Low modulus and high strength polyurethane structural adhesive for power battery assembly and preparation method thereof

By using low modulus and high strength polyurethane structural adhesive in power battery assembly, combined with bio-based polyol and isocyanate-based silane coupling agent, an interpenetrating cross-linked network structure is formed, which solves the problem of high modulus and poor bonding performance of polyurethane structural adhesive. problem, achieving stable performance and improved security in complex environments.

CN116676068BActive Publication Date: 2024-10-29NANTONG GAOMENG NEW MATERIAL
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310705202.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-14
Publication Date
2024-10-29
Estimated Expiration
2043-06-14

AI Technical Summary

Technical Problem

The existing polyurethane structural adhesive used for power battery assembly has a high modulus and poor bonding performance, and there is a risk of reduced reliability and safety in high-frequency vibration and hot and humid environments.

Method used

Using low modulus and high strength polyurethane structural adhesive, through the combination of component A and component B, including bio-based polyols, aromatic ring modified polyols, isocyanate-based silane coupling agents and other raw materials, an interpenetrating cross-linked network structure is formed. , improve bonding strength and heat and humidity aging resistance, and reduce modulus.

Benefits of technology

It achieves stable performance in high-frequency vibration and hot and humid environments, improving the reliability and safety of power batteries. The modulus is less than 400MPa, the shear strength is greater than 8MPa, it has excellent heat and humidity aging resistance and good flame retardant properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0005057153640000081
    Figure GDA0005057153640000081
  • Figure GDA0005057153640000091
    Figure GDA0005057153640000091
Patent Text Reader

Abstract

The invention discloses a low modulus and high strength polyurethane structural adhesive for power battery assembly and a preparation method thereof, wherein the structural adhesive comprises: a volume ratio of component A to component B of 1:1; component A comprises: bio-based polyol, aromatic ring modified polyol, polyether polyol, crosslinking agent, catalyst, flame retardant, water and thixotropic agent; component B comprises: isocyanate, terminal isocyanate polyurethane prepolymer, isocyanate silane coupling agent modified polyether polyol, flame retardant, coupling agent, water absorbent, thixotropic agent and catalyst. The structural adhesive has excellent bonding strength to substrates such as aluminum, steel, PC, and PET, and has the properties of low modulus, high strength, excellent flame retardancy, excellent wet heat aging, etc., which effectively ensures the stable performance of power batteries in long-term use under complex environments such as high-frequency vibration, wet heat, severe cold, extreme heat, and heat accumulation, thereby improving reliability and safety.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of polymer material preparation, and in particular to a low modulus and high strength polyurethane structural adhesive for power battery assembly and a preparation method thereof. Background Art

[0002] As one of the core components of new energy vehicles, the production and assembly quality of power batteries directly affects key performance of new energy vehicles such as cruising range, service life, safety and reliability, charging time and temperature.

[0003] With the innovation of power battery structure, power battery assembly technology (i.e. PACK technology) has developed from traditional CTM technology to CTP technology, and then to CTC and CTB technology. The higher the grouping rate of modules and systems, the fewer the number of modules. In the PACK assembly process, more and more metal structural parts are replaced by adhesives, and the number of adhesive points and the amount of adhesive used continue to increase. Adhesives directly affect the thermal conductivity, aging resistance, service life and safety of power batteries, and directly determine the product quality of battery packs. No matter how power battery PACK technology develops, power battery PACK adhesives are one of the core factors to achieve stable, efficient, durable and safe operation of electric drive systems. Its importance is unshakable and its role is irreplaceable. It helps to optimize and improve the entire power battery industry and contribute to the realization of dual carbon goals.

[0004] Polyurethane adhesive has the advantages of high tensile strength, moderate stiffness, good high and low temperature resistance, etc. It has obvious advantages when used as an adhesive for structural bonding between battery cells, but it must be applied to harsh environments such as high-frequency vibration, high and low temperature and high humidity, and it must have sufficiently good bonding properties to materials such as Al, steel, PET, and PC. Therefore, it is usually necessary to add polyols containing aromatic functional groups to improve the compatibility with the substrate and enhance the interaction force, which is manifested in the improvement of bonding performance in the macroscopic sense. The addition of aromatic polyols will reduce the flexibility of the molecular chain of polyurethane structural adhesive, enhance the rigidity, and increase the modulus, which is not enough to buffer the high-frequency vibration of new energy vehicles during driving. At present, polyurethane structural adhesives for power battery PACK still have shortcomings such as relatively high modulus (>500MPa) and poor bonding performance (Al-Al shear strength <8MPa). When used for a long time in complex environments, there is a risk of reduced reliability and safety, threatening the safety of life and property.

[0005] In summary, how to provide a polyurethane structural adhesive for power battery assembly with a low modulus of less than 400 MPa and a high strength of more than 8 MPa is an urgent problem to be solved.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] In order to solve the above-mentioned problems existing in the prior art, the present invention provides a low-modulus and high-strength polyurethane structural adhesive for power battery assembly and a preparation method thereof. The structural adhesive does not contain solvents, is safe and environmentally friendly, has excellent bonding strength for substrates such as aluminum, steel, PC, and PET, and has high strength, low modulus, excellent flame retardancy, excellent moisture and heat aging and other properties. It can meet the performance requirements of power battery PACK structural adhesives, and effectively ensure the stability of the performance of power batteries during long-term use in complex environments such as high-frequency vibration, humidity and heat, severe cold, extreme heat, and heat accumulation, thereby improving reliability and safety.

[0008] The present invention is achieved through the following technical solutions:

[0009] A low modulus and high strength polyurethane structural adhesive for power battery assembly, comprising:

[0010] Component A and component B, wherein the volume ratio of component A to component B is 1:1, and the molar ratio of functional groups is: NCO:OH=1.05:1-2.0:1;

[0011] The component A is composed of the following raw materials in parts by mass: 5-30 parts of bio-based polyol, 10-30 parts of aromatic ring modified polyol, 0.001-15 parts of polyether polyol, 0.001-3 parts of cross-linking agent, 0.001-0.1 parts of catalyst, 15-45 parts of flame retardant, 0.001-0.3 parts of water and 0.001-5 parts of thixotropic agent;

[0012] The B component is composed of the following raw materials in parts by mass: 0.001-15 parts of isocyanate, 35-75 parts of terminal isocyanate polyurethane prepolymer, 5-25 parts of isocyanate silane coupling agent modified polyether polyol, 10-25 parts of flame retardant; 0.001-5 parts of coupling agent, 0.001-0.3 parts of water absorbent, 0.001-5 parts of thixotropic agent and 0.001-0.1 parts of catalyst.

[0013] A method for preparing a low modulus and high strength polyurethane structural adhesive for power battery assembly according to the present invention comprises the following steps:

[0014] preparing a terminal isocyanate prepolymer and an isocyanate silane coupling agent modified polyether polyol respectively;

[0015] According to the formula of component A and component B of the present invention, the constituent raw materials of component A and component B are respectively taken, and the raw materials of component A and component B are respectively mixed evenly to obtain component A and component B, and the prepared component A and component B are combined and used in a volume ratio of 1:1 to obtain a low modulus and high strength polyurethane structural adhesive for power battery assembly.

[0016] Compared with the prior art, the low modulus and high strength polyurethane structural adhesive for power battery assembly provided by the present invention has the following beneficial effects:

[0017] By adding an appropriate amount of isocyanate silane coupling agent to modify polyether polyol in component B, the modulus of polyurethane adhesive can be effectively reduced. The silane coupling agent can react with the hydroxyl group on the surface of the substrate to form a covalent bond, while still maintaining sufficiently high tensile strength and shear strength. After curing, the isocyanate silane coupling agent modified polyether polyol and polyurethane can form an interpenetrating cross-linked network structure, which can block the entry of water vapor and improve the resistance to wet heat aging. Adding bio-based polyols containing long carbon chains and poly dimer acid hexanediol polyester diols can improve The hydrophobicity of the molecular chain improves the resistance to moisture and heat aging, while increasing the flexibility of the molecular chain, and to a certain extent, the modulus is lower; the addition of aromatic ring-containing polyols increases the rigidity of the molecular chain, increases the glass transition temperature, improves the heat resistance, and also effectively improves the bonding strength to PET, PC and metal substrates; compared with the prior art, the present invention has at least the following beneficial effects: (1) The modulus is relatively low, the storage modulus is ≤400MPa at 25°C, and it has excellent buffering and shock absorption effect when applied to power battery PACK glue. (2) The strength is relatively high, the tensile strength of the body is ≥8MPa, and the shear strength for substrates such as PET, PC, aluminum alloy, and steel is ≥8MPa, ensuring safety and reliability during driving. (3) The resistance to moisture and heat aging is excellent, and after aging for 1000h with double 85, the tensile strength and shear strength decay by <20%. DETAILED DESCRIPTION

[0018] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in combination with the specific content of the present invention; it is obvious that the described embodiments are only part of the embodiments of the present invention, not all of the embodiments, which does not constitute a limitation of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.

[0019] First, the terms that may be used in this article are explained as follows:

[0020] The term “and / or” means that either or both of them can be realized at the same time. For example, X and / or Y means both “X” or “Y” and “X and Y”.

[0021] The terms "include", "comprises", "contains", "has" or other descriptions with similar semantics should be interpreted as non-exclusive inclusion. For example, including certain technical feature elements (such as raw materials, components, ingredients, carriers, dosage forms, materials, dimensions, parts, components, mechanisms, devices, steps, procedures, methods, reaction conditions, processing conditions, parameters, algorithms, signals, data, products or products, etc.) should be interpreted as including not only certain technical feature elements explicitly listed, but also other technical feature elements known in the art that are not explicitly listed.

[0022] The term "consisting of..." means excluding any technical feature elements not explicitly listed. If this term is used in a claim, it will make the claim closed, so that it does not contain technical feature elements other than the technical feature elements explicitly listed, except for the conventional impurities related to them. If this term only appears in a clause of a claim, it only limits the elements explicitly listed in the clause, and the elements recorded in other clauses are not excluded from the overall claim.

[0023] The term "parts by mass" refers to the mass ratio relationship between multiple components. For example, if it is described that component X is x parts by mass and component Y is y parts by mass, then the mass ratio of component X to component Y is x:y. 1 part by mass can represent any mass, for example, 1 part by mass can be represented as 1 kg or 3.1415926 kg. The sum of the parts by mass of all components is not necessarily 100 parts, but can be greater than 100 parts, less than 100 parts or equal to 100 parts. Unless otherwise specified, the parts, proportions and percentages described herein are all measured by mass.

[0024] When concentration, temperature, pressure, size or other parameters are expressed in the form of a numerical range, the numerical range should be understood to specifically disclose all ranges formed by the pairing of any upper limit, lower limit, and preferred value in the numerical range, regardless of whether the range is explicitly stated; for example, if a numerical range of "2 to 8" is stated, the numerical range should be interpreted as including ranges such as "2 to 7", "2 to 6", "5 to 7", "3 to 4 and 6 to 7", "3 to 5 and 7", "2 and 5 to 7", etc. Unless otherwise specified, the numerical ranges stated herein include both their end values ​​and all integers and fractions within the numerical range.

[0025] The high barrier heat-resistant solvent-free polyurethane composite material and the preparation method thereof provided by the present invention are described in detail below. The contents not described in detail in the embodiments of the present invention belong to the prior art known to professional and technical personnel in the field. If no specific conditions are specified in the embodiments of the present invention, the conventional conditions in the field or the conditions recommended by the manufacturer are followed. The reagents or instruments used in the embodiments of the present invention, if the manufacturer is not specified, are all conventional products that can be purchased commercially.

[0026] The embodiment of the present invention provides a low modulus and high strength polyurethane structural adhesive for power battery assembly, comprising:

[0027] Component A and component B, wherein the volume ratio of component A to component B is 1:1, and the molar ratio of functional groups is: NCO:OH=1.05:1-2.0:1;

[0028] The component A is composed of the following raw materials in parts by mass: 5-30 parts of bio-based polyol, 10-30 parts of aromatic ring modified polyol, 0.001-15 parts of polyether polyol, 0.001-3 parts of cross-linking agent, 0.001-0.1 parts of catalyst, 15-45 parts of flame retardant, 0.001-0.3 parts of water and 0.001-5 parts of thixotropic agent;

[0029] The B component is composed of the following raw materials in parts by mass: 0.001-15 parts of isocyanate, 35-75 parts of terminal isocyanate polyurethane prepolymer, 5-25 parts of isocyanate silane coupling agent modified polyether polyol, 10-25 parts of flame retardant; 0.001-5 parts of coupling agent, 0.001-0.3 parts of water absorbent, 0.001-5 parts of thixotropic agent and 0.001-0.1 parts of catalyst.

[0030] Preferably, in the component A of the structural adhesive, the bio-based polyol is one or more of soybean oil, castor oil, palm oil, hydrogenated castor oil, and aromatic ring-modified castor oil;

[0031] The aromatic ring modified polyol is one or more of bisphenol A or bisphenol F modified polyether diol with a molecular weight of 400-3000, or phthalic anhydride polyester diol;

[0032] The polyether polyol is polypropylene glycol with a molecular weight of 400-2000.

[0033] Preferably, in the component A of the structural adhesive, the crosslinking agent is one or more polyether polyols or amines with a functionality of 4-6.

[0034] Preferably, in the component A and the component B of the structural adhesive, the catalyst is one or more of bismuth isooctanoate, bismuth laurate, bismuth neodecanoate, bismuth cyclohexaneate, zinc isooctanoate, zinc neodecanoate, dibutyltin dilaurate, stannous octoate, and chelated tin;

[0035] The flame retardant is one or more of solid flame retardants such as aluminum hydroxide, magnesium hydroxide, aluminum hypophosphite, diethyl aluminum phosphite, or liquid flame retardants such as tricresyl phosphate, triethyl phosphate, tri(chloroisopropyl) phosphate, etc.;

[0036] In the component A and the component B, the thixotropic agent is one or more of fumed silica and bentonite.

[0037] Preferably, in the component B of the structural adhesive, the isocyanate is one or more of diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, toluene diisocyanate, isophorone diisocyanate, hexamethylene isocyanate, liquefied MDI, polymerized MDI, HDI trimer, and TDI trimer;

[0038] The terminal isocyanate polyurethane prepolymer is produced by reacting a diol with a molecular weight of 1000-3000 with an isocyanate, and the mass fraction of NCO is controlled to be 6-22%;

[0039] The isocyanate silane coupling agent modified polyether polyol is produced by the reaction of an isocyanate silane coupling agent and a polyether polyol, and the molar ratio is controlled to be: NCO:OH=1.005:1-1.3:1.

[0040] Preferably, in the above-mentioned isocyanate-terminated polyurethane prepolymer, the diol is one or more of polypropylene glycol, polyethylene glycol, polyethylene adipate diol, polyneopentyl adipate diol, and polyhexamethylene dimer diol; and the isocyanate in the isocyanate-terminated polyurethane prepolymer is one or more of diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, toluene diisocyanate, isophorone diisocyanate, hexamethylene isocyanate, liquefied MDI, polymeric MDI, HDI trimer, and TDI trimer.

[0041] Preferably, in the above-mentioned isocyanate silane coupling agent modified polyether polyol, the isocyanate silane coupling agent is one or more of isocyanate propyl triethoxy silane, isocyanate propyl trimethoxy silane, isocyanate propyl dimethoxy silane; and the polyether polyol is polypropylene glycol with a molecular weight of 3000-16000.

[0042] Preferably, in the above component B, the water absorbent is p-toluenesulfonyl isocyanate.

[0043] The embodiment of the present invention also provides a method for preparing the above-mentioned low modulus and high strength polyurethane structural adhesive for power battery assembly, comprising the following steps:

[0044] preparing a terminal isocyanate prepolymer and an isocyanate silane coupling agent modified polyether polyol respectively;

[0045] According to the above-mentioned formula of component A and component B, the constituent raw materials of component A and component B are respectively taken, and the raw materials of component A and component B are respectively mixed evenly to obtain component A and component B, and the prepared component A and component B are combined and used in a volume ratio of 1:1 to obtain a low modulus and high strength polyurethane structural adhesive for power battery assembly.

[0046] Preferably, in the above method, the isocyanate-terminated prepolymer is prepared in the following manner, comprising:

[0047] Heat the diol to 110-120°C, stir and evacuate at the same time, dehydrate for 1-3 hours, cool to below 50°C, fill with nitrogen, add isocyanate at a ratio of 6-20% of theoretical NCO content, heat to 65-85°C, continue stirring to react for 1-3 hours, until the titration NCO content no longer changes, end the reaction, and cool to room temperature to obtain a terminal isocyanate prepolymer;

[0048] The isocyanate-based silane coupling agent-modified polyether polyol is prepared in the following manner, comprising:

[0049] Heat the polyether polyol to 110-120°C, stir and evacuate at the same time, dehydrate for 1-3 hours, cool to below 50°C, fill with nitrogen, add isocyanate silane coupling agent according to the ratio of NCO:OH=1.005:1~1.3:1, heat to 70-90°C, continue stirring to react for 1-3 hours, until the titration NCO content no longer changes, end the reaction, and cool to room temperature to obtain isocyanate silane coupling agent modified polyether polyol.

[0050] In order to more clearly demonstrate the technical solution and technical effects provided by the present invention, a low modulus and high strength polyurethane structural adhesive for power battery assembly and a preparation method thereof provided by an embodiment of the present invention are described in detail with reference to specific embodiments below.

[0051] Example 1

[0052] This embodiment provides a low modulus and high strength polyurethane structural adhesive for power battery assembly, and the preparation method thereof includes:

[0053] Preparing in advance an isocyanate-based silane coupling agent-modified polyether polyol and an isocyanate-terminated prepolymer, wherein the raw materials of the isocyanate-based silane coupling agent-modified polyether polyol and the isocyanate-terminated prepolymer are calculated by weight;

[0054] (1) Preparing an isocyanate silane coupling agent modified polyether polyol, comprising: taking 100 parts of polypropylene glycol with a molecular weight of 12,000, stirring and heating to 120° C., maintaining vacuum to remove water for 2 hours, cooling to 45° C., filling with nitrogen, adding 3.59 parts of isocyanate propyltrimethoxysilane, slowly heating to 85° C., stirring for reaction for 3 hours, and cooling to room temperature to obtain an isocyanate silane coupling agent modified polyether polyol.

[0055] (2) preparing a terminal isocyanate prepolymer, comprising: taking 50 parts of polypropylene glycol with a molecular weight of 2000, stirring and heating to 120° C., maintaining vacuum to remove water for 2 hours, cooling to 40° C., filling with nitrogen, adding 50 parts of liquefied MDI, slowly heating to 80° C., stirring and reacting for 2 hours, and cooling to room temperature to obtain a terminal isocyanate prepolymer.

[0056] Then, component A and component B are prepared respectively, wherein each raw material in component A and component B is calculated by weight;

[0057] (3) Preparation of component A: 20 parts of hydrogenated castor oil polyol, 15 parts of bisphenol A polyether polyol, 20 parts of polypropylene glycol with a molecular weight of 1000, 0.04 parts of quadrifunctional polyether polyol, 0.05 parts of bismuth isooctanoate, 35 parts of aluminum hydroxide, 8 parts of aluminum hypophosphite, 1 part of fumed silica, and 0.1 parts of water are dispersed and stirred evenly, and component A is obtained after stirring for 2 hours;

[0058] (4) Preparation of component B: 60 parts of isocyanate-terminated prepolymer, 15 parts of isocyanate-silane coupling agent-modified polyether polyol, 23 parts of aluminum hydroxide, 2 parts of γ-methacryloxypropyltrimethoxysilane, 0.2 parts of p-toluenesulfonyl isocyanate, 1 part of fumed silica, and 0.04 parts of chelated tin catalyst were taken, and stirred for 2 hours to obtain component B;

[0059] Example 2

[0060] This embodiment provides a low modulus and high strength polyurethane structural adhesive for power battery assembly, and the preparation method thereof includes:

[0061] Preparing in advance an isocyanate-based silane coupling agent-modified polyether polyol and an isocyanate-terminated prepolymer, wherein the raw materials of the isocyanate-based silane coupling agent-modified polyether polyol and the isocyanate-terminated prepolymer are calculated by weight;

[0062] (1) Preparing an isocyanate silane coupling agent modified polyether polyol, comprising: taking 10 parts of polypropylene glycol with a molecular weight of 4000 and 90 parts of polypropylene glycol with a molecular weight of 12000, stirring and heating to 120° C., maintaining vacuum to remove water for 2 hours, cooling to 45° C., filling with nitrogen, adding 4.305 parts of isocyanate propyltrimethoxysilane, slowly heating to 85° C., stirring for reaction for 2 hours, and cooling to room temperature to obtain an isocyanate silane coupling agent modified polyether polyol.

[0063] (2) preparing a terminal isocyanate prepolymer, comprising: taking 40 parts of polypropylene glycol with a molecular weight of 2000, stirring and heating to 110° C., maintaining vacuum to remove water for 3 hours, cooling to 40° C., filling with nitrogen, adding 60 parts of liquefied MDI, slowly heating to 75° C., stirring and reacting for 2.5 hours, and cooling to room temperature to obtain a terminal isocyanate prepolymer.

[0064] Then, component A and component B are prepared respectively, wherein each raw material in component A and component B is calculated by weight;

[0065] (3) Preparation of component A: 10 parts of castor oil, 30 parts of hydrogenated castor oil polyol, 20 parts of bisphenol A polyether polyol, 0.7 parts of tetrafunctional polyether polyol as a crosslinking agent, 0.08 parts of bismuth isooctanoate, 23 parts of aluminum hydroxide, 8 parts of aluminum hypophosphite, 2 parts of fumed silica, and 0.2 parts of water, disperse and stir evenly, and stir for 3 hours to obtain component A;

[0066] (4) Preparation of component B: 60 parts of isocyanate-terminated prepolymer, 10 parts of isocyanate-silane coupling agent-modified polyether polyol, 28 parts of aluminum hydroxide, 2 parts of γ-methacryloxypropyltrimethoxysilane, 0.2 parts of p-toluenesulfonyl isocyanate, 2 parts of fumed silica, and 0.04 parts of chelated tin catalyst were stirred for 3 hours to obtain component B;

[0067] Example 3

[0068] This embodiment provides a low modulus and high strength polyurethane structural adhesive for power battery assembly, and the preparation method thereof includes:

[0069] Preparing in advance an isocyanate-based silane coupling agent-modified polyether polyol and an isocyanate-terminated prepolymer, wherein the raw materials of the isocyanate-based silane coupling agent-modified polyether polyol and the isocyanate-terminated prepolymer are calculated by weight;

[0070] (1) Preparing an isocyanate silane coupling agent modified polyether polyol, comprising: taking 100 parts of polypropylene glycol with a molecular weight of 8000, stirring and heating to 120° C., maintaining vacuum to remove water for 2 hours, cooling to 45° C., filling with nitrogen, adding 5.23 parts of isocyanate propyl dimethoxy silane, slowly heating to 80° C., stirring for reaction for 3 hours, and cooling to room temperature to obtain an isocyanate silane coupling agent modified polyether polyol.

[0071] (2) preparing a terminal isocyanate prepolymer, comprising: taking 20 parts of polypropylene glycol with a molecular weight of 2000 and 20 parts of poly(hexamethylene dimer glycol) with a molecular weight of 2000, heating the mixture to 120° C. while stirring, maintaining vacuum to remove water for 2 hours, cooling the mixture to 40° C., introducing nitrogen, adding 60 parts of liquefied MDI, slowly heating the mixture to 80° C., stirring the mixture for reaction for 2 hours, and cooling the mixture to room temperature to obtain a terminal isocyanate prepolymer.

[0072] Then, component A and component B are prepared respectively, wherein each raw material in component A and component B is calculated by weight;

[0073] (3) Preparation of component A: 40 parts of hydrogenated castor oil polyol, 20 parts of bisphenol A polyether polyol, 10 parts of polypropylene glycol with a molecular weight of 1000, 0.8 parts of N,N,N',N'-tetrakis-(2-hydroxypropyl)ethylenediamine, 0.05 parts of bismuth isooctanoate, 30 parts of aluminum hydroxide, 8 parts of aluminum hypophosphite, 2 parts of fumed silica, and 0.1 parts of water are dispersed and stirred evenly, and component A is obtained after stirring for 2 hours;

[0074] (4) Preparation of component B: 65 parts of isocyanate-terminated prepolymer, 10 parts of isocyanate silane coupling agent-modified polyether polyol, 23 parts of aluminum hydroxide, 2 parts of γ-methacryloxypropyltrimethoxysilane, 0.2 parts of p-toluenesulfonyl isocyanate, 2 parts of fumed silica, and 0.04 parts of chelated tin catalyst were taken, and stirred for 2 hours to obtain component B;

[0075] Example 4

[0076] This embodiment provides a low modulus and high strength polyurethane structural adhesive for power battery assembly, and the preparation method thereof includes:

[0077] Preparing in advance an isocyanate-based silane coupling agent-modified polyether polyol and an isocyanate-terminated prepolymer, wherein the raw materials of the isocyanate-based silane coupling agent-modified polyether polyol and the isocyanate-terminated prepolymer are calculated by weight;

[0078] (1) Preparation of terminal isocyanate prepolymer: 40 parts of poly(hexamethylene dimer) diol with a molecular weight of 2000 were taken, heated to 120°C while stirring, and vacuumed to remove water for 2 h, cooled to 40°C, filled with nitrogen, added with 60 parts of liquefied MDI, slowly heated to 80°C, stirred for reaction for 2 h, and cooled to room temperature to obtain a terminal isocyanate prepolymer.

[0079] (2) Preparation of component A: 30 parts of hydrogenated castor oil polyol, 20 parts of bisphenol A polyether polyol, 10 parts of polypropylene glycol with a molecular weight of 1000, 0.4 parts of N,N,N',N'-tetrakis-(2-hydroxypropyl)ethylenediamine, 0.05 parts of bismuth isooctanoate, 30 parts of aluminum hydroxide, 8 parts of aluminum hypophosphite, 2 parts of fumed silica, and 0.1 parts of water, disperse and stir evenly, and stir for 2 hours to obtain component A;

[0080] Then, component A and component B are prepared respectively, wherein each raw material in component A and component B is calculated by weight;

[0081] (3) Preparation of component B: 60 parts of terminal isocyanate prepolymer, 15 parts of MS resin S203H, 23 parts of aluminum hydroxide, 2 parts of γ-methacryloxypropyltrimethoxysilane, 0.2 parts of p-toluenesulfonyl isocyanate, 2 parts of fumed silica, and 0.04 parts of chelated tin catalyst were taken, and stirred for 2 hours to obtain component B;

[0082] The low modulus and high strength polyurethane structural adhesive for power battery assembly prepared in the above embodiments was used in combination with component A and component B in a volume ratio of 1:1. The tensile strength, shear strength, modulus, and flame retardancy at 25°C were tested, as were the tensile strength and shear strength after double 85 aging for 1000 hours. Untreated aluminum alloy and PET were used as the substrate.

[0083]

[0084]

[0085] It can be seen from the test data in the above table that the low modulus and high strength polyurethane structural adhesive for power battery assembly of the present invention has a low modulus of less than 400 MPa, excellent tensile strength, excellent shear strength for untreated Al and PET, and flame retardant performance that can reach the flame retardant level. After double 85 aging for 1000 hours, the attenuation is less than 20%, which can effectively ensure the stable performance of the power battery during long-term use in complex environments such as high-frequency vibration, damp heat, severe cold, extreme heat, heat accumulation, etc., thereby improving reliability and safety.

[0086] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed in the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims. The information disclosed in the background technology section of this article is only intended to deepen the understanding of the overall background technology of the present invention, and should not be regarded as an admission or in any form that the information constitutes prior art known to those skilled in the art.

Claims

1. A low modulus and high strength polyurethane structural adhesive for power battery assembly, It is characterized in that include: Component A and component B, wherein the volume ratio of component A to component B is 1:1, and the molar ratio of functional groups is: NCO:OH=1.05:1-2.0:1; The component A is composed of the following raw materials in parts by mass: 5-30 parts of bio-based polyol, 10-30 parts of aromatic ring modified polyol, 0.001-15 parts of polyether polyol, 0.001-3 parts of cross-linking agent, 0.001-0.1 parts of catalyst, 15-45 parts of flame retardant, 0.001-0.3 parts of water and 0.001-5 parts of thixotropic agent; The B component is composed of the following raw materials in parts by mass: 0.001-15 parts of isocyanate, 35-75 parts of terminal isocyanate polyurethane prepolymer, 5-25 parts of isocyanate silane coupling agent modified polyether polyol, 10-25 parts of flame retardant; 0.001-5 parts of coupling agent, 0.001-0.3 parts of water absorbent, 0.001-5 parts of thixotropic agent and 0.001-0.1 parts of catalyst.

2. The low modulus and high strength polyurethane structural adhesive for power battery assembly according to claim 1, It is characterized in that In the component A, the bio-based polyol is one or more of soybean oil, castor oil, palm oil, hydrogenated castor oil, and aromatic ring-modified castor oil; The aromatic ring modified polyol is one or more of bisphenol A or bisphenol F modified polyether diol with a molecular weight of 400-3000, or phthalic anhydride polyester diol; The polyether polyol is polypropylene glycol with a molecular weight of 400-2000.

3. The low modulus and high strength polyurethane structural adhesive for power battery assembly according to claim 1 or 2, It is characterized in that In the component A, the crosslinking agent is one or more polyether polyols or amines with a functionality of 4-6.

4. The low modulus and high strength polyurethane structural adhesive for power battery assembly according to claim 1 or 2, It is characterized in that In the A component and the B component, the catalyst is one or more of bismuth isooctanoate, bismuth laurate, bismuth neodecanoate, bismuth cyclohexaneate, zinc isooctanoate, zinc neodecanoate, dibutyltin dilaurate, stannous octoate, and chelated tin; The flame retardant is one or more of aluminum hydroxide, magnesium hydroxide, aluminum hypophosphite, aluminum diethylphosphinate, tricresyl phosphate, triethyl phosphate, and tri(chloroisopropyl) phosphate; In the component A and the component B, the thixotropic agent is one or more of fumed silica and bentonite.

5. The low modulus and high strength polyurethane structural adhesive for power battery assembly according to claim 1 or 2, It is characterized in that In the B component, the isocyanate is one or more of diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, toluene diisocyanate, isophorone diisocyanate, hexamethylene isocyanate, liquefied MDI, polymeric MDI, HDI trimer, and TDI trimer; The terminal isocyanate polyurethane prepolymer is produced by reacting a diol with a molecular weight of 1000-3000 with an isocyanate, and the mass fraction of NCO is controlled to be 6-22%; The isocyanate silane coupling agent modified polyether polyol is produced by the reaction of an isocyanate silane coupling agent and a polyether polyol, and the molar ratio is controlled to be: NCO:OH=1.005:1-1.3:

1.

6. The low modulus and high strength polyurethane structural adhesive for power battery assembly according to claim 5, It is characterized in that The diol in the isocyanate-terminated polyurethane prepolymer is one or more of polypropylene glycol, polyethylene glycol, polyethylene adipate glycol diol, polyneopentyl adipate glycol diol, and polyhexamethylene dimer glycol diol; The isocyanate in the isocyanate-terminated polyurethane prepolymer is one or more of diphenylmethane diisocyanate, dicyclohexylmethane diisocyanate, toluene diisocyanate, isophorone diisocyanate, hexamethylene isocyanate, liquefied MDI, polymerized MDI, HDI trimer, and TDI trimer.

7. The low modulus and high strength polyurethane structural adhesive for power battery assembly according to claim 5, It is characterized in that In the isocyanate silane coupling agent modified polyether polyol, the isocyanate silane coupling agent is one or more of isocyanate propyl triethoxy silane, isocyanate propyl trimethoxy silane and isocyanate propyl dimethoxy silane; and the polyether polyol is polypropylene glycol with a molecular weight of 3000-16000.

8. The low modulus and high strength polyurethane structural adhesive for power battery assembly according to claim 1 or 2, It is characterized in that In the component B, the water absorbing agent is p-toluenesulfonyl isocyanate.

9. A method for preparing the low modulus and high strength polyurethane structural adhesive for power battery assembly according to any one of claims 1 to 8, It is characterized in that The following steps are involved: preparing a terminal isocyanate prepolymer and an isocyanate silane coupling agent modified polyether polyol respectively; According to the formula of component A and component B described in any one of claims 1 to 8, the constituent raw materials of component A and component B are respectively taken, and the raw materials of component A and component B are respectively mixed evenly to obtain component A and component B, and the prepared component A and component B are combined and used in a volume ratio of 1:1 to obtain a low modulus and high strength polyurethane structural adhesive for power battery assembly.

10. The method for preparing the low modulus and high strength polyurethane structural adhesive for power battery assembly according to claim 9, It is characterized in that The isocyanate-terminated prepolymer is prepared in the following manner, comprising: Heat the diol to 110-120°C, stir and evacuate at the same time, dehydrate for 1-3 hours, cool to below 50°C, fill with nitrogen, add isocyanate at a ratio of 6-20% of theoretical NCO content, heat to 65-85°C, continue stirring to react for 1-3 hours, until the titration NCO content no longer changes, end the reaction, and cool to room temperature to obtain a terminal isocyanate prepolymer; The isocyanate-based silane coupling agent-modified polyether polyol is prepared in the following manner, comprising: Heat the polyether polyol to 110-120°C, stir and evacuate at the same time, dehydrate for 1-3 hours, cool to below 50°C, fill with nitrogen, add isocyanate silane coupling agent according to the ratio of NCO:OH=1.005:1~1.3:1, heat to 70-90°C, continue stirring to react for 1-3 hours, until the titration NCO content no longer changes, end the reaction, and cool to room temperature to obtain isocyanate silane coupling agent modified polyether polyol.

Citation Information

Patent Citations

  • Polyurethane adhesive used for structural bonding of power battery PACK

    CN109609081A

  • Heat-conducting two-component polyurethane adhesive and preparation method and application thereof

    CN113999643A