 1000°C or higher and 1500°C or lower in an atmospheric atmosphere and atmospheric pressure.
[0145] As another preferred sintering step, there can be mentioned a step of sintering the molded body at 800°C or higher and lower than 1000°C to obtain a pre-sintered body, sintering the pre-sintered body at 1000°C or higher and lower than 1150°C to obtain a primary sintered body, and sintering the primary sintered body at 1150°C or higher and 1500°C or lower. In this way, a denser CMC can be easily obtained. As sintering conditions in this sintering step, for example, the sintering method is normal pressure sintering, and the sintering atmosphere is an oxidizing atmosphere (preferably an air atmosphere).
[0146] Example
[0147] Hereinafter, the present invention will be described using examples, but the present invention is not limited to these examples.
[0148] (Heat exposure treatment)
[0149] The sintered CMC was kept at 1200° C. for 100 hours in an electric furnace (under atmospheric pressure and air atmosphere) and then cooled to room temperature.
[0150] (Tensile test)
[0151] Using a diamond cutter, cut the sintered CMC or the heat-exposed CMC into a width of 10±1mm, a length of more than 110mm, or 110±10mm and a thickness of 2±1mm to make a test piece that complies with JIS R 1656. Using an epoxy adhesive, aluminum pull tabs inclined at 14 degrees are installed at both ends of both sides as test pieces. Using a universal testing machine (device name: AG-XPlus, made by Shimadzu Corporation) and a tensile test fixture, a tensile test is performed at a load speed of 0.5mm / min. The cross-sectional area of the test piece is calculated based on the thickness and width of the test piece measured using a micrometer, and the tensile strength of the CMC is calculated using the cross-sectional area of the test piece and the maximum strength at break.
[0152] (Calculation of strength retention rate)
[0153] The tensile strength of the CMC after the heat exposure treatment was divided by the tensile strength of the CMC before the heat exposure treatment and converted into a percentage to obtain the strength retention rate.
[0154] (Calculation of average inhibitor particle size)
[0155] For CMC, a diamond cutter was used to cut the sample into a 5 mm square plate, and an argon ion beam irradiation cross-section polisher was used to make an observation section. For the observation section, a field emission scanning microscope with an energy dispersive characteristic X-ray analyzer (device name: JSM-7600F, manufactured by JEOL) was used to obtain EDS mapping data of silicon (sintering inhibitor) in the matrix at 5000 times, and the data was converted into a two-dimensional EDS mapping image using image analysis software (software name: ImageJ, manufactured by the National Institutes of Health, USA). The obtained mapping image (two-dimensional EDS mapping image) was binarized using image analysis software ImageJ with 8 bits and a threshold of 50 to obtain a processed image. The average inhibitor particle size of silicon (sintering inhibitor) was calculated based on the area of the white area using the processed image.
[0156] (Calculation of average center-of-gravity distance)
[0157] Using the processed image obtained in the same manner as for the average inhibitor particle size, the coordinates of the center of gravity of each white region corresponding to the sintering inhibitor in the image are determined by the following method.
[0158] The coordinates of the center of gravity of the white area are set as (Xg, Yg), and the coordinates of the center of gravity of each white area are calculated using the following formula: The long side of the processing image is set as the X axis, and the short side is set as the Y axis.
[0159] Xg = (the sum of the x-coordinate values of each unit pixel when the white area is divided) / the sum of the number of unit pixels constituting the white area
[0160] Yg = (the sum of the y coordinate values of each unit pixel when the white area is divided) / the sum of the number of unit pixels constituting the white area
[0161] The centroids of different white areas are connected by straight lines according to the criteria of (a) and (b) below, and the average length of the obtained line segments is calculated.
[0162] (a) Connect the centroids to each other in a way that they do not pass over other white areas.
[0163] (b) When a straight line connecting centroids intersects another straight line connecting centroids, the shorter straight line is used.
[0164] The coordinates of the center of gravity, the length of the line segment, and the average value were calculated using image analysis software (software name: NS2K-PRO, manufactured by NANOSYSTEM). The number of sintering inhibitors used for calculation was set to 150±50.
[0165] (Raw material particle size and average inhibitor source particle size)
[0166] The raw material particle size and the average inhibitor source particle size were determined using a laser diffraction / scattering particle size distribution measuring apparatus (apparatus name: MT3300EX-II, manufactured by Macrotrac BEL) according to a method in accordance with JIS R 1629. The measurement conditions are shown below.
[0167] Light source: semiconductor laser
[0168] Voltage: 780mW
[0169] Measurement sample: Slurry prepared by dispersing raw material powder in pure water
[0170] Refractive index of aluminum oxide: 1.77
[0171] Refractive index of zirconium oxide: 2.17
[0172] Refractive index of silicon dioxide: 1.48
[0173] Refraction of solvent (water): 1.333
[0174] Rate
[0175] Calculation mode: MT3000EXII
[0176] As a pretreatment, the sample powder and 0.2 mass % of an ammonium polyacrylate dispersant were suspended in pure water to prepare a slurry, and then a dispersion treatment was performed for 3 minutes using an ultrasonic homogenizer (device name: BRANSON SONIFIER 250, manufactured by Emerson).
[0177] (Fiber volume fraction)
[0178] The fiber volume ratio was calculated using the following formula from the mass of the ceramic continuous fibers, the density of the ceramic continuous fibers, and the volume of the CMC.
[0179] Fiber volume ratio [vol %] = (V f / V CMC )100
[0180] V f =m / ρ f
[0181] V CMC =A×B×t
[0182] In the above formula, V f is the volume of ceramic continuous fiber, V CMC is the volume of CMC, m is the mass of ceramic continuous fiber [g], ρ f is the density of ceramic continuous fiber [g / cm 3 ], A is the length of CMC [cm], B is the width of CMC [cm], and t is the thickness of CMC [cm].
[0183] (density)
[0184] Density is the ratio of volume measured by the Archimedean method to mass measured using an electronic balance according to JIS R 1634 (g / cm 3 Before the measurement, the mass of the dried CMC was measured, and then the CMC was placed in water and boiled for 3 hours as a pretreatment.
[0185] (Example 1)
[0186] 363 g of α-alumina powder with an average particle size (raw material particle size) of 0.15 μm (raw material powder amount (slurry): 72.8 mass%), 11.3 g of silica raw material (silicon dioxide powder) with an average particle size (inhibitor particle size) of 0.10 μm (inhibitor source amount (slurry): 2.2 mass%, inhibitor source amount: 3.1 mass%), and 125 g of pure water (25.0 mass% relative to the mass of the matrix slurry) were mixed, and then mixed with 1.2 kg of alumina balls with a diameter of 10 mm, and ball milled for 24 hours. Thus, a matrix slurry with a volume solid content concentration of 43 vol% (solid content concentration of 75 mass%) and a viscosity of 40.6 cP was obtained.
[0187] The commercially available mullite continuous fiber cloth (i.e., mullite and alumina continuous fiber cloth) (Nextel-720 manufactured by 3M Company) is heat treated (desizing) at 800°C in the air. The desizing mullite continuous fiber cloth is impregnated with the matrix slurry to obtain a mixture. The mixture is heat treated twice at 120±10°C for 6±2 hours to obtain a molded body having a width of 110 mm×a length of 130 mm×a thickness of about 2 mm (thickness 2.0 mm). The molded body is sintered at normal pressure at 900°C in the air to form a calcined body. After the calcined body is sintered at 1100°C in the air for 2 hours, it is heat treated (sintered) at 1200°C in the air to obtain CMC. The fiber volume ratio of the obtained CMC was 45 vol%, the tensile strength was 189 MPa, the tensile strength after heat exposure treatment was 175 MPa, the strength retention rate was 93%, the average particle size of silica in the matrix (average inhibitor particle size) was 0.11 μm (0.108 μm), and the average center-of-gravity distance was 2.0 μm.
[0188] (Example 2)
[0189] 363 g of α-alumina powder with an average particle size (raw material particle size) of 0.15 μm (raw material powder amount (slurry): 72.8 mass%), 11.3 g of silica raw material (silicon dioxide powder) with an average particle size (inhibitor particle size) of 0.24 μm (inhibitor source amount (slurry): 2.2 mass%, inhibitor source amount: 3.1 mass%), and 125 g of pure water (25.0 mass% relative to the mass of the matrix slurry) were mixed, mixed with 1.2 kg of alumina balls with a diameter of 10 mm, and ball milled for 24 hours. Thus, a matrix slurry with a volume solid content concentration of 43 vol% (solid content concentration of 75 mass%) and a viscosity of 36.9 cP was obtained.
[0190] The commercially available mullite continuous fiber cloth (i.e., mullite and alumina continuous fiber cloth) (Nextel-720 manufactured by 3M Company) is heat treated (desizing) at 800°C in the air. The desizing mullite continuous fiber cloth is impregnated with the matrix slurry to obtain a mixture. The mixture is heat treated twice at 120±10°C for 6±2 hours to obtain a molded body having a width of 110 mm×a length of 130 mm×a thickness of about 2 mm (thickness 2.1 mm). The molded body is sintered at normal pressure at 900°C in the air to form a calcined body. After the calcined body is sintered at 1100°C in the air for 2 hours, it is heat treated (sintered) at 1200°C in the air to obtain CMC. The fiber volume ratio of the obtained CMC was 43 vol%, the tensile strength was 189 MPa, the tensile strength after heat exposure treatment was 198 MPa, the strength retention rate was 105%, the average particle size of silica in the matrix (average inhibitor particle size) was 0.21 μm (0.211 μm), and the average center-of-gravity distance was 2.0 μm.
[0191] (Example 3)
[0192] 363 g of α-alumina powder with an average particle size (raw material particle size) of 0.15 μm (raw material powder amount (slurry): 72.8 mass%), 11.3 g of silica raw material (silicon dioxide powder) with a purity of 99.9% and an average particle size (inhibitor particle size) of 0.24 μm (inhibitor source amount (slurry): 2.2 mass%, inhibitor source amount: 3.1 mass%), and 125 g of water (25.0 mass% relative to the mass of the matrix slurry) were mixed, mixed with 1.2 kg of alumina balls with a diameter of 10 mm, and ball milled for 24 hours. A ceramic matrix slurry with a volume solid content concentration of 43 vol% (solid content concentration of 75 mass%) and a viscosity of 50.6 cP was obtained.
[0193] A commercially available alumina continuous fiber cloth (Nextel-610 manufactured by 3M Company) is heat treated (desizing) at 800°C in the air. The desizing alumina continuous fiber cloth is impregnated with a matrix slurry to obtain a mixture. The mixture is heat treated twice at 120±10°C for 6±2 hours to obtain a molded body having a width of 110 mm×a length of 130 mm×a thickness of about 2 mm (thickness 1.9 mm). The molded body is sintered at normal pressure at 900°C in the air to form a pre-calcined body. After the pre-calcined body is sintered at 1100°C in the air for 2 hours, it is heat treated (sintered) at 1200°C in the air to obtain CMC. The obtained CMC contained fibers having a fiber volume ratio of 43 vol%, a tensile strength of 221 MPa, a tensile strength after heat exposure treatment of 192 MPa, a strength retention rate of 87%, an average particle size of silica in the matrix (average inhibitor particle size) of 0.22 μm (0.221 μm), and an average center-of-gravity distance of 2.3 μm.
[0194] (Example 4)
[0195] 363 g of α-alumina powder with an average particle size (raw material particle size) of 0.15 μm (raw material powder amount (slurry): 72.8 mass%), 11.3 g of silica powder with a purity of 99.9% and an average particle size (inhibitor particle size) of 0.10 μm (inhibitor source amount (slurry): 2.2 mass%, inhibitor source amount: 3.1 mass%), and 125 g of water (25.0 mass% relative to the mass of the matrix slurry) were mixed, mixed with 1.2 kg of alumina balls with a diameter of 10 mm, and ball milled for 24 hours. Thus, a matrix slurry with a volume solid content concentration of 43 vol% (solid content concentration of 75 mass%) and a viscosity of 28.6 cP was obtained.
[0196] A commercially available alumina continuous fiber cloth (Nextel-610 manufactured by 3M Company) is heat treated (desizing) at 800°C in the air. The desizing alumina continuous fiber cloth is impregnated with a matrix slurry to obtain a mixture. The mixture is heat treated twice at 120±10°C for 6±2 hours to obtain a molded body having a width of 110 mm×a length of 130 mm×a thickness of about 2 mm (thickness 1.8 mm). The molded body is sintered at normal pressure at 900°C in the air to form a calcined body. After the calcined body is sintered at 1100°C in the air for 2 hours, it is heat treated (sintered) at 1200°C in the air to obtain CMC. The obtained CMC had a fiber volume ratio of 41 vol%, a tensile strength of 211 MPa, a tensile strength after heat exposure treatment of 207 MPa, a strength retention rate of 98%, an average inhibitor particle size of 0.15 (0.151) μm, and an average center-of-gravity distance of 2.7 μm.
[0197] (Example 5)
[0198] 358 g of α-alumina powder with an average particle size (raw material particle size) of 0.15 μm (raw material powder amount (slurry): 71.6 mass %), 11.3 g of silica powder with a purity of 99.9% and an average particle size (inhibitor particle size) of 0.24 μm (inhibitor source amount (slurry): 3.4 mass %, inhibitor source amount: 4.8 mass %), and 125 g of water (25.0 mass % relative to the mass of the matrix slurry) are mixed, mixed with 1.2 kg of alumina balls with a diameter of 10 mm, and treated in a ball mill for 24 hours to obtain a matrix slurry with a volume solid content concentration of 43 vol % (solid content concentration of 75 mass %) and a viscosity of 48.9 cP.
[0199] A commercially available alumina continuous fiber cloth (Nextel-610 manufactured by 3M Company) is heat treated (desizing) at 800°C in the air. The desizing alumina continuous fiber cloth is impregnated with a matrix slurry to obtain a mixture. The mixture is heat treated twice at 120±10°C for 6±2 hours to obtain a molded body having a width of 110 mm×a length of 130 mm×a thickness of about 2 mm (thickness 1.9 mm). The molded body is sintered at normal pressure at 900°C in the air to form a pre-calcined body. After the pre-calcined body is sintered at 1100°C in the air for 2 hours, it is heat treated (sintered) at 1200°C in the air to obtain CMC. The obtained CMC had a fiber volume ratio of 39 vol%, a tensile strength of 189 MPa, a tensile strength after heat exposure treatment of 189 MPa, a strength retention rate of 100%, an average inhibitor particle size of 0.22 (0.219) μm, and an average center-of-gravity distance of 1.8 μm.
[0200] (Example 6)
[0201] 363 g of α-alumina powder with an average particle size (raw material particle size) of 0.15 μm (raw material powder amount (slurry): 72.8 mass%), 11.3 g of silica powder with a purity of 99.9% and an average particle size (inhibitor particle size) of 2.4 μm (inhibitor source amount (slurry): 2.2 mass%, inhibitor source amount: 3.1 mass%), and 125 g of water (25.0 mass% relative to the mass of the matrix slurry) were mixed, mixed with 1.2 kg of alumina balls with a diameter of 10 mm, and ball milled for 24 hours. Thus, a matrix slurry with a volume solid content concentration of 43 vol% (solid content concentration of 75 mass%) and a viscosity of 58.1 cP was obtained.
[0202] A commercially available alumina continuous fiber cloth (Nextel-610 manufactured by 3M Company) is heat treated (desizing) at 800°C in the air. The desizing alumina continuous fiber cloth is impregnated with a matrix slurry to obtain a mixture. The mixture is heat treated twice at 120±10°C for 6±2 hours to obtain a molded body having a width of 110 mm×a length of 130 mm×a thickness of about 2 mm (thickness 1.9 mm). The molded body is sintered at normal pressure at 900°C in the air to form a pre-calcined body. After the pre-calcined body is sintered at 1100°C in the air for 2 hours, it is heat treated (sintered) at 1200°C in the air to obtain CMC. The fiber volume ratio of the obtained CMC was 41 vol%, the tensile strength was 222 MPa, the tensile strength after heat exposure treatment was 211 MPa, the strength retention rate was 95%, the average inhibitor particle size was 0.17 μm (0.166 μm), and the average center-of-gravity distance was 2.4 μm.
[0203] (Example 7)
[0204] 371 g of α-alumina powder with an average particle size (raw material particle size) of 0.15 μm (raw material powder amount (slurry): 74.3 mass%), 3.8 g of silica powder with a purity of 99.9% and an average particle size (inhibitor particle size) of 0.24 μm (inhibitor source amount (slurry): 0.75 mass%, inhibitor source amount: 1.0 mass%), and 125 g of water (25.0 mass% relative to the mass of the matrix slurry) were mixed, mixed with 1.2 kg of alumina balls with a diameter of 10 mm, and ball milled for 24 hours. Thus, a matrix slurry with a volume solid content concentration of 43 vol% (solid content concentration of 75 mass%) and a viscosity of 50.6 cP was obtained.
[0205] The commercially available mullite continuous fiber cloth (i.e., mullite and alumina continuous fiber cloth) (Nextel-720 manufactured by 3M Company) is heat treated (desizing) at 800°C in the air. The desizing mullite continuous fiber cloth is impregnated with the matrix slurry to obtain a mixture. The mixture is heat treated twice at 120±10°C for 6±2 hours to obtain a molded body having a width of 110 mm×length of 130 mm×thickness of 2.1 mm. The molded body is sintered at normal pressure at 900°C in the air to form a pre-calcined body. After the pre-calcined body is sintered at 1100°C in the air for 2 hours, it is heat treated (sintered) at 1200°C in the air to obtain CMC. The obtained CMC had a fiber volume ratio of 42 vol%, a tensile strength of 180 MPa, a tensile strength after heat exposure treatment of 181 MPa, a strength retention rate of 100%, an average inhibitor particle size of 0.11 (0.109) μm, and an average center-of-gravity distance of 2.2 μm.
[0206] In addition, the CMC of Example 7 was kept at 1200°C for 1000 hours in air atmosphere and then cooled to room temperature. The tensile strength of the treated CMC was 153 MPa, and the ratio of the tensile strength of the treated CMC to the tensile strength of the CMC before treatment was 85%.
[0207] (Comparative Example 1)
[0208] 363 g of α-alumina powder with an average particle size (raw material particle size) of 0.15 μm (raw material powder amount (slurry): 72.8 mass%), 11.3 g of silica powder with a purity of 99.9% and an average particle size (inhibitor particle size) of 0.05 μm (inhibitor source amount (slurry): 2.2 mass%, inhibitor source amount: 3.1 mass%), and 125 g of pure water (25.0 mass% relative to the mass of the matrix slurry) were mixed, and after mixing with 1.2 kg of alumina balls with a diameter of 10 mm, a ball mill treatment was performed for 24 hours. Thus, a matrix slurry with a volume solid content concentration of 43 vol% (solid content concentration of 75 mass%) and a viscosity of 21.6 cP was obtained.
[0209] The commercially available mullite continuous fiber cloth (i.e., mullite and alumina continuous fiber cloth) (Nextel-720 manufactured by 3M Company) is heat treated (desizing) at 800°C in the air. The desizing mullite continuous fiber cloth is impregnated with the matrix slurry to obtain a mixture. The mixture is heat treated twice at 120±10°C for 6±2 hours to obtain a molded body having a width of 110 mm×a length of 130 mm×a thickness of about 2 mm (thickness 2.4 mm). The molded body is sintered at normal pressure at 900°C in the air to form a pre-calcined body. After the pre-calcined body is sintered at 1100°C in the air for 2 hours, it is heat treated (sintered) at 1200°C in the air to obtain CMC. The fiber volume ratio of the obtained CMC was 39 vol%, the tensile strength was 132 MPa, the tensile strength after heat exposure treatment was 151 MPa, the strength retention rate was 109%, the average particle size of silica in the ceramic matrix (average inhibitor particle size) was 0.29 μm (0.287 μm), and the average center-of-gravity distance was 4.9 μm. The average particle size in the matrix (average inhibitor particle size) was larger than the average particle size of the silica powder of the raw material, which can be inferred that the silica powder agglomerated in the matrix slurry to form coarse particles. In addition, due to the large average center-of-gravity distance, the sintering inhibitor in the CMC of Comparative Example 1 is insufficient as a sintering inhibitor of alumina, that is, the effect of inhibiting the grain growth of alumina grains constituting the matrix is insufficient, so it can be considered that the CMC of Comparative Example 1 shows low tensile strength.
[0210] (Comparative Example 2)
[0211] 363 g of α-alumina powder with an average particle size (raw material particle size) of 0.15 μm (raw material powder amount (slurry): 72.8 mass%), 11.3 g of silica raw material (silicon dioxide powder) with a purity of 99.9% and an average particle size (inhibitor particle size) of 38 μm (inhibitor source amount (slurry): 2.2 mass%, inhibitor source amount: 3.1 mass%), and 125 g of pure water (25.0 mass% relative to the mass of the matrix slurry) were mixed, and then mixed with 1.2 kg of alumina balls with a diameter of 10 mm, and ball milled for 24 hours. Thus, a matrix slurry with a volume solid content concentration of 43 vol% (solid content concentration of 75 mass%) and a viscosity of 52.3 cP was obtained.
[0212] A commercially available mullite continuous fiber cloth (i.e., mullite and alumina continuous fiber cloth) (Nextel-720 manufactured by 3M Company) is heat treated (desizing) at 800°C in the air and impregnated with the matrix slurry to obtain a mixture. The mixture is heat treated twice at 120±10°C for 6±2 hours to obtain a molded body having a width of 110 mm×a length of 130 mm×a thickness of about 2 mm (thickness 2.4 mm). The molded body is sintered at 900°C in the air at normal pressure to obtain a calcined body. After the calcined body is sintered at 1100°C in the air, it is heat treated (sintered) at 1200°C in the air to obtain CMC. The fiber volume ratio of the obtained CMC was 41 vol%, the tensile strength was 115 MPa, the tensile strength after heat exposure treatment was 113 MPa, the strength retention rate was 98%, the average particle size of silica in the matrix (average inhibitor particle size) was 0.68 μm (0.675 μm), and the average center of gravity distance was 4.8 μm.
[0213] The fact that the average particle size (average inhibitor particle size) in the ceramic matrix is smaller than the average particle size of the raw material silica powder is presumed to be pulverized during the ball mill process when the ceramic matrix slurry is prepared. However, the average particle size (average inhibitor particle size) of silica in the ceramic matrix of Example 1 is larger and the average center of gravity distance is larger, so the effect of suppressing the sintering of alumina is weak, that is, the effect of suppressing the grain growth of alumina grains constituting the matrix is insufficient, which is considered to be the reason why the CMC of Comparative Example 2 shows a low tensile strength.
[0214] (Comparative Example 3)
[0215] 375 g of α-alumina powder (raw material powder amount (slurry): 75.0 mass %) with an average particle size (raw material particle size) of 0.15 μm and 125 g of pure water (25.0 mass % relative to the mass of the matrix slurry) were mixed, and then mixed with 1.2 kg of alumina balls with a diameter of 10 mm, and then subjected to ball milling for 24 hours. Thus, a matrix slurry with a volume solid content concentration of 43 vol% (solid content concentration of 75 mass %) and a viscosity of 28.6 cP was obtained.
[0216] The commercially available mullite continuous fiber cloth (i.e., mullite and alumina continuous fiber cloth) (Nextel-720 manufactured by 3M Company) is heat treated (desizing treatment) at 800°C in the air and impregnated with the matrix slurry to obtain a mixture. The mixture is heat treated twice at 120±10°C for 6±2 hours to obtain a molded body of 110 mm wide × 130 mm long × 2.1 mm thick. The molded body is sintered at normal pressure at 900°C in the air to form a pre-calcined body. After the pre-calcined body is sintered at 1100°C in the air for 2 hours, it is heat treated (sintered) at 1200°C in the air to obtain CMC. The fiber volume fraction of the obtained CMC is 43 vol%, the tensile strength is 93 MPa, the tensile strength after heat exposure treatment is 88 MPa, and the strength retention rate is 95%.
[0217] The results of CMC obtained in Examples and Comparative Examples are shown in the following table.
[0218] [Table 1]
[0219]
[0220] In Examples 1 to 7, it was confirmed that the average inhibitor particle size was 0.28 μm or less, and the strength before the heat exposure treatment was 150 MPa or more. In addition, it was confirmed that the strength retention rate was 80% or more, and the decrease in the strength of the CMC caused by the heat exposure treatment was suppressed. On the other hand, in the comparative examples, the average inhibitor particle size exceeded 0.28 μm, the strength before the heat exposure treatment was less than 150 MPa, and the strength of the CMC was low.
[0221] In addition, the average interatomic distance was confirmed to be 4.5 μm or less in all Examples 1 to 7. From this, it is presumed that the sintering inhibitor is uniformly dispersed in the matrix in the CMC of the Examples.
[0222] The entire contents of the specification, claims, drawings, and abstract of Japanese Patent Application No. 2020-216328 filed on December 25, 2020 are incorporated herein as the disclosure of the specification of this claim.
Claims
1. A ceramic matrix composite material, characterized in that: The invention comprises a ceramic matrix and ceramic continuous fibers, wherein the ceramic matrix contains a sintering inhibitor having an average particle size of 0.28 μm or less. The average distance between centers of gravity of the sintering inhibitor is 4.5 μm or less.
2. The ceramic matrix composite material according to claim 1, wherein: The average distance between the centers of gravity of the sintering inhibitor is not less than 0.03 μm and not more than 3.5 μm.
3. The ceramic matrix composite material according to claim 1 or 2, wherein: The sintering inhibitor is one or more selected from the group consisting of silicon dioxide, zirconium oxide, yttrium oxide, magnesium oxide, mullite, and strontium oxide.
4. The ceramic matrix composite material according to any one of claims 1 to 3, wherein The ceramic continuous fibers are continuous fibers of at least one oxide ceramic selected from the group consisting of alumina, silica, mullite, and zirconia.
5. The ceramic matrix composite material according to any one of claims 1 to 4, wherein The ceramic substrate is one or more oxides selected from the group consisting of alumina, mullite, and zirconia.
6. The ceramic matrix composite material according to any one of claims 1 to 5, characterized in that The ceramic matrix composite material has a tensile strength of 150 MPa or more, and a strength retention rate of 80% or more after heat exposure treatment at 1200° C. for 100 hours.
7. The method for producing a ceramic matrix composite material according to any one of claims 1 to 6, wherein: A molded body obtained by impregnating ceramic continuous fibers into a ceramic base slurry obtained by adding a sintering inhibitor having a purity of 99% or more to a ceramic base raw material powder and drying the mixture is sintered.
8. The method for producing a ceramic matrix composite material according to claim 7, wherein: The average particle size of the sintering inhibitor is more than 0.05 μm and less than or equal to 30 μm.