Environmentally friendly high-content palm oil putty concrete and preparation method thereof
Nano-scale palm putty ash is prepared by acid leaching, spray drying, supercritical carbon separation and grinding, and combined with an exciter, the problems of palm putty in concrete are solved, and the problems of coarse particles, many impurities and high carbon content in the concrete are achieved. High-volume resource utilization improves the comprehensive performance and economic and environmental benefits of concrete.
Patent Information
- Application Number
- CN202310550434.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-05-16
AI Technical Summary
In the prior art, palm putty ash has a coarse particle, a lot of impurities and a high carbon content, resulting in a decrease in the fluidity and mechanical properties of concrete, and a limited substitution rate, so it cannot fully exert its economic and environmental benefits.
Nano-grade palm putty ash is prepared by acid leach, spray drying, supercritical carbon separation, coarse grinding, fine grinding, etc., and combined with calcium-magnesium composite exciter and functional additives such as dodecyl phosphate, as the main gelling of concrete Materials to realize the resource utilization of large amounts of palm putty.
It improves the working performance, mechanical properties and durability of concrete, reduces the adverse effects of settling time, and realizes the high value-added resource utilization of palm putty solid waste, with significant economic and environmental benefits.
Smart Images

Figure BDA0004231198220000082 
Figure BDA0004231198220000091 
Figure BDA0004231198220000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and particularly relates to an environmentally friendly high-content palm oil putty concrete and a preparation method thereof. Background Art
[0002] At present, byproducts of power generation, steel smelting and agricultural product processing have been widely used as admixtures to replace traditional cement binders. Among them, industrial byproducts mainly include granulated blast furnace slag, fly ash, silica fume, etc., and agricultural byproducts mainly include corn cobs, wood waste ash, coconut shells and fibers, rice husk ash, etc. These industrial and agricultural solid wastes can replace cement after industrial processing, which can not only turn waste into treasure, but also improve and improve the comprehensive performance of concrete, with significant economic and environmental benefits.
[0003] Palm oil ash is a byproduct of palm oil mill combustion. It has very low commercial value and is difficult to recycle. It is usually buried directly in landfills, causing ecological pollution and land scarcity. Studies have shown that palm oil ash contains more than 55% silica and a certain amount of alumina and calcium oxide. Using palm oil ash as an auxiliary cementitious material to partially replace cement helps to react with calcium hydroxide produced during cement hydration to form calcium silicate hydrate (CSH) gel, thereby improving the mechanical properties and durability of concrete. However, palm oil ash obtained from palm oil mills usually has coarse particles (mostly larger than 300μm) and high impurities and carbon content. When palm oil fuel ash is directly used as a cement substitute, it will lead to problems such as reduced fluidity and mechanical properties of concrete and prolonged setting time. In addition, palm oil ash is currently only used as a partial substitute for cement, with a substitution rate mostly below 30%. Its substitution use in concrete is limited and cannot achieve good economic and environmental benefits.
[0004] Patent CN103539400A discloses a green high-performance concrete containing ultra-fine oil palm shell ash, but the final particle size is still large, and the carbon removal effect is limited. When it is used as an admixture to prepare concrete, it is easy to cause durability problems such as long initial and final setting time and insufficient impermeability, which limits the full use of the benefits of oil palm ash (only a maximum of 60% cement replacement can be achieved). Therefore, further exploring the high-value-added resource utilization of palm oil ash in the fields of concrete and the like has important economic, environmental and application significance. Summary of the invention
[0005] The main purpose of the present invention is to provide an environmentally friendly high-content palm oil ash concrete in view of the problems and shortcomings of the prior art. First, nano-scale palm oil ash is prepared by acid leaching, spray drying, supercritical carbon separation, coarse grinding, fine grinding and other treatments on palm oil combustion ash; then it is used as the main cementitious material of concrete, and combined with functional additives such as stimulating materials and admixtures, while realizing the resource utilization of large-content palm oil ash, effectively taking into account the better working performance, mechanical properties and durability of the obtained palm oil ash concrete, and basically having no adverse effect on the setting time of concrete, thereby realizing the high-value-added resource utilization of palm oil ash solid waste, and having significant economic and environmental benefits.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] The invention discloses an environmentally friendly high-content palm oil putty concrete, wherein the components and their weight proportions include: 80-150 parts of cement, 360-430 parts of ultrafine palm oil putty, 950-1050 parts of crushed stone, 580-640 parts of sand, 70-100 parts of calcium-magnesium composite activator, 80-100 parts of water, 2-3 parts of lauryl phosphate and 5-7 parts of water reducing agent.
[0008] In the above scheme, the ultrafine palm oil ash is obtained by sequentially subjecting palm oil combustion ash to acid leaching, spray drying, supercritical carbon separation, coarse grinding and fine grinding; its SiO2 content is greater than 68wt%, Al2O3 content is greater than 7wt%, and Fe2O3 content is greater than 6.0wt%; the average particle size is 200-350nm, and the specific surface area is 5.0-6.2m 2 / g, density 2.3~2.5g / cm 3 , the carbon content is less than 0.5wt%.
[0009] In the above scheme, the SiO2 content in the palm oil combustion ash is less than 60wt%, the SiO2+Al2O3+Fe2O3 content is less than 70wt%, the unburned carbon content is greater than 15wt%, and the average particle size is 50-200μm.
[0010] In the above scheme, the acid leaching step includes: adding palm oil putty into a citric acid solution and soaking it for 4 to 6 hours to remove grease, chloride ions and sulfate ions on the surface of the palm oil putty; then taking it out and washing it with water; through acid leaching, the adhesion between particles can be reduced and the efficiency of spray drying can be improved.
[0011] In the above scheme, the concentration of the citric acid solution is 8-10wt%.
[0012] In the above scheme, the drying step adopts a spray drying method to quickly dry the palm oil putty into dispersed particles with a moisture content of less than 3%.
[0013] Furthermore, the spray drying method adopts a centrifugal spray tower with a centrifugal speed of 10000-15000 r / min and an air intake volume of 320-350 m 3 / H, spray drying time is 5 to 10s.
[0014] In the above scheme, the supercritical carbon separation step includes: 1) adding water to the palm oil ash after spray drying and stirring evenly to obtain a mixed slurry, then adding oleic acid and hexadecyltrimethylammonium bromide, performing ultrasonic vibration treatment, and removing the surface floating liquid; 2) placing the obtained pretreated slurry in a reactor, passing ethanol supercritical fluid to perform supercritical carbon separation; then performing solid-liquid separation, washing with water, and drying.
[0015] In the above scheme, the solid content of the mixed slurry is 50-60%.
[0016] In the above scheme, the oleic acid accounts for 0.4-0.6% of the water mass in the mixed slurry, and the purity of oleic acid is ≥98%; the hexadecyltrimethylammonium bromide accounts for 0.4-0.8% of the water mass in the mixed slurry.
[0017] In the above scheme, the ultrasonic oscillation treatment time is 10 to 20 minutes.
[0018] In the above scheme, the mass of the ethanol supercritical fluid (calculated as the amount of ethanol before treatment) accounts for 6-8% of the mass of the pre-treated slurry in step 2).
[0019] In the above scheme, the conditions for producing the ethanol supercritical fluid include: pressure 6.4-6.5MPa, temperature 243.1-245°C.
[0020] In the above scheme, the gas flow rate used in the supercritical carbon separation step is set to 0.1-0.2 ml / min; the separation treatment time is 10-20 min.
[0021] In the above scheme, the coarse grinding step adopts a rod mill process, and the specific steps include: adding chitosan solution to palm oil putty treated by supercritical carbon separation, and rod milling at a speed of 200 to 300 r / min for 40 to 60 minutes.
[0022] Furthermore, the concentration of the chitosan solution is 1-1.5wt%, and the amount added is 0.2-0.5% of the mass of the palm oil ash after supercritical carbon separation.
[0023] In the above scheme, the fine grinding step adopts a ball milling process, and the specific steps include: ball milling at a speed of 300-400r / min for 40-60min.
[0024] The invention firstly soaks palm oil putty with a citric acid solution to remove impurities such as grease, chloride ions and sulfate ions on the surface of palm oil putty, and then quickly dries and disperses the palm oil putty into fine particles by a spray drying method, which is conducive to more efficient supercritical carbon separation. In the supercritical carbon separation, oleic acid and hexadecyltrimethylammonium bromide are firstly used to separate and adsorb most of the activated carbon and unburned carbon in the palm oil putty onto the surface of the solution, and in view of the problem that there are still fine particles in the interior and in the water that cannot float out, the ethanol in the supercritical state is further penetrated into the gaps of the palm oil putty through the high diffusion and high permeability, and the tiny carbon particles are adsorbed and brought into the water and then floated out, and finally solid-liquid separation is performed. The carbon content in the palm oil putty can be greatly reduced, and the later grinding efficiency and the application effect in concrete are improved.
[0025] The present invention further adopts a coarse grinding + fine grinding process to prepare ultrafine palm oil putty. First, a rod mill is used for coarse grinding. For palm oil putty with a larger particle size, coarse grinding by a rod mill can make the material more uniform, and most of the particles are ground to a particle size below 5 μm. At the same time, chitosan (a natural polysaccharide substance from crabs, shrimps or shellfish, etc.) is introduced during the coarse grinding process. Its good lubrication and adsorption capacity are used to reduce the friction between the abrasive and the ground material, prevent the abrasive from agglomerating and settling, and improve the dispersion and grinding efficiency and quality of the palm oil putty. A ball mill with a higher degree of fineness is then used for fine grinding, so that the fineness of the palm oil putty is further increased, the specific surface area is increased, and finally nano-level ultrafine palm oil putty is obtained.
[0026] When the ultrafine palm oil ash with extremely low carbon content obtained by the present invention is used to prepare concrete, the main components such as silicon dioxide rich in the palm oil ash can be used to produce silicate ions when fully in contact with water, and the silicate ions can promote the hydrolysis reaction of C3S in cement; the nano-scale palm oil ash particles can serve as the nucleation site of CSH seeds, and promote the rapid formation of CSH gel; with the increase of age, Ca(OH)2 generated by the continuous hydration reaction of cement, the silicon dioxide in the palm oil ash can accelerate the consumption of Ca(OH)2 in the slurry, promote the volcanic ash reaction, and generate CSH gel (2S+3CH=C3S2H); the formed hydration products can fill large capillary holes, and then form a dense and uniform cement stone microstructure.
[0027] In the above scheme, the cement can be selected from P·O42.5 ordinary silicate cement, etc., and its specific surface area is 340-360m 2 / kg.
[0028] In the above scheme, the particle size of the crushed stone is 5-10 mm, the parent rock is dolomite, and the apparent density is 2400-2700 kg / m 3 .
[0029] In the above scheme, the sand is stone powder machine-made sand with a particle size of 0 to 5 mm, its parent rock is dolomite, the fineness modulus is 2.6 to 3.0, and the passing percentage after passing through a 0.15 mm sieve is less than 15%.
[0030] The dolomite aggregate used in the present invention has low alkali activity, which can effectively inhibit the alkali-aggregate reaction and effectively avoid the alkali-aggregate reaction problem of palm oil putty concrete that is easily caused by the introduction of magnesium hydroxide solution; the dolomite aggregate dissolves in water to produce Ca 2+ , which can stabilize the Mg(OH)2-SiO2-H2O gel generated by magnesium hydroxide and silicon dioxide.
[0031] The lauryl phosphate introduced in the present invention has the dual properties of hydrophilicity and lipophilicity, which can effectively increase the contact area between palm oil putty particles and water, reduce surface tension, improve the wettability and coverage area of water on the surface of palm oil putty, and accelerate the rate of hydrolysis of silicate ions of palm oil putty in water.
[0032] In the above scheme, the water reducing agent is a naphthalene-based high-efficiency water reducing agent with a water reducing rate of 30-36%; it has better chemical stability and adaptability in concrete with high alkalinity.
[0033] In the above scheme, the calcium-magnesium composite activator is obtained by compounding a calcium oxide-magnesium hydroxide aqueous solution with polyethylene glycol; wherein the concentration of the calcium oxide-magnesium hydroxide aqueous solution (the total concentration of calcium oxide and magnesium hydroxide) is 0.5-1 mol / L; and the amount of polyethylene glycol used accounts for 5-8% of the mass of the calcium oxide-magnesium hydroxide aqueous solution.
[0034] In the above scheme, the calcium oxide-magnesium hydroxide aqueous solution is prepared by adding calcium oxide and magnesium hydroxide into water and adopting a heating ultrasonic method; wherein the mass ratio of calcium oxide to magnesium hydroxide is (1-1.3):(0.1-0.13).
[0035] Furthermore, the ultrasonic power used in the heating ultrasonic method is 250-350W, the heating temperature is 80-90°C, and the heating ultrasonic time is 20-30min.
[0036] Furthermore, the particle size of the magnesium hydroxide powder introduced in the preparation of the calcium-magnesium composite activator is 10-20 nm, and the average molecular weight of the polyethylene glycol is 1000-2000.
[0037] The calcium oxide and magnesium hydroxide introduced in the present invention decompose into alkaline hydroxide ions (OH - ), promoting the reaction rate of cement and water, hydroxide ions (OH -) can promote the silicon dioxide and aluminum oxide in nano-scale palm oil putty to form a three-dimensional network structure of aluminosilicate gel, thereby improving the strength and density of palm oil putty concrete; CaO can provide a large amount of free Ca 2+ , making the system easier to form calcium silicate hydrate gel (CSH). Some incompletely hydrolyzed magnesium hydroxide, silicon dioxide in palm oil putty and water in concrete can generate a small amount of Mg(OH)2-SiO2-H2O gel, which improves the overall strength of concrete. The Ca precipitated from dolomite 2+ ions and free Ca provided by CaO 2+ As a divalent cation, it can enter the Mg(OH)2-SiO2-H2O gel in small amounts to reduce its surface negative charge and stabilize it. In addition, in view of the problem that calcium hydroxide and magnesium hydroxide are prone to precipitation in concrete, the present invention further compounds them with polyethylene glycol, and utilizes the good solubility and dispersibility of polyethylene glycol to effectively improve the dispersion effect of calcium hydroxide and magnesium hydroxide in concrete, thereby ensuring and promoting the use effect of the composite calcium-magnesium solution.
[0038] The method for preparing the above-mentioned environmentally friendly high-content palm oil putty concrete comprises the following steps:
[0039] 1) Weigh each component according to the proportion, and each component and its weight proportion include: 80-150 parts of cement, 360-430 parts of ultrafine palm oil putty, 950-1050 parts of crushed stone, 580-640 parts of sand, 70-100 parts of calcium-magnesium composite activator, 80-100 parts of water, 2-3 parts of lauryl phosphate, and 5-7 parts of water reducer;
[0040] 2) Mix the weighed cement, ultrafine palm oil putty, crushed stone and sand evenly (1.5-2 minutes); then add calcium-magnesium composite activator and mix evenly (4-6 minutes); then add water, lauryl phosphate and water reducing agent and mix evenly (4-5 minutes) to obtain a concrete mixture;
[0041] 3) The concrete mixture is poured out of the machine, vibrated and formed, then left to stand, the mold is removed, and then heated for thermosetting treatment, and then standard curing is carried out to obtain palm oil putty concrete specimens.
[0042] In the above scheme, the standing temperature is 24-26°C.
[0043] In the above scheme, the heat curing treatment temperature is 60-65°C and the time is 20-24h.
[0044] The present invention can effectively improve the preparation quality of palm oil putty admixtures, prepare nano-scale palm oil putty with a low carbon content, and can achieve a cement replacement amount of up to 85% in concrete by combining with other excitation systems and admixtures, while taking into account the good working performance, mechanical properties and durability of the obtained palm oil putty concrete.
[0045] Compared with the prior art, the present invention has the following beneficial effects:
[0046] (1) The present invention adopts acid washing, spray drying, supercritical carbon separation, rod mill coarse grinding, ball mill fine grinding and other means to prepare nano palm oil ash; it can effectively remove impurities in the original palm oil combustion ash, reduce the carbon content, increase the percentage of volcanic ash minerals, enhance the gelling effect after combining with water, compact the microstructure of cement stone, and effectively improve the comprehensive performance of the obtained concrete; and it has high production efficiency and is suitable for popularization and application.
[0047] (2) With the synergistic effect of nano-scale palm oil putty, calcium-magnesium composite activator, lauryl phosphate surfactant and other substances, the dosage of palm oil putty in cementitious materials can be more than 70% (up to 85%), and at the same time, it can effectively avoid the problems of insufficient early strength and easy cracking caused by palm oil putty concrete, effectively taking into account the good working performance, mechanical properties and durability of the obtained concrete, and basically has no adverse effect on the setting time of concrete, with good economic and environmental benefits. DETAILED DESCRIPTION
[0048] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] In the following examples, the cement used is ordinary Portland cement P·O52.5; the particle size of the coarse aggregate crushed stone (dolomite) is 5 to 10 mm; the stone powder machine-made sand (dolomite) is prepared by a dry process, with a particle size of 0 to 5 mm and a fineness modulus of 2.6 to 3.0.
[0050] The naphthalene-based high-efficiency water-reducing agent used has a water reduction rate of 33% and a solid content of 36%; the SBTJM-A naphthalene-based high-efficiency water-reducing agent provided by Subote.
[0051] Example 1
[0052] A method for preparing ultrafine palm oil putty comprises the following steps:
[0053] 1) 10 kg of raw palm oil ash was added to a citric acid solution (9 wt%) and soaked for 5 h. After being taken out, it was washed with water for 15 min. Then the palm oil ash was quickly dried by spray drying (centrifugal spray tower, centrifugal speed of 12000 r / min, air intake of 320 m 3 / H, spray drying time is 8s) into dispersed particles with a moisture content of less than 3%; add water to the palm oil ash after spray drying to prepare a mixed slurry with a solid content of 50%, then add oleic acid accounting for 0.4% of the water mass in the mixed slurry and cetyltrimethylammonium bromide accounting for 0.5% of the water in the mixed slurry, respectively, and after ultrasonic vibration treatment for 15 minutes, clean the surface floating liquid; then place the obtained pre-treated slurry in a reactor, and pass ethanol supercritical fluid into it for supercritical carbon separation for 15 minutes (ethanol supercritical fluid is formed under the conditions of pressure 6.5MPa and temperature 244°C, the amount accounts for 7% of the mass of the pre-treated slurry, and the gas flow rate is 0.1ml / min); then perform solid-liquid separation, water washing and drying;
[0054] 2) adding a chitosan solution (1.4 wt % chitosan solution, 0.4 wt % of the mass of the palm oil putty) to the palm oil putty treated by supercritical carbon separation, adding 30 to 40 low-carbon steel rods with a diameter of 8 mm and a length of 400 mm to a rod mill, and grinding the rods at 250 r / min for 50 min; then taking out the palm oil putty and putting it into a ball mill, putting in steel balls with a diameter of 16 to 20 mm, and grinding the ball mill at a speed of 350 r / min for 50 min to obtain nano-level ultrafine palm oil putty.
[0055] Comparative Example 1
[0056] A kind of ground palm oil ash is obtained by drying the original palm oil combustion ash of the factory described in Example 1 in an environment of 105° C. for 24 hours, directly adding it into a ball mill, and ball milling it at a speed of 350 r / min for 100 minutes, and then taking it out.
[0057] Comparative Example 2
[0058] A kind of ground palm oil ash, after the original palm oil combustion ash of the factory described in Example 1 is dried in an environment of 105°C for 24 hours, it is ball-milled in a ball mill at 350r / min for 100min, taken out and calcined in a calcining furnace at 500°C for 90min; then it is taken out and sieved, and it is ball-milled in a ball mill at 350r / min for 100min again.
[0059] The palm oil putty obtained in Example 1 and Comparative Examples 1-2 was analyzed by scanning electron microscopy. The results showed that: the surface of the palm oil putty particles obtained in Example 1 was basically free of pores, and the particles were mainly round; the palm oil putty particles obtained in Comparative Example 1 were irregularly angular and had more pores on the surface, while the surface of Comparative Example 2 still had some pores compared to Example 1, and the round particles were relatively less; in addition, the average particle size of the particles obtained in Example 1 was about 300 nm, and the average particle size of the particles obtained in Comparative Example 2 was about 2-3 μm.
[0060] The carbon content of the palm oil ash obtained in Example 1, Comparative Example 1 and Comparative Example 2 was analyzed by X-ray fluorescence spectrometry and found that the carbon content of the palm oil ash obtained in Example 1 was 0.4%, while the carbon content of the palm oil ash obtained in the original and Comparative Example 1 was greater than 15.3%, and the carbon content of the palm oil ash obtained in Comparative Example 2 was 3.8%. If the carbon content of palm oil ash is too high, solid carbon particles will occupy the micropores and pores inside the concrete, resulting in a decrease in the effective filling rate in the concrete, thereby reducing the density and durability of the concrete; at the same time, it will hinder the reaction of cement and other components in the concrete to a certain extent, resulting in problems such as a longer setting and curing time of the concrete.
[0061] The chemical components of the palm oil ash obtained in the embodiment and the comparative example were analyzed using a SEM / EDX detector, and the test results include the following:
[0062] (1) Example 1: The content of SiO2+Al2O3+Fe2O3 is 84.02%, of which the content of SiO2 is 69.5%;
[0063] (2) Original palm oil ash: SiO2+Al2O3+Fe2O3 content is 68.4%, of which SiO2 content is 56.4%;
[0064] (3) Comparative Example 1: The content of SiO2+Al2O3+Fe2O3 is 71.4%, of which the content of SiO2 is 58.3%;
[0065] (4) Comparative Example 2: The content of SiO2+Al2O3+Fe2O3 is 77.2%, of which the content of SiO2 is 61.4%.
[0066] Through SEM / EDX analysis, it is found that the volcanic ash mineral (SiO2, Fe2O3 and Al2O3) content in the palm oil ash obtained in Example 1 is higher than that in Comparative Example 1 and Comparative Example 2. The total volcanic ash mineral content of Example 1 is 17.6% and 8.8% higher than that of Comparative Example 1 and Comparative Example 2, respectively. In addition, the SiO2 content of the palm oil ash in Example 1 is close to 70%. The palm oil ash with a high SiO2 content can effectively promote cement hydration and form CSH required for concrete strength.
[0067] Example 2
[0068] A high-content palm oil putty concrete, the preparation method of which comprises the following steps:
[0069] 1) Weighing raw materials, each raw material and its weight proportion are: 150 parts of cement, 360 parts of ultrafine palm oil putty (obtained in Example 1, the same below), 1050 parts of coarse aggregate crushed stone, 580 parts of stone powder machine-made sand, 70 parts of calcium-magnesium composite activator, 100 parts of water, 2 parts of lauryl phosphate, and 5 parts of water reducer; wherein the calcium-magnesium composite activator used is an aqueous solution with a total concentration of 0.6 mol / L prepared by mixing calcium oxide and magnesium hydroxide in a mass ratio of 1:0.1 by using a heated ultrasonic method (ultrasonic power of 280 W, heating temperature of 85° C., and heating ultrasonic time of 25 min), and then adding polyethylene glycol accounting for 5% of the mass of the aqueous solution, mixing evenly, to form a calcium-magnesium composite activator;
[0070] 2) Weigh each component by weight, and dry mix the weighed cement, ultrafine palm oil putty, coarse aggregate crushed stone, and stone powder machine-made sand in a mixing pot for 1.5 minutes;
[0071] 3) Add calcium-magnesium composite activator and continue mixing for 4 minutes, then add water, lauryl phosphate and water reducing agent and mix for 4 minutes to obtain a concrete mixture;
[0072] 4) After the concrete mixture is poured and vibrated into shape, it is placed in an environment of 25°C for 24 hours before demolding. The test block is then placed in a high temperature environment of 62°C for thermal curing for 22 hours before being taken out. Subsequently, it is cured in a standard curing room to the age, and the palm oil putty concrete specimen is obtained.
[0073] Example 3
[0074] A high-content palm oil putty concrete, the preparation method of which comprises the following steps:
[0075] 1) Weigh the raw materials, and the raw materials and their weight proportions are: 80 parts of cement, 430 parts of ultrafine palm oil putty (obtained in Example 1, the same below), 950 parts of coarse aggregate crushed stone, 640 parts of stone powder machine-made sand, 100 parts of calcium-magnesium composite activator (prepared under the same conditions as in Example 2), 80 parts of water, 3 parts of lauryl phosphate, and 7 parts of water reducer;
[0076] 2) Weigh each component by weight, and dry mix the weighed cement, ultrafine palm oil putty, coarse aggregate crushed stone, and stone powder machine-made sand in a mixing pot for 2 minutes;
[0077] 3) Add calcium-magnesium composite activator and continue mixing for 5 minutes, then add water, lauryl phosphate and water reducing agent and mix for 5 minutes to obtain a concrete mixture;
[0078] 4) After the concrete mixture is poured and vibrated into shape, it is placed in a 26°C environment for 24 hours before demolding. The test block is then placed in a 62°C high temperature environment for heat curing for 24 hours before being taken out. It is then cured in a standard curing room to the age, and the palm oil putty concrete specimen is obtained.
[0079] Comparative Example 3
[0080] A high-content palm oil putty concrete, the preparation method of which is substantially the same as that of Example 2, except that: no calcium-magnesium composite activator and dodecyl phosphate are added.
[0081] Comparative Example 4
[0082] A high-content palm oil putty concrete, the preparation method of which is substantially the same as that of Example 2, except that: no calcium-magnesium composite activator is added, and MgO (analytical grade, purity ≥98%) accounting for 10% of the total mass of the cementitious material is added.
[0083] The stimulating effect of MgO on palm oil putty is mainly achieved through Mg(OH)2. When MgO meets water, it will preferentially react with water to generate Mg(OH)2, forming an alkaline environment. However, the direct addition of MgO is usually prone to cause excessive Mg(OH)2 insoluble matter to form in the concrete, which precipitates in the concrete and occupies the voids that should be filled by CSH gel, affecting continuous hydration and further affecting the strength and density of the concrete. The measured 7d compressive strength of the palm oil putty concrete obtained in Comparative Example 2 is 69.9MPa, and the 28d compressive strength is 92.3MPa; the initial setting time and final setting time are 4.6h and 7.4h respectively; the 28d chloride ion diffusion coefficient is 1.02×10 -12 m 2 / s.
[0084] Comparative Example 5
[0085] A concrete with a high content of palm oil putty, the preparation method of which is substantially the same as that of Example 3, except that the ultrafine palm oil putty is replaced by the palm oil putty in Comparative Example 2.
[0086] With reference to the provisions of GB / T50080-2016 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures" and GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Ordinary Concrete", the working performance and mechanical properties of the fresh concrete of the embodiments and comparative examples were tested, and the test results are shown in Table 2.
[0087] Table 2 Working performance and mechanical properties of palm oil putty concrete
[0088]
[0089] It can be seen from Table 2 that the slump of the palm oil putty concrete obtained by the present invention is basically above 220 mm, and the fluidity and cohesion are good. When the palm oil putty content is close to 85%, the slump can still reach 220 mm. The palm oil putty concrete prepared by the traditional calcined ball milling method used in Comparative Example 5 has a slump of 180 mm, and there is more unburned carbon inside it, absorbing a large amount of water reducer, and the fineness is relatively large, the dispersibility is insufficient, and the cohesion performance is relatively poor. When it is used in a large amount, the disadvantages are particularly obvious.
[0090] The compressive strength test results of concrete show that the compressive strength of the palm oil putty concrete obtained by the present invention decreases with the increase of palm oil putty content at each age, but the amplitude is small. When the content is close to 85%, the 28d compressive strength can still reach 106.2MPa, which is 8.2% higher than the 28d compressive strength of the concrete obtained in Comparative Example 1. And the 7d strength in Examples 2 to 3 can basically reach 80% of the 28d strength, and the early strength growth rate is significantly improved compared with the comparative example. In addition, as the content of palm oil putty increases, its effect on the setting time of concrete is relatively small. Compared with Comparative Examples 3 and 5, the initial and final setting times are both advanced, which is conducive to the rapid formation of concrete strength, improving construction speed and rapid turnover of formwork.
[0091] With reference to GB / T50082-2009 “Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete”, shrinkage test, chloride ion penetration test and early crack resistance plate test were carried out on concrete. The test results are shown in Table 3.
[0092] Table 3 Drying shrinkage and early crack resistance of palm oil putty concrete
[0093]
[0094] It can be seen from the test results that the 28d chloride ion diffusion coefficient of the palm oil ash concrete obtained by the present invention reaches 0.84 and 0.66 at 70% and 85% dosage (relative to the total amount of cementitious materials), and the concrete structure is relatively dense, and the anti-permeability performance is excellent and significantly better than other comparative examples. The drying shrinkage value of the palm oil ash concrete obtained in Examples 2 to 3 is significantly lower than that of the comparative example, which is mainly attributed to the high filler effect and volcanic ash activity of nano-scale palm oil ash. On the one hand, the small-sized palm oil ash particles with extremely low carbon content have good adaptability to admixtures and can absorb excess free water; on the other hand, the nano-scale palm oil ash can further synergize with the calcium-magnesium composite activator and the lauryl phosphate-based surfactant to reduce the pore size of the concrete and make the concrete structure more dense, thereby improving the anti-permeability and compacting effect of the concrete, reducing water evaporation and drying shrinkage. From the early anti-cracking flat plate test results, it can be found that the total cracking area per unit area of the concrete obtained in Examples 2 to 3 is less than 100, and the final cracking grade is grade V. The final crack resistance grade of the concrete in the comparative example was maintained at Grade IV, and its crack resistance performance was relatively average.
[0095] The above results show that: the scheme of the present invention can realize the large-amount application of palm oil putty, avoiding the problems of poor workability, insufficient early and late strength, prolonged setting and curing time, poor corrosion resistance, easy cracking, etc. that are easily caused by the large-amount application of palm oil putty concrete; while realizing the large-amount use of palm oil putty in concrete, it can effectively take into account the good working mechanical properties, construction characteristics and durability of concrete, etc., and has good economic and environmental benefits.
[0096] The present invention is not limited to the above-mentioned embodiments. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention. The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.
Claims
1. An environmentally friendly high-content palm oil putty concrete, It is characterized in that The components and their weight proportions include: 80-150 parts of cement, 360-430 parts of ultrafine palm oil putty, 950-1050 parts of crushed stone, 580-640 parts of sand, 70-100 parts of calcium-magnesium composite activator, 80-100 parts of water, 2-3 parts of lauryl phosphate, and 5-7 parts of water reducer; The ultra-fine palm oil ash is obtained by sequentially subjecting palm oil combustion ash to acid leaching, spray drying, supercritical carbon separation, coarse grinding and fine grinding; the SiO 2 Content greater than 68wt%, Al 2 O 3 Content greater than 7wt%, Fe 2 O 3 The content is greater than 6.0wt%; the average particle size is 200~350nm, and the carbon content is less than 0.5wt%.
2. Palm oil putty concrete according to claim 1, It is characterized in that The supercritical carbon separation step comprises: 1) adding water to the spray-dried palm oil ash and stirring evenly to obtain a mixed slurry, then adding oleic acid and hexadecyltrimethylammonium bromide, performing ultrasonic vibration treatment, and removing the surface floating liquid; 2) placing the obtained pre-treated slurry in a reactor, and introducing ethanol supercritical fluid to perform supercritical carbon separation; and then performing solid-liquid separation, water washing, and drying.
3. Palm oil putty concrete according to claim 1, It is characterized in that The coarse grinding step adopts a rod mill process, and the specific steps include: adding chitosan solution to the palm oil putty treated by supercritical carbon separation, and rod milling at a speed of 200-300 r / min for 40-60 minutes.
4. Palm oil putty concrete according to claim 1, It is characterized in that The fine grinding step adopts a ball milling process, and the specific steps include: ball milling at a speed of 300-400 r / min for 40-60 minutes.
5. Palm oil putty concrete according to claim 1, It is characterized in that The particle size of the crushed stone is 5-10 mm, the parent rock is dolomite, and the apparent density is 2400-2700 kg / m 3 .
6. Palm oil putty concrete according to claim 1, It is characterized in that The sand is machine-made sand with a particle size of 0-5 mm. The parent rock is dolomite, the fineness modulus is 2.6-3.0, and the passing percentage after passing through a 0.15 mm sieve is less than 15%.
7. Palm oil putty concrete according to claim 1, It is characterized in that The water reducing agent is a naphthalene-based high-efficiency water reducing agent, and its water reducing rate is 30-36%.
8. Palm oil putty concrete according to claim 1, It is characterized in that The calcium-magnesium composite activator is obtained by compounding a calcium oxide-magnesium hydroxide aqueous solution with polyethylene glycol; The concentration of the calcium oxide-magnesium hydroxide aqueous solution is 0.5-1 mol / L; the amount of polyethylene glycol used accounts for 5-8% of the mass of the calcium oxide-magnesium hydroxide aqueous solution.
9. The method for preparing the environmentally friendly high-content palm oil putty concrete according to any one of claims 1 to 8, It is characterized in that The following steps are involved: 1) Weigh each component according to the proportion, and each component and its weight percentage include: 80-150 parts of cement, 360-430 parts of ultrafine palm oil putty, 950-1050 parts of crushed stone, 580-640 parts of sand, 70-100 parts of calcium-magnesium composite activator, 80-100 parts of water, 2-3 parts of lauryl phosphate, and 5-7 parts of water reducer; 2) Mix the weighed cement, ultrafine palm oil putty, crushed stone and sand evenly; then add calcium-magnesium composite activator and stir evenly, then add water, lauryl phosphate and water reducing agent and stir evenly to obtain a concrete mixture; 3) After the concrete mixture is poured out of the machine and vibrated into shape, it is left to stand, the mould is removed, and then heat-cured and standardly cured to obtain palm oil putty concrete specimens.
Citation Information
Patent Citations
Green high-performance concrete with superfine oil palm fruit shell ash
CN103539400A
Palm oil fuel ash based mortar compositions
US20210024416A1
Alkali-activated concrete containing palm oil fuel ash
US20210039997A1
Concrete composition containing palm oil fuel ash
US20210380485A1
High strength concrete based on palm oil fuel ash
WO2013019100A1