A method for preparing a metallic pigment protective layer

By using materials such as tetraethoxysilane, dimethyl azobisisobutyrate and 3-aminopropyltriethoxysilane in the metallic pigment protective layer to form a dense organic layer, and adding dibromo-p-methylazo Methanesulfonate solves the problem of the protective layer of metallic pigments reducing gloss and water solubility, significantly improves the color brightness and hydrophilicity of metallic pigments, and expands its application scope.

CN116694113BActive Publication Date: 2024-10-01GUANGZHOU XINBO PIGMENT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310609738.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-29
Publication Date
2024-10-01
Estimated Expiration
2043-05-29

AI Technical Summary

Technical Problem

The existing metallic pigment protective layer will reduce the metallic gloss, saturation and water solubility of the metallic pigment, limiting its application scope.

Method used

Using materials such as tetraethoxysilane, dimethyl azobisisobutyrate, 3-aminopropyltriethoxysilane and dibromo-p-methylazomethanesulfonate, a dense organic layer is formed through hydrolysis and condensation polymerization reactions. , enhance the gloss and color of metallic pigments, and add 3-aminopropyltriethoxysilane and 3-(2-aminoethyl)-aminopropyltrimethoxysilane to synergistically improve the hydrophilicity and color of metallic pigments. Dispersion.

Benefits of technology

It effectively maintains the metallic luster of metallic pigments, enhances the brightness and saturation of colors, improves its dispersion and hydrophilic durability in water, and expands its application range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004252149820000081
    Figure BDA0004252149820000081
  • Figure BDA0004252149820000091
    Figure BDA0004252149820000091
  • Figure BDA0004252149820000092
    Figure BDA0004252149820000092
Patent Text Reader

Abstract

The present invention relates to a method for preparing a metal pigment protective layer, and belongs to the technical field of preparing a metal pigment protective layer. The present invention adds tetraethoxysilane, dimethyl azobisisobutyrate and 3-aminopropyltriethoxysilane to prepare a metal pigment protective layer, effectively maintaining the metallic luster unique to the metal pigment; dibromo-p-methylazosulfonate is added to make the color of the metal pigment more vivid and saturated. In addition, the present invention adds 3-aminopropyltriethoxysilane and 3-(2-aminoethyl)-aminopropyltrimethoxysilane synergistically in the process of preparing the metal pigment protective layer, significantly improving the dispersibility of the metal pigment in water, further enhancing the hydrophilicity and hydrophilic durability of the metal pigment surface, solving the problem of weak solubility of the metal pigment, and also expanding the application range of the metal pigment, making it more suitable for use in complex environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of metal pigment protective layer preparation, and in particular, relates to a method for preparing a metal pigment protective layer. Background Art

[0002] Metallic pigments are a kind of high-end pigments widely used in the fields of spraying, manicure, cosmetics, automobile spray painting, etc. They show shiny metallic luster and rich color effects on the surface. And with the continuous improvement of people's requirements for the performance of metallic pigments, in order to enhance the metallic gloss, saturation and water solubility of metallic pigments, improve their application fields and application effects, metallic pigment protective layer technology has come into being. At the same time, in the near future, metallic pigment coating protective layer technology will be more and more widely used in all walks of life. However, there are few studies on metallic pigment protective layers on the market, and due to the special properties of metallic pigments, there are certain challenges in the preparation of their protective layer technology. As for the existing metallic pigment protective layers, due to the color, structure and other factors of the protective layer, there is a general problem of reducing the metallic gloss, saturation and water solubility of the metallic pigment. Therefore, it is particularly important to find a preparation method for a metallic pigment protective layer that can solve these problems. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a metal pigment protective layer, wherein tetraethoxysilane, dimethyl azobisisobutyrate and 3-aminopropyltriethoxysilane are added to obtain a metal pigment protective layer, which effectively maintains the metallic luster unique to the metal pigment; dibromomethyl azosulfonate is added to make the color of the metal pigment more vivid and saturated. In addition, the present invention further adds 3-aminopropyltriethoxysilane and 3-(2-aminoethyl)-aminopropyltrimethoxysilane to the synergistic effect in the process of preparing the metal pigment protective layer, which significantly improves the dispersibility of the metal pigment in water, further enhances the hydrophilicity and hydrophilic durability of the metal pigment surface, solves the problem of weak solubility of the metal pigment, and also expands the application range of the metal pigment, making it more suitable for use in complex environments. The problem that the metal pigment protective layer in the prior art weakens the luster, color and hydrophilicity of the metal pigment is solved.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A method for preparing a metallic pigment protective layer, the method comprising the following steps:

[0006] S10, pre-treating part of the raw materials to obtain pre-treated pigment, mixed solution A and mixed solution B;

[0007] S20, preparing a mixed solution C: controlling the temperature and stirring the pretreated pigment, anhydrous ethanol, tetraethoxysilane, dimethyl azobisisobutyrate, mixed solution A, mixed solution B and aqueous ammonia to obtain a mixed solution C;

[0008] S30, preparing a mixed solution D: taking the mixed solution C, and adding dibromo-p-methylazosulfonylamine, ethanol and dimethyl sulfoxide thereto, and stirring under controlled temperature to obtain a mixed solution D;

[0009] S40, filtering the mixed solution D, washing the filter cake with ethanol and then with distilled water, respectively, and drying the washed filter cake under vacuum at controlled temperature to obtain a metal pigment protective layer.

[0010] As a preferred solution of the present invention, the specific operation steps of step S10 are:

[0011] S11, washing the pigment with ethanol and then with distilled water, and then vacuum drying to obtain a pretreated pigment;

[0012] S12, 3-aminopropyltriethoxysilane, methanol and deionized water are mixed evenly, and then the pH is adjusted. After the adjustment is completed, the mixture is allowed to stand to obtain a mixed solution A for standby use;

[0013] S13, 3-(2-aminoethyl)-aminopropyltrimethoxysilane, methanol and deionized water are mixed evenly, and then the pH is adjusted. After the adjustment is completed, the mixture is allowed to stand to obtain a mixed solution B for standby use.

[0014] As a preferred embodiment of the present invention, the pigment in step S11 is a metallic pigment; the washing times of ethanol and distilled water are 3-5 times respectively; the temperature of the vacuum drying is 50-55° C., and the time is 1-1.5 h.

[0015] As a preferred embodiment of the present invention, the volume ratio of 3-aminopropyltriethoxysilane, methanol and deionized water in step S12 is 20-25:70-75:8-10; the volume ratio of 3-(2-aminoethyl)-aminopropyltrimethoxysilane, methanol and deionized water in step S13 is 20-25:70-75:8-10.

[0016] As a preferred embodiment of the present invention, the pH adjustment in step S12 and step S13 is: adjusting the pH to 9.5-10 using glacial acetic acid, and the standing time is 22-24 hours.

[0017] As a preferred embodiment of the present invention, the dosage ratio of the pretreated pigment, anhydrous ethanol, tetraethoxysilane, dimethyl azobisisobutyrate, mixed solution A, mixed solution B and ammonia water in step S20 is 2-5g:80-100mL:2-3mL:0.1-0.2g:2-3mL:3-4mL:6-10mL.

[0018] As a preferred embodiment of the present invention, the temperature-controlled stirring in step S20 is specifically as follows: under nitrogen conditions, the temperature is controlled at 50-75° C. and stirred for 3-6 hours.

[0019] As a preferred embodiment of the present invention, the dosage ratio of the mixed solution C, dibromo-p-methylazosulfonate, ethanol and dimethyl sulfoxide in step S30 is 80-100 mL: 0.5-1 g: 10-15 mL: 10-20 mL.

[0020] As a preferred embodiment of the present invention, the temperature of the temperature-controlled stirring in step S30 is 60-80° C., and the stirring time is 20-24 hours.

[0021] As a preferred embodiment of the present invention, the washing times of ethanol and distilled water in step S40 are 3-5 times respectively; the temperature of the temperature-controlled vacuum drying is 60-70° C., and the time is 4-6 hours.

[0022] Beneficial effects of the present invention:

[0023] (1) The present invention adds tetraethoxysilane, dimethyl azobisisobutyrate and 3-aminopropyl triethoxysilane to prepare a metal pigment protective layer, which effectively maintains the metallic luster unique to the metal pigment. This is because tetraethoxysilane and 3-aminopropyl triethoxysilane will undergo hydrolysis and polycondensation reactions in the system, bond with the surface of the metal pigment to form new bonds, and on this basis, dimethyl azobisisobutyrate is added to generate free radicals, which trigger the system to form more active chains, further promote the chain growth and mutual entanglement in the system, and finally form a dense organic layer on the surface of the metal pigment, which increases the uniformity and smoothness of the organic layer on the surface of the metal pigment, while effectively maintaining the metallic luster unique to the metal pigment.

[0024] (2) The present invention adds dibromo-p-methylazosulfonyl to make the color of the metallic pigment more vivid and saturated. This is because dibromo-p-methylazosulfonyl contains bonding structures such as benzene rings and azo groups that absorb and reflect light of a specific wavelength. When it absorbs photons, it captures the energy and releases stronger and more vivid light, thereby increasing the light absorption range and reflection intensity of the metallic pigment, thereby enhancing the vividness and saturation of the metallic pigment's color.

[0025] (3) The present invention adds 3-aminopropyl triethoxysilane and 3-(2-aminoethyl)-aminopropyl trimethoxysilane in the process of preparing the metal pigment protective layer, and the synergistic effect significantly improves the dispersibility of the metal pigment in water, further enhances the hydrophilicity and hydrophilic durability of the metal pigment surface, solves the problem of weak solubility of the metal pigment, and also expands the application range of the metal pigment, making it more suitable for use in complex environments. This is because the two silane molecules added in the present invention have complementary functions and characteristics. Specifically, 3-aminopropyl triethoxysilane and 3-(2-aminoethyl)-aminopropyl trimethoxysilane can adsorb each other through hydrogen bonds between their respective functional groups to form a layer of dense silicon-oxygen bond ring structure, which reduces the surface energy, thereby greatly increasing the hydrophilicity of the metal pigment surface. At the same time, the ethoxy and methoxy groups in the two silane molecules can form a stable chemical bond layer with the metal pigment surface, thereby increasing the hydrophilic durability of the metal particle surface. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] A method for preparing a metallic pigment protective layer, the method comprising the following steps:

[0029] S10, pre-treating part of the raw materials to obtain pre-treated pigment, mixed solution A and mixed solution B:

[0030] S11, washing the metallic pigment with ethanol for 3 times and then with distilled water for 5 times, and then vacuum drying at 53° C. for 1 h to obtain a pretreated pigment;

[0031] S12, 20 mL of 3-aminopropyltriethoxysilane, 75 mL of methanol and 8 mL of deionized water were mixed evenly, and then the pH was adjusted to 9.5 with glacial acetic acid. After the adjustment, the mixture was allowed to stand for 23 hours to obtain a mixed solution A for standby use;

[0032] S13, 23 mL of 3-(2-aminoethyl)-aminopropyltrimethoxysilane, 73 mL of methanol and 8 mL of deionized water were mixed evenly, and then the pH was adjusted to 10 with glacial acetic acid. After the adjustment, the mixture was allowed to stand for 24 hours to obtain a mixed solution B for standby use;

[0033] S20, preparing mixed solution C: taking 2 g of pretreated pigment, 90 mL of anhydrous ethanol, 2 mL of tetraethoxysilane, 0.1 g of dimethyl azobisisobutyrate, 3 mL of mixed solution A, 3.5 mL of mixed solution B and 6 mL of ammonia water, stirring at 75° C. for 3 h, to obtain mixed solution C;

[0034] S30, preparing a mixed solution D: taking 80 mL of the mixed solution C, and adding 1 g of dibromo-p-methylazosulfonylamine, 10 mL of ethanol and 10 mL of dimethyl sulfoxide to the mixed solution C, and stirring at 80° C. for 20 h to obtain a mixed solution D;

[0035] S40, filtering the mixed solution D, washing the filter cake with ethanol and then with distilled water for 4 times, respectively, and drying the washed filter cake under vacuum at 65° C. for 4 hours to obtain a metal pigment protective layer.

[0036] Example 2

[0037] A method for preparing a metallic pigment protective layer, the method comprising the following steps:

[0038] S10, pre-treating part of the raw materials to obtain pre-treated pigment, mixed solution A and mixed solution B:

[0039] S11, washing the metallic pigment with ethanol 4 times and then with distilled water 3 times, and then vacuum drying at 50° C. for 1 h to obtain a pretreated pigment;

[0040] S12, 23 mL of 3-aminopropyltriethoxysilane, 70 mL of methanol and 10 mL of deionized water were mixed evenly, and then the pH was adjusted to 10 with glacial acetic acid. After the adjustment, the mixture was allowed to stand for 24 hours to obtain a mixed solution A for standby use;

[0041] S13, 20 mL of 3-(2-aminoethyl)-aminopropyltrimethoxysilane, 75 mL of methanol and 9 mL of deionized water were mixed evenly, and then the pH was adjusted to 10 with glacial acetic acid. After the adjustment, the mixture was allowed to stand for 23 hours to obtain a mixed solution B for standby use;

[0042] S20, preparing mixed solution C: taking 5 g of pretreated pigment, 100 mL of anhydrous ethanol, 2.5 mL of tetraethoxysilane, 0.2 g of dimethyl azobisisobutyrate, 2 mL of mixed solution A, 4 mL of mixed solution B and 8 mL of ammonia water, stirring at 63° C. for 4.5 h, to obtain mixed solution C;

[0043] S30, preparing a mixed solution D: taking 100 mL of the mixed solution C, and adding 0.5 g of dibromo-p-methylazosulfonylamine, 13 mL of ethanol and 10 mL of dimethyl sulfoxide to the mixed solution C, and stirring at 60° C. for 24 h to obtain a mixed solution D;

[0044] S40, filtering the mixed solution D, washing the filter cake with ethanol and then with distilled water for 5 times, respectively, and drying the washed filter cake under vacuum at 60° C. for 6 h to obtain a metal pigment protective layer.

[0045] Example 3

[0046] A method for preparing a metallic pigment protective layer, the method comprising the following steps:

[0047] S10, pre-treating part of the raw materials to obtain pre-treated pigment, mixed solution A and mixed solution B:

[0048] S11, washing the metallic pigment with ethanol for 5 times and then with distilled water for 4 times, and then vacuum drying at 55° C. for 1.5 h to obtain a pretreated pigment;

[0049] S12, 25 mL of 3-aminopropyltriethoxysilane, 73 mL of methanol and 9 mL of deionized water were mixed evenly, and then the pH was adjusted to 10 with glacial acetic acid. After the adjustment, the mixture was allowed to stand for 23 hours to obtain a mixed solution A for standby use;

[0050] S13, 25 mL of 3-(2-aminoethyl)-aminopropyltrimethoxysilane, 70 mL of methanol and 10 mL of deionized water were mixed evenly, and then the pH was adjusted to 9.5 with glacial acetic acid. After the adjustment, the mixture was allowed to stand for 23 hours to obtain a mixed solution B for standby use;

[0051] S20, preparing mixed solution C: taking 4 g of pretreated pigment, 80 mL of anhydrous ethanol, 3 mL of tetraethoxysilane, 0.2 g of dimethyl azobisisobutyrate, 2.5 mL of mixed solution A, 3 mL of mixed solution B and 10 mL of ammonia water, stirring at 50° C. for 6 h, to obtain mixed solution C;

[0052] S30, preparing a mixed solution D: taking 90 mL of the mixed solution C, and adding 1 g of dibromo-p-methylazosulfonylamine, 15 mL of ethanol and 15 mL of dimethyl sulfoxide to the mixed solution C, and stirring at 70° C. for 22 h to obtain a mixed solution D;

[0053] S40, filtering the mixed solution D, washing the filter cake three times with ethanol and then with distilled water, respectively, and drying the washed filter cake under vacuum at 70° C. for 5 h to obtain a metal pigment protective layer.

[0054] Comparative Example 1

[0055] Compared with Example 1, the difference is that tetraethoxysilane is not added in Comparative Example 1, and the addition amounts of other raw materials and the operating steps remain unchanged.

[0056] Comparative Example 2

[0057] Compared with Example 1, the difference is that in Comparative Example 2, dimethyl azobisisobutyrate is not added, and the amounts of other raw materials added and the operating steps remain unchanged.

[0058] Comparative Example 3

[0059] Compared with Example 1, the difference is that in Comparative Example 3, 3-aminopropyltriethoxysilane is not added, and the amounts of other raw materials added and the operating steps remain unchanged.

[0060] Comparative Examples 4-5

[0061] Compared with Example 1, the difference is that the amounts of 3-aminopropyltriethoxysilane and 3-(2-aminoethyl)-aminopropyltrimethoxysilane used in Comparative Example 4-5 are as shown in Table 1, and the amounts of other raw materials added and the operating steps remain unchanged.

[0062] Table 1

[0063] 3-Aminopropyltriethoxysilane (mL) 3-(2-Aminoethyl)-aminopropyltrimethoxysilane (mL) Comparative Example 4 0 43 Comparative Example 5 43 0

[0064] Comparative Example 6

[0065] Compared with Example 1, the difference is that in Comparative Example 6, dibromo-p-methylazosulfonyl is not added, and the amounts of other raw materials added and the operating steps remain unchanged.

[0066] Test Example 1

[0067] (1) The common coating and scratching card method was used to evaluate the metallic gloss of the metallic pigments prepared in Examples 1-3 and Comparative Examples 1-3, and the color saturation of the metallic pigments prepared in Examples 1-3 and Comparative Example 6. Specifically, a metallic pigment protective layer accounting for 10% of the total mass fraction was added to the acrylic resin, and the film was formed by coating and scratching the card, and then dried. The gloss (L value) and color saturation (C value) data at five angles were measured using an X-Rite MA68 colorimeter to reflect the following aspects of the metallic pigment: 1) metallic gloss; 2) color saturation;

[0068] Data is presented in CIE L*, a*, b* system; L* value represents brightness, c value (c 2 =a 2 +b 2 ) represents color concentration, the results of metallic luster are shown in Table 2, and the results of color saturation are shown in Table 3.

[0069] (2) The color vividness of the metallic pigments obtained in Examples 1 to 3 and Comparative Example 6 was visually observed by the naked eyes of the same observer and scored. The results are shown in Table 3;

[0070] The scoring standard is: 5 points (the metallic pigment has bright colors), 3 points (the metallic pigment has relatively bright colors), and 1 point (the metallic pigment has yellowing or blackening).

[0071] Table 2

[0072] 15° 25° 45° 75° 110° Example 1 126.47 101.83 75.75 65.37 65.03 Example 2 125.91 101.07 75.11 64.55 64.49 Example 3 125.84 101.02 74.98 64.47 64.26 Comparative Example 1 85.50 60.43 33.49 21.53 21.04 Comparative Example 2 93.65 66.85 42.43 30.84 29.15 Comparative Example 3 83.32 57.81 31.07 20.85 20.19

[0073] Table 3

[0074]

[0075]

[0076] It can be seen from Table 2 and Table 3 that the metallic pigment protective layer prepared in the present invention effectively maintains the metallic luster unique to the metallic pigment and enhances the brightness and saturation of the color development of the metallic pigment. This is because, tetraethoxysilane, dimethyl azobisisobutyrate and 3-aminopropyltriethoxysilane are added in the present invention, and tetraethoxysilane and 3-aminopropyltriethoxysilane will undergo hydrolysis and polycondensation reactions in the system, bond with the surface of the metal pigment to form new bonds, and on this basis, dimethyl azobisisobutyrate is added to generate free radicals, which trigger the system to form more active chains, further promote the chain growth and mutual entanglement in the system, and finally form a dense organic layer on the surface of the metal pigment, thereby increasing the uniformity and smoothness of the organic layer on the surface of the metal pigment and effectively maintaining the unique metallic luster of the metal pigment; in addition, dibromo-p-methylazosulfonate is added in the present invention, and the bonding structure of the benzene ring and azo group contained in dibromo-p-methylazosulfonate absorbs and reflects light of a specific wavelength. When it absorbs photons, it captures energy and releases stronger and brighter light, thereby increasing the light absorption range and reflection intensity of the metal pigment, and further enhancing the brightness and saturation of the color of the metal pigment.

[0077] Test Example 2

[0078] (1) Hydrophilicity test: The metal pigments prepared in Examples 1-3 and Comparative Examples 4-5 were tested for water contact angle using a contact angle meter by a static drop-three-point method. The results are shown in Table 4.

[0079] (2) Hydrophilic durability test: The metallic pigments prepared in Examples 1-3 and Comparative Examples 4-5 were immersed in 250 mL of distilled water at 35° C. for 8 days. The immersion solution was replaced every other day. The contact angles were measured using a contact angle meter on the 0th, 2nd, 4th, 6th and 8th days, respectively. The changes in the contact angles of the sample surfaces were observed. The results are shown in Table 4.

[0080] Table 4

[0081]

[0082]

[0083] As can be seen from Table 4, the present invention adds 3-aminopropyl triethoxysilane and 3-(2-aminoethyl)-aminopropyl trimethoxysilane in the process of preparing the metal pigment protective layer, which has a synergistic effect, significantly improving the dispersibility of the metal pigment in water, and further enhancing the hydrophilicity and hydrophilic durability of the metal pigment surface. This is because the two silane molecules added in the present invention have complementary functions and characteristics. Specifically, 3-aminopropyl triethoxysilane and 3-(2-aminoethyl)-aminopropyl trimethoxysilane can adsorb each other through hydrogen bonds between their respective functional groups to form a layer of dense silicon-oxygen bond ring structure, which reduces the surface energy, thereby greatly increasing the hydrophilicity of the metal pigment surface. At the same time, the ethoxy and methoxy groups in the two silane molecules can form a stable chemical bond layer with the metal pigment surface, thereby increasing the hydrophilic durability of the metal particle surface.

[0084] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0085] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for preparing a metal pigment protective layer, characterized in that: The preparation method comprises the following steps: S10, pre-treating part of the raw materials to obtain pre-treated pigment, mixed solution A and mixed solution B; S20, preparing a mixed solution C: controlling the temperature and stirring the pretreated pigment, anhydrous ethanol, tetraethoxysilane, dimethyl azobisisobutyrate, mixed solution A, mixed solution B and aqueous ammonia to obtain a mixed solution C; The dosage ratio of the pretreated pigment, anhydrous ethanol, tetraethoxysilane, dimethyl azobisisobutyrate, mixed solution A, mixed solution B and ammonia water is 2-5g:80-100mL:2-3mL:0.1-0.2g:2-3mL:3-4mL:6-10mL; S30, preparing a mixed solution D: taking the mixed solution C, and adding dibromo-p-methylazosulfonylamine, ethanol and dimethyl sulfoxide thereto, and stirring under controlled temperature to obtain a mixed solution D; S40, filtering the mixed solution D, washing the filter cake with ethanol and then with distilled water, respectively, and drying the washed filter cake under vacuum at a controlled temperature to obtain a metal pigment protective layer; The specific operation steps of step S10 are: S11, washing the pigment with ethanol and then with distilled water, and then vacuum drying to obtain a pretreated pigment; The pigment is a metallic pigment; S12, 3-aminopropyltriethoxysilane, methanol and deionized water are mixed evenly, and then the pH is adjusted. After the adjustment is completed, the mixture is allowed to stand to obtain a mixed solution A for standby use; The volume ratio of the 3-aminopropyltriethoxysilane, methanol and deionized water is 20-25:70-75:8-10; S13, 3-(2-aminoethyl)-aminopropyltrimethoxysilane, methanol and deionized water are mixed evenly, and then the pH is adjusted. After the adjustment is completed, the mixture is allowed to stand to obtain a mixed solution B for standby use; The volume ratio of the 3-(2-aminoethyl)-aminopropyltrimethoxysilane, methanol and deionized water is 20-25:70-75:8-10.

2. The method for preparing a metal pigment protective layer according to claim 1, characterized in that: In step S11, the washing times of ethanol and distilled water are 3-5 times respectively; the temperature of vacuum drying is 50-55° C., and the time is 1-1.5 h.

3. The method for preparing a metal pigment protective layer according to claim 1, characterized in that: The pH adjustment in step S12 and step S13 is: using glacial acetic acid to adjust the pH to 9.5-10, and the standing time is 22-24 hours.

4. The method for preparing a metal pigment protective layer according to claim 1, characterized in that: The temperature-controlled stirring in step S20 specifically includes: controlling the temperature at 50-75° C. and stirring for 3-6 hours under nitrogen conditions.

5. The method for preparing a metal pigment protective layer according to claim 1, characterized in that: In step S30, the dosage ratio of the mixed solution C, dibromo-p-methylazosulfonyl, ethanol and dimethyl sulfoxide is 80-100 mL: 0.5-1 g: 10-15 mL: 10-20 mL.

6. The method for preparing a metal pigment protective layer according to claim 1, characterized in that: The temperature of the temperature-controlled stirring in step S30 is 60-80° C., and the stirring time is 20-24 hours.

7. The method for preparing a metal pigment protective layer according to claim 1, characterized in that: In step S40, the washing times of ethanol and distilled water are 3-5 times respectively; the temperature of the temperature-controlled vacuum drying is 60-70° C., and the time is 4-6 hours.