Antioxidant for rubber and preparation method thereof
Through the design of loaded antioxidants and the chemical bonding of the composite with components such as chitosan/nano-silica hybrid materials, the problem of easy migration and volatilization of existing rubber antioxidants has been solved, and the resistance of rubber has been improved. Oxidation properties and service life, especially aging resistance in high temperature environments.
Patent Information
- Application Number
- CN202310849974.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-07-12
AI Technical Summary
Existing rubber antioxidants are easy to migrate and volatilize, resulting in poor long-term protection and pollution to the environment. In addition, the oxidation reaction speed is fast in high temperature environments, affecting the service life and performance of rubber.
Using a loaded antioxidant, the compound, tri-(2,4-di-tert-butylphenyl) phosphite, chitosan/nano-silica hybrid material, white carbon black, and 2-nonyl Components such as hydrogen disulfide and 4,4'-dimethyldiphenol are mixed to form a chemically bonded antioxidant, which enhances its dispersion and compatibility in rubber and prevents oxidation reactions.
It effectively overcomes the problems of easy migration and volatilization of small molecule antioxidants, improves the stability of antioxidants and the anti-aging properties of rubber, extends the service life of rubber and improves its heat resistance in high temperature environments.
Abstract
Description
Technical Field
[0001] The invention relates to the field of rubber, in particular to an antioxidant for rubber and a preparation method thereof. Background Art
[0002] Rubber is an important engineering material with excellent elasticity, wear resistance, aging resistance, corrosion resistance and other characteristics. It is widely used in the fields of automobile, aerospace, construction, medical, etc. However, rubber is easily affected by oxidation during long-term use, leading to performance degradation, cracking, aging and other problems.
[0003] Oxidation refers to the reaction between rubber and oxygen, which leads to the breakage of rubber molecular chains and cross-linking, resulting in the reduction of mechanical and physical properties of rubber materials. Especially under high temperature environment, the oxidation reaction rate is faster. Therefore, in order to extend the service life of rubber and improve the quality stability of rubber products, the application of antioxidants is of great significance. Antioxidants are a class of compounds that can react with free radicals in rubber to stabilize the chemical structure of rubber and delay oxidation reactions. Common antioxidants include phenols, amines, thiols, etc. Antioxidants improve the antioxidant properties of rubber by intercepting free radicals and stabilizing oxidation reactions.
[0004] With the continuous development of science and technology, the research on rubber antioxidants has also made significant progress. At present, researchers have achieved the long-term, low-toxicity and high-efficiency of rubber antioxidants by continuously improving the chemical structure of antioxidants, improving the thermal stability of antioxidants, and improving environmental friendliness. Generally, aromatic amine antioxidants are small molecule compounds that are easy to migrate and volatilize, so the long-term protection effect is poor and they will also cause pollution to the environment. Supported antioxidants are a method to solve the problems of aromatic amine antioxidants. Supported antioxidants use a method of grafting small molecule antioxidants on the surface of fillers. This chemical bonding can not only solve the problem of easy migration and volatility of small molecule antioxidants, but also improve the dispersion of fillers in the rubber matrix and the compatibility with the rubber matrix, thereby effectively improving the comprehensive performance of rubber composites.
[0005] Therefore, we propose an antioxidant for rubber and a preparation method thereof. Summary of the invention
[0006] The object of the present invention is to provide an antioxidant for rubber and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0008] A method for preparing a rubber antioxidant comprises the following steps:
[0009] Step 1: uniformly mix the composite, tris-(2,4-di-tert-butylphenyl) phosphite and dimethyl sulfoxide; the composite comprises components: an amino compound, 3-isocyanate propyltrimethoxysilane and a carrier, wherein the carrier is a chitosan / nano-silica hybrid material;
[0010] Step 2: Add white carbon black, vinyl triethoxysilane, 2-nonyl disulfide, and 4,4'-dimethyl diphenol, raise the temperature to 70-80°C, and stir for 10-20 minutes;
[0011] Step 3: Take out the pellets to obtain the antioxidant.
[0012] In the above technical scheme, the antioxidant performance of the antioxidant can be enhanced by using a composite and tris-(2,4-di-tert-butylphenyl) phosphite in combination; dimethyl sulfoxide as a solvent can make them mix better; white carbon black as a filler of the antioxidant is conducive to the uniform dispersion of the antioxidant during the mixing process of rubber; vinyl triethoxysilane can enhance the combination between organic and inorganic substances and improve the fractional performance of the filler; and the use of 2-nonyl ammonium disulfide and 4,4'-dimethyldiphenol to cooperate with each other is conducive to enhancing the antioxidant performance of the antioxidant and further preventing or slowing down the oxidation reaction of the rubber.
[0013] Further, the antioxidant comprises the following components by weight:
[0014] 10-20 parts of the composite, 5-15 parts of tris-(2,4-di-tert-butylphenyl) phosphite, 3-5 parts of dimethyl sulfoxide, 10-20 parts of white carbon black, 1-2 parts of vinyl triethoxysilane, 1-2 parts of 2-nonyl disulfide, and 3-5 parts of 4,4'-dimethyl diphenol.
[0015] Furthermore, the preparation steps of the composite are as follows:
[0016] Step (1): heat diphenylamine to 60-70° C. to melt, add anhydrous aluminum chloride, stir for 30-60 min, raise the temperature to 140-160° C., add allyl 4-aminobenzoate dropwise, and add the mixture over 3-4 h, continue the reaction for 2-4 h, extract, wash with water, recrystallize, and further distill under reduced pressure to obtain an amino compound;
[0017] Step (2): under nitrogen protection, the amino compound and toluene are mixed evenly, 3-isocyanatepropyltrimethoxysilane and dibutyltin dilaurate are added, the temperature is raised to 50-70° C., the reaction is carried out for 3-5 hours, and the mixture is rotary evaporated to obtain compound A;
[0018] Step (3): Mix chitosan and acetic acid solution evenly, filter and obtain chitosan solution; add sodium phosphate solution, adjust the pH value to 3-5, add tetraethyl orthosilicate, stir and react at 50-60°C for 10-12h, wash and dry to obtain chitosan / nanosilica hybrid material; then add a mixed solution of compound A obtained in S2 and ethanol, react for 12-14h, wash and dry to obtain a composite.
[0019] In the above technical scheme, diphenylamine is used as a raw material, and reacts with the carbon-carbon double bond of allyl 4-aminobenzoate under the catalytic action of anhydrous aluminum chloride to synthesize a compound containing an amino group; a chitosan solution is mixed with a phosphoric acid solution to form a polymer network structure; tetraethyl orthosilicate is used as a silicon precursor, and the tetraethyl orthosilicate dispersed in the chitosan polymer network is hydrolyzed, dehydrated and condensed to form silica colloidal particles that are bonded to chitosan through hydrogen bonds and chemical bonds to obtain a chitosan / nano-silica hybrid material, wherein a single particle is a spherical organic-inorganic hybrid particle with chitosan as an outer shell and silica as an inner core; 3-isocyanate propyltrimethoxysilane is used as a bridging agent, and the chitosan / nano-silica hybrid material is used as a carrier, and the amino-containing compound is grafted on the surface of the chitosan / nano-silica hybrid material in a chemically bonded manner through in-situ modification to obtain a supported composite.
[0020] Furthermore, in the step (1), the mass ratio of diphenylamine to anhydrous aluminum chloride catalyst is 1:(0.3-0.5).
[0021] Furthermore, in the step (1), the mass ratio of diphenylamine to allyl 4-aminobenzoate is 1:(1.2-1.5).
[0022] Furthermore, in the step (2), the mass ratio of the amino compound to toluene is 1:(10-12).
[0023] Furthermore, in the step (2), the mass ratio of the amino compound to 3-isocyanatepropyltrimethoxysilane is 1:(0.9-1.2).
[0024] Furthermore, the amount of dibutyltin dilaurate used in step (2) is 2-5% of the mass of the amino compound.
[0025] Furthermore, in step (3), the concentration of the chitosan solution is 5-7 g / L, and the concentration of the sodium phosphate solution is 0.5-1.0 mol / L.
[0026] Furthermore, in step (3), the mass ratio of chitosan to tetraethyl orthosilicate is 1:(10-15).
[0027] Furthermore, in the step (3), the mass ratio of compound A to ethanol is 1:(12-15).
[0028] An application of an antioxidant for rubber comprises the following steps:
[0029] S1: The natural rubber is thinly passed on an open mill for 3-5 times, and then carbon black, zinc oxide, stearic acid, accelerator, antioxidant and sulfur are added in sequence for mixing, and the mixing is performed at 110-130° C. for 3-5 minutes to obtain a mixed rubber;
[0030] S2: The mixed rubber is left for 24-48 hours and vulcanized using a flat vulcanizer to obtain natural rubber products.
[0031] Furthermore, the natural rubber product comprises the following components by weight: 100-120 parts of natural rubber, 30-40 parts of carbon black, 3-5 parts of zinc oxide, 1-3 parts of stearic acid, 2-5 parts of accelerator, 2-6 parts of antioxidant, and 1-3 parts of sulfur.
[0032] The natural rubber is Yunnan standard rubber SCRWF, provided by Shanghai Yuanxiang Industrial Co., Ltd.
[0033] The carbon black was carbon black N774, which was provided by Tianjin Tianyi Century Chemical Products Technology Development Co., Ltd.
[0034] The zinc oxide was Bajiao brand zinc oxide with a content of ≥99.7%, provided by Changzhou Shanglian Chemical Co., Ltd.
[0035] Stearic acid was Indonesian Sven SA1801, provided by Guangzhou Yixin Chemical Technology Co., Ltd.
[0036] The sulfur model is S-80, provided by Shanghai Donghu Industrial Co., Ltd.
[0037] Furthermore, the accelerator is composed of 1-2 parts by mass of accelerator TMTD and 1-3 parts by mass of accelerator CZ.
[0038] Furthermore, the vulcanization treatment parameters in step S2 are: vulcanization pressure 15-25 MPa, vulcanization temperature 145-165° C., and vulcanization time 15-40 min.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] 1. An antioxidant for rubber and a preparation method thereof of the present invention comprises the following steps: using diphenylamine as a raw material, reacting the carbon-carbon double bond of allyl 4-aminobenzoate under the catalytic action of anhydrous aluminum chloride to synthesize a compound containing an amino group; mixing a chitosan solution with a phosphoric acid solution to form a polymer network structure; using tetraethyl orthosilicate as a silicon precursor, and hydrolyzing and dehydrating and condensing the tetraethyl orthosilicate dispersed in the chitosan polymer network to form silica colloidal particles that are bonded to chitosan through hydrogen bonds and chemical bonds to obtain a chitosan / nano-silica hybrid material, wherein a single particle is a spherical organic-inorganic hybrid particle with chitosan as an outer shell and silica as an inner core; and then 3-isocyanate propyl trimethoxy silane is used as a bridging agent, chitosan / nano-silica hybrid material is used as a carrier, and the amino compound is grafted on the surface of the chitosan / nano-silica hybrid material in a chemical bonding manner through in-situ modification technology, wherein the isocyanate group of 3-isocyanate propyl trimethoxy silane reacts with the amino group of the amino compound to obtain chemical A; and then reacts with the hydroxyl group in the chitosan / nano-silica hybrid material to obtain a loaded composite, which effectively overcomes the problems of easy migration and volatility of small molecule antioxidants, and can not only improve the stability of the antioxidant, but also improve the dispersion of the filler in the rubber matrix and the compatibility with the rubber matrix. Its anti-thermal oxidative aging mechanism is: the -NH group can capture the active free radicals such as R· and ROO· generated by the natural rubber molecular chain due to thermal oxidative aging, and combine with them to form a stable compound, effectively delaying the aging rate of natural rubber, so that it has better anti-aging performance.
[0041] 2. The present invention provides an antioxidant for rubber and a preparation method thereof. The antioxidant performance of the antioxidant can be enhanced by using a composite and tris-(2,4-di-tert-butylphenyl) phosphite in combination; dimethyl sulfoxide is used as a solvent to make them mix better; white carbon black is used as a filler of the antioxidant, which is beneficial to the uniform dispersion of the antioxidant during the mixing process of the rubber; vinyl triethoxysilane can enhance the combination between organic and inorganic substances and improve the fractional performance of the filler; and the use of 2-nonyl ammonium disulfide and 4,4'-dimethyldiphenol to cooperate with each other is beneficial to enhancing the antioxidant performance and further preventing or slowing down the oxidation reaction of the rubber. By mixing the complex, tris-(2,4-di-tert-butylphenyl) phosphite, dimethyl sulfoxide, white carbon black, vinyl triethoxysilane, 2-nonylamino disulfide and 4,4'-dimethyldiphenol in a certain proportion and reacting them under appropriate conditions, a synergistic effect will occur between the raw materials, which will promote the antioxidant properties of the antioxidants. These synergistic effects help to finally prepare an antioxidant product with excellent antioxidant properties. DETAILED DESCRIPTION
[0042] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] In this embodiment, the white carbon black is precipitated white carbon black, model A200, particle size 400 mesh, provided by Jinan Baoda Dye Chemical Co., Ltd.; chitosan: KJT-12, provided by Xi'an Zhipin Biotechnology Co., Ltd.; natural rubber is Yunnan standard rubber SCRWF, provided by Shanghai Yuanxiang Industrial Co., Ltd.; carbon black is carbon black N774, provided by Tianjin Tianyi Century Chemical Products Technology Development Co., Ltd.; zinc oxide is banana brand zinc oxide, content ≥99.7%, provided by Changzhou Shanglian Chemical Co., Ltd.; stearic acid is Indonesia Sven SA1801, provided by Guangzhou Yixin Chemical Technology Co., Ltd.; accelerator TMTD is provided by Hebei Gaochang Chemical Co., Ltd.; accelerator CZ is provided by Shijiazhuang Taisheng Chemical Co., Ltd. Sulfur model is S-80, provided by Shanghai Donghu Industrial Co., Ltd.
[0044] In the following examples and comparative examples, 1 part is equal to 10 g.
[0045] Example 1: A method for preparing a rubber antioxidant, comprising the following process:
[0046] Step 1: Evenly mix 10 parts of a composite, 5 parts of tris-(2,4-di-tert-butylphenyl) phosphite, and 3 parts of dimethyl sulfoxide; the composite comprises components: an amino compound, 3-isocyanate propyltrimethoxysilane, and a carrier, wherein the carrier is a chitosan / nano-silica hybrid material;
[0047] Step 2: Add 10 parts of white carbon black, 1 part of vinyl triethoxysilane, 1 part of 2-nonyl disulfide, and 3 parts of 4,4'-dimethyl diphenol, heat to 70°C, and stir for 10 minutes;
[0048] Step 3: taking out the pellets to obtain an antioxidant;
[0049] The preparation method of the composite is as follows:
[0050] Step (1): heat 10 parts of diphenylamine to 60°C to melt, add 3 parts of anhydrous aluminum chloride, stir for 30 minutes, heat to 140°C, dropwise add 12 parts of allyl 4-aminobenzoate, and continue to react for 2 hours. After extraction, washing, recrystallization, and further vacuum distillation, an amino compound is obtained.
[0051] Step (2): Under nitrogen protection, 10 parts of an amino compound and 100 parts of toluene were mixed evenly, 9 parts of 3-isocyanatepropyltrimethoxysilane and 0.2 parts of dibutyltin dilaurate were added, the temperature was raised to 50° C., the reaction was carried out for 3 hours, and compound A was obtained by rotary evaporation;
[0052] Step (3): 10 parts of chitosan and 2100 parts of acetic acid solution are mixed evenly, and filtered to obtain a 5 g / L chitosan solution; 0.5 mol / L sodium phosphate solution is added to adjust the pH value to 3, 100 parts of tetraethyl orthosilicate are added, and the mixture is stirred and reacted at 50° C. for 10 hours. After washing and drying, a chitosan / nanosilica hybrid material is obtained; then a mixed solution of 10 parts of compound A obtained by S2 and 120 parts of ethanol is added, and the mixture is reacted for 12 hours. After washing and drying, a composite material is obtained;
[0053] An application of an antioxidant for rubber comprises the following steps:
[0054] S1: 100 parts of natural rubber were thinly passed on an open mill for 3 times, and then 30 parts of carbon black, 3 parts of zinc oxide, 1 part of stearic acid, 2 parts of accelerators, 2 parts of antioxidants, and 1 part of sulfur were added in sequence for mixing, and mixed at 110° C. for 3 minutes to obtain a mixed rubber;
[0055] S2: The mixed rubber was left standing for 24 hours and subjected to vulcanization treatment using a flat vulcanizer (vulcanization pressure 15 MPa, vulcanization temperature 145° C., vulcanization time 15 min) to obtain a natural rubber product.
[0056] Embodiment 2: A method for preparing a rubber antioxidant, comprising the following process:
[0057] Step 1: Evenly mix 15 parts of a composite, 10 parts of tris-(2,4-di-tert-butylphenyl) phosphite, and 4 parts of dimethyl sulfoxide; the composite comprises components: an amino compound, 3-isocyanate propyltrimethoxysilane, and a carrier, wherein the carrier is a chitosan / nano-silica hybrid material;
[0058] Step 2: Add 15 parts of white carbon black, 1.5 parts of vinyl triethoxysilane, 1.5 parts of 2-nonyl disulfide, and 4 parts of 4,4'-dimethyl diphenol, raise the temperature to 75°C, and stir for 15 minutes;
[0059] Step 3: taking out the pellets to obtain an antioxidant;
[0060] The preparation method of the composite is as follows:
[0061] Step (1): heat 15 parts of diphenylamine to 65°C to melt, add 6 parts of anhydrous aluminum chloride, stir for 45 minutes, heat to 140°C, dropwise add 21 parts of allyl 4-aminobenzoate, and complete the dropwise addition within 3.5 hours. Continue the reaction for 3 hours, extract, wash with water, recrystallize, and further distill under reduced pressure to obtain an amino compound;
[0062] Step (2): Under nitrogen protection, 15 parts of an amino compound and 165 parts of toluene were mixed evenly, 15 parts of 3-isocyanatepropyltrimethoxysilane and 0.6 parts of dibutyltin dilaurate were added, the temperature was raised to 60° C., the reaction was carried out for 4 hours, and compound A was obtained by rotary evaporation;
[0063] Step (3): 15 parts of chitosan and 2625 parts of acetic acid solution are mixed evenly, and filtered to obtain a 6 g / L chitosan solution; 0.8 mol / L sodium phosphate solution is added to adjust the pH value to 4, and 195 parts of tetraethyl orthosilicate are added, and stirred at 55°C for 11 hours. After washing and drying, a chitosan / nanosilica hybrid material is obtained; then 15 parts of a mixed solution of compound A obtained by S2 and 195 parts of ethanol are added, and the mixture is reacted for 13 hours. After washing and drying, a composite material is obtained;
[0064] An application of an antioxidant for rubber comprises the following steps:
[0065] S1: The natural rubber is thinly passed on an open mill for 4 times, and then carbon black, zinc oxide, stearic acid, accelerator, antioxidant and sulfur are added in sequence for mixing, and the mixture is mixed at 120° C. for 4 minutes to obtain a mixed rubber;
[0066] S2: The mixed rubber was left for 36 hours and vulcanized using a flat vulcanizer (vulcanization pressure 20 MPa, vulcanization temperature 155° C., vulcanization time 25 min) to obtain a natural rubber product.
[0067] Embodiment 3: A method for preparing a rubber antioxidant, comprising the following process:
[0068] Step 1: Evenly mix 20 parts of a composite, 15 parts of tris-(2,4-di-tert-butylphenyl) phosphite, and 5 parts of dimethyl sulfoxide; the composite comprises components: an amino compound, 3-isocyanate propyltrimethoxysilane, and a carrier, wherein the carrier is a chitosan / nano-silica hybrid material;
[0069] Step 2: Add 20 parts of white carbon black, 2 parts of vinyl triethoxysilane, 2 parts of 2-nonyl disulfide, and 5 parts of 4,4'-dimethyl diphenol, heat to 80°C, and stir for 20 minutes;
[0070] Step 3: taking out the pellets to obtain an antioxidant;
[0071] The preparation method of the composite is as follows:
[0072] Step (1): heat 20 parts of diphenylamine to 70°C to melt, add 10 parts of anhydrous aluminum chloride, stir for 60 minutes, heat to 160°C, dropwise add 30 parts of allyl 4-aminobenzoate, add the mixture over 4 hours, continue the reaction for 4 hours, extract, wash with water, recrystallize, and further distill under reduced pressure to obtain an amino compound;
[0073] Step (2): Under nitrogen protection, 20 parts of an amino compound and 240 parts of toluene were mixed evenly, 24 parts of 3-isocyanatepropyltrimethoxysilane and 1 part of dibutyltin dilaurate were added, the temperature was raised to 70° C., the reaction was carried out for 5 hours, and compound A was obtained by rotary evaporation;
[0074] Step (3): 20 parts of chitosan and 3000 parts of acetic acid solution are mixed evenly, and filtered to obtain 7 g / L chitosan solution; 1 mol / L sodium phosphate solution is added to adjust the pH value to 5, and 300 parts of tetraethyl orthosilicate are added, and stirred at 60°C for 12 hours. After washing and drying, chitosan / nano-silica hybrid material is obtained; then 20 parts of a mixed solution of compound A obtained by S2 and 300 parts of ethanol are added, and the mixture is reacted for 14 hours. After washing and drying, a composite material is obtained;
[0075] An application of an antioxidant for rubber comprises the following steps:
[0076] S1: 120 parts of natural rubber were thinly passed on an open mill for 5 times, and then 40 parts of carbon black, 5 parts of zinc oxide, 3 parts of stearic acid, 5 parts of accelerator, 6 parts of antioxidant and 3 parts of sulfur were added in sequence for mixing, and mixed at 130° C. for 5 minutes to obtain a mixed rubber;
[0077] S2: The mixed rubber was left for 48 hours and vulcanized using a flat vulcanizer (vulcanization pressure 25 MPa, vulcanization temperature 165° C., vulcanization time 40 min) to obtain a natural rubber product.
[0078] Comparative Example 1: The antioxidant includes the following components by weight: 10 parts of a complex, 5 parts of tris-(2,4-di-tert-butylphenyl) phosphite, 3 parts of dimethyl sulfoxide, 10 parts of white carbon black, 1 part of vinyl triethoxysilane, 1 part of 2-nonyl disulfide, and 3 parts of 4,4'-dimethyldiphenol. In Comparative Example 1, the complex is replaced with the same mass of N,N'-di(2-naphthyl)-p-phenylenediamine, and the preparation steps of the complex are deleted. The other steps and processes are the same as those in Example 1.
[0079] Comparative Example 2: The antioxidant comprises the following components by weight: 10 parts of a complex, 5 parts of tris-(2,4-di-tert-butylphenyl) phosphite, 3 parts of dimethyl sulfoxide, 10 parts of white carbon black, 1 part of vinyl triethoxysilane, and 1 part of 2-nonyl disulfide. Compared with Example 1, Comparative Example 2 does not add 4,4'-dimethyldiphenol, and other steps and processes are the same as Example 1.
[0080] Comparative Example 3: Compared with Example 2, in Comparative Example 3, the complex is replaced with an amino compound of the same mass, step (2) and step (3) are deleted, and the other steps and processes are the same as those of Example 2.
[0081] Comparative Example 4: A method for preparing an antioxidant for rubber, comprising the following process:
[0082] The preparation method of the composite is as follows:
[0083] (1) 15 parts of diphenylamine were heated to 65°C to melt, 6 parts of anhydrous aluminum chloride were added, stirred for 45 minutes, heated to 140°C, 21 parts of allyl 4-aminobenzoate were added dropwise, and the dripping was completed within 3.5 hours. The reaction was continued for 3 hours, and the amino compound was obtained after extraction, water washing, recrystallization, and further vacuum distillation.
[0084] (2) Under nitrogen protection, 15 parts of an amino compound and 165 parts of toluene were mixed evenly, 15 parts of 3-isocyanatepropyltrimethoxysilane and 0.6 parts of dibutyltin dilaurate were added, the temperature was raised to 60° C., the reaction was carried out for 4 hours, and the mixture was rotary evaporated to obtain compound A;
[0085] (3) 15 parts of chitosan and 2625 parts of acetic acid solution were mixed evenly, filtered, and a 6 g / L chitosan solution was obtained; 0.8 mol / L sodium phosphate solution was added, the pH value was adjusted to 4, 60 parts of tetraethyl orthosilicate were added, and the mixture was stirred and reacted at 55° C. for 11 hours. After washing and drying, a chitosan / nanosilica hybrid material was obtained; then 15 parts of a mixed solution of compound A obtained in S2 and 195 parts of ethanol were added, the mixture was reacted for 13 hours, and after washing and drying, a composite material was obtained;
[0086] Compared with Example 2, the mass ratio of chitosan to tetraethyl orthosilicate in Comparative Example 4 is 1:4, and the remaining steps are the same as those in Example 2.
[0087] experiment
[0088] The products obtained in Examples 1-3 and Comparative Examples 1-4 were taken to prepare samples, and their properties were tested and the test results were recorded:
[0089] The heat resistance was measured by thermogravimetric analyzer. The experimental steps were as follows: the antioxidant was prepared into a uniform sample, and the bubbles were removed by vacuum degassing. The sample size was 10 mg. The sample was placed in a nitrogen atmosphere and heated at a heating rate of 10 °C / min, starting at 25 °C, and heated to 800 °C. The experimental data were recorded.
[0090] According to the ASTM D573-04 (2015) standard, an accelerated thermal oxidation aging experiment was carried out. The experimental steps were as follows: the natural rubber product was cut into dumbbell-shaped specimens with a length of 100 mm, a width of 10 mm, and a thickness of 2 mm, and placed in a thermal oxidation aging box. The aging temperature was 100°C and the aging was 7 days. The tensile test was carried out according to the ASTM D412-15a standard. The tensile rate was 500 mm / min. The experimental data were recorded. The product of the tensile strength of the rubber and the elongation at break was the tensile product. The tensile product aging coefficient k was equal to the tensile product of the sample after aging / the tensile product of the sample before aging × 100%.
[0091] Tg / ℃ Tensile aging coefficient k / % Example 1 296 63% Example 2 300 65% Example 3 297 64% Comparative Example 1 258 40% Comparative Example 2 282 52% Comparative Example 3 267 42% Comparative Example 4 275 48%
[0092] According to the data in the above table, we can clearly draw the following conclusions:
[0093] 1. Compared with Comparative Example 1 and Comparative Example 3, the Tg and tensile aging coefficient of the samples of Examples 1-3 are increased, indicating that the antioxidant effect of the composite prepared by the present invention is significantly better than that of N, N'-di(2-naphthyl)-p-phenylenediamine and amino compounds. The composite is not easy to migrate and volatilize under the aging temperature, and can improve the antioxidant properties of rubber.
[0094] 2. Compared with Examples 1-3, the Tg and tensile aging coefficient of the sample in Comparative Example 2 are both reduced, indicating that the addition of 4,4'-dimethyldiphenol in the present invention can play a synergistic role with other components to improve the antioxidant performance of the antioxidant.
[0095] 3. Compared with Examples 1-3, the Tg and tensile aging coefficient of Comparative Example 4 are both reduced, indicating that the composite prepared by the present invention is affected by the ratio of each reagent in its preparation process. Selecting the reagent ratio within the said range can improve the antioxidant performance of the antioxidant, thereby improving the aging resistance of the rubber and extending its service life.
[0096] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.
[0097] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing an antioxidant for rubber, characterized in that: The steps include: Step 1: uniformly mix the composite, tris-(2,4-di-tert-butylphenyl) phosphite and dimethyl sulfoxide; the composite comprises components: an amino compound, 3-isocyanate propyltrimethoxysilane and a carrier, wherein the carrier is a chitosan / nano-silica hybrid material; Step 2: Add white carbon black, vinyl triethoxysilane, 2-nonyl disulfide, and 4,4'-dimethyl diphenol, raise the temperature to 70-80°C, and stir for 10-20 minutes; Step 3: taking out the pellets to obtain an antioxidant; The antioxidant comprises the following components by weight: 10-20 parts of the composite, 5-15 parts of tris-(2,4-di-tert-butylphenyl) phosphite, 3-5 parts of dimethyl sulfoxide, 10-20 parts of white carbon black, 1-2 parts of vinyl triethoxysilane, 1-2 parts of 2-nonyl disulfide, 3-5 parts of 4,4'-dimethyl diphenol; The steps for preparing the composite are as follows: Step (1): heat diphenylamine to 60-70° C. to melt, add anhydrous aluminum chloride, stir for 30-60 min, raise the temperature to 140-160° C., add allyl 4-aminobenzoate dropwise, and add the mixture over 3-4 h, continue the reaction for 2-4 h, extract, wash with water, recrystallize, and further distill under reduced pressure to obtain an amino compound; Step (2): under nitrogen protection, the amino compound and toluene are mixed evenly, 3-isocyanatepropyltrimethoxysilane and dibutyltin dilaurate are added, the temperature is raised to 50-70° C., the reaction is carried out for 3-5 hours, and the mixture is rotary evaporated to obtain compound A; Step (3): Mix chitosan and acetic acid solution evenly, filter and obtain chitosan solution; add sodium phosphate solution, adjust the pH value to 3-5, add tetraethyl orthosilicate, stir and react at 50-60°C for 10-12h, wash and dry to obtain chitosan / nanosilica hybrid material; then add a mixed solution of compound A obtained in S2 and ethanol, react for 12-14h, wash and dry to obtain a composite.
2. The method for preparing a rubber antioxidant according to claim 1, characterized in that: In the step (1), the mass ratio of diphenylamine to anhydrous aluminum chloride is 1:(0.3-0.5).
3. The method for preparing a rubber antioxidant according to claim 1, characterized in that: The mass ratio of the amino compound to 3-isocyanatepropyltrimethoxysilane in step (2) is 1:(0.9-1.2).
4. The method for preparing a rubber antioxidant according to claim 1, characterized in that: In the step (3), the concentration of the chitosan solution is 5-7 g / L, and the concentration of the sodium phosphate solution is 0.5-1.0 mol / L.
5. The method for preparing a rubber antioxidant according to claim 1, characterized in that: In the step (3), the mass ratio of compound A to ethanol is 1:(12-15).
6. An antioxidant for rubber obtained according to the preparation method according to any one of claims 1 to 5.
7. Use of the rubber antioxidant according to claim 6, characterized in that: The following steps are involved: S1: The natural rubber is thinly passed on an open mill for 3-5 times, and then carbon black, zinc oxide, stearic acid, accelerator, antioxidant and sulfur are added in sequence for mixing, and the mixing is performed at 110-130° C. for 3-5 minutes to obtain a mixed rubber; S2: The mixed rubber is left for 24-48 hours and vulcanized using a flat vulcanizer to obtain natural rubber products.
8. The use of an antioxidant for rubber according to claim 7, characterized in that: The vulcanization treatment parameters in step S2 are: vulcanization pressure 15-25 MPa, vulcanization temperature 145-165° C., and vulcanization time 15-40 min.