A coating resistant to strong alkali cleaning and a coating method

By designing a multi-layer structure on the lens coating and adjusting the gas ratio, the problem of poor resistance of existing coatings during strong alkali cleaning is solved, higher density and acid resistance are achieved, reducing the need for manual wiping, and improving the Application range of coating.

CN116695073BActive Publication Date: 2024-11-01XUZHOU LIANCHAO PHOTOELECTRIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310155188.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-23
Publication Date
2024-11-01
Estimated Expiration
2043-02-23

AI Technical Summary

Technical Problem

The existing lens coating has poor resistance when washed with strong alkali, resulting in a short ring measurement time, requiring a lot of manual wipe, and the film-forming structure is not dense, which limits its application range.

Method used

Multi-layer coating structures are provided on the glass substrate in turn, including silica, titanium pentoxide, lanthanide materials, etc., through the ion source film formation process and the adjustment of the oxygen and argon ratio, a columnar structure coating is formed to increase the density of the coating. and acid-resistant.

Benefits of technology

It significantly improves the alkali resistance and density of the coating, extends the ring measurement time, reduces the need for manual wiping, and enhances the corrosion resistance and strength of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116695073B_ABST
    Figure CN116695073B_ABST
Patent Text Reader

Abstract

The present invention proposes a coating resistant to strong alkali cleaning, including a glass substrate, on which a silicon dioxide coating, titanium pentoxide, silicon dioxide coating, titanium pentoxide, silicon dioxide coating, titanium pentoxide, silicon dioxide, lanthanide material coating, silicon dioxide, lanthanide material coating are sequentially arranged, and the coating method thereof includes: S1: providing a glass substrate; S2: vacuumizing a coating sputtering machine to 5.00*10‑3PA; S3: pre-melting of materials, fixing three groups of cathode targets in a cavity, taking solid titanium pentoxide and pre-melting and heating to liquid by setting the current intensity of the equipment to 440MA, taking a lanthanide material in the form of solid powder to cooperate with a titanium dioxide target and tantalum pentoxide, the present invention adopts an ion source film forming process using TI3O5 / SIO2 for film forming, and simultaneously adding an appropriate amount of lanthanide material for film processing, and the film forming structure is columnar, and the system density is better. And the coating process can ensure the film strength and the density of the film by adjusting the ratio of oxygen and argon, and improve the acid and alkali resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of lens coating, in particular to a coating resistant to strong alkali cleaning and a coating method. Background Art

[0002] The vacuum film-forming process generally consists of a vacuum chamber, an exhaust system, a heating system, a film-forming material heating system and a monitoring system. The film-forming products are widely used, such as mobile phone cameras, cameras, projectors, security cameras, etc.

[0003] At present, the commonly used method in China is to use TI3O5 / SIO2 for film formation by heating. The film structure is layered and has poor density (attached Figure 1 ), resulting in a shorter subsequent environmental test time, and it can actually only be used as an internal accessory of the equipment. At the same time, the cleaning alkali resistance (PH ≥ 12, temperature: 70 degrees, time: 5 minutes) is not good, which causes trouble to the finished product process. More manpower is required for manual wiping operations. Summary of the invention

[0004] In order to solve the above technical problems, the present invention proposes a coating resistant to strong alkali cleaning, including a glass substrate, on which a silicon dioxide coating, a titanium pentoxide, a silicon dioxide coating, a titanium pentoxide, a silicon dioxide coating, a titanium pentoxide, a silicon dioxide coating, a titanium pentoxide, a silicon dioxide, a lanthanide material coating, a silicon dioxide, and a lanthanide material coating are sequentially arranged.

[0005] Preferably, the lanthanide material coating includes one or a mixture of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium.

[0006] Preferably, the lanthanide material is also mixed with tantalum and titanium elements.

[0007] A coating method for a strong alkali-resistant coating, comprising the following steps:

[0008] S1: providing a glass substrate;

[0009] S2: Vacuum the coating sputtering machine to 5.00*10-3PA;

[0010] S3: Pre-melting of materials. Three groups of cathode targets are fixed in the cavity. Solid titanium pentoxide is pre-melted and heated to liquid by setting the current intensity of the equipment to 440MA. Lanthanide materials in solid powder form are combined with titanium dioxide target and tantalum pentoxide. The current intensity of the equipment is set to 480MA and pre-melted and heated to liquid, so that the lanthanide materials are mixed with titanium and tantalum elements. After cooling down, solid cathode targets are formed. Silicon dioxide is used as the third group of cathode targets.

[0011] S4: Material evaporation, followed by injection of oxygen and argon, with the ratio of oxygen to argon being 1:3-5; ionizing the argon through a sputtering device, bombarding the cathode target with ions, and sputtering in the order of silicon dioxide, titanium pentoxide, silicon dioxide, titanium pentoxide, silicon dioxide, titanium pentoxide, silicon dioxide, lanthanide material coating, silicon dioxide, and lanthanide material coating. The obtained titanium pentoxide coating has a thickness of 450nm, the current used is 420MA, and the rate is The thickness of silicon dioxide coating is 418nm, the current is 180MA, and the rate is The coating thickness of the lanthanide material mixture is 53nm, the current is 460MA, and the rate is

[0012] S5: Maintain pressure for 30 minutes;

[0013] S6: Perform deflation operation;

[0014] S7: Alkali resistance cleaning measurement spectrum inspection packaging process.

[0015] Preferably, the ratio and amount of argon and oxygen are adjusted during the evaporation process. When plating silicon dioxide and titanium pentoxide, the total amount injected is 1 and 0.8%, and the injection ratio of oxygen and argon is 1:3 and 2:5. When plating lanthanide material coating, the total amount injected is 0.4%, and the injection ratio of oxygen and argon is 1:5.

[0016] Preferably, the pre-dissolution temperature is 1800°C-2000°C.

[0017] The coating resistant to strong alkali cleaning proposed by the present invention has the following beneficial effects: the present invention adopts an ion source film forming process using Ti3O5 / SIO2 to form a film, and at the same time adds an appropriate amount of lanthanide materials to process the film, and the film structure is columnar (attached Figure 2 ), the density is better. And the coating process can ensure the strength and density of the film by adjusting the ratio of oxygen and argon, and improve the acid and alkali resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for describing the embodiments are briefly introduced below.

[0019] Figure 1 It is a microscopic picture of the coating of common silicon dioxide and titanium pentoxide in the prior art;

[0020] Figure 2 It is a coating structure diagram of the present invention;

[0021] Figure 3 It is a microscopic picture of the coating of the present invention;

[0022] Figure 4 A summary table of the test method of the reliability test report of the present invention;

[0023] Figure 5 The coating spectrophotometer of the present invention;

[0024] Figure 6 A cleaning spectrophotometer test table according to the present invention;

[0025] Figure 7 It is a high temperature and high humidity storage test table of the present invention;

[0026] Figure 8 The hot and cold shock test table of the present invention;

[0027] Fig. 9 A high temperature storage test table of the present invention;

[0028] Fig.10 The low temperature storage test table of the present invention;

[0029] Among them, 1. liquid storage cylinder; 1A, liquid baffle; 2. inlet pipeline; 3. outlet pipeline; 4. ventilation pipeline; 5. first flow control component; 6. high-pressure gas; 7. liquid connecting pipeline; 8. second flow control component; 9. low-pressure pipeline. DETAILED DESCRIPTION

[0030] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention.

[0031] Example 1

[0032] A coating resistant to strong alkali cleaning comprises a glass substrate, on which silicon dioxide coating, titanium pentoxide, silicon dioxide coating, titanium pentoxide, silicon dioxide coating, titanium pentoxide, silicon dioxide, a cerium-tantalum-titanium mixed layer, silicon dioxide and a lanthanide material coating are sequentially arranged.

[0033] Example 2

[0034] A coating resistant to strong alkali cleaning comprises a glass substrate, on which a silicon dioxide coating, a titanium pentoxide, a silicon dioxide coating, a titanium pentoxide, a silicon dioxide coating, a titanium pentoxide, a silicon dioxide coating, a titanium pentoxide, a silicon dioxide, a lanthanum-tantalum-titanium mixed layer, a silicon dioxide and a lanthanide material coating are sequentially arranged.

[0035] Example 3

[0036] A coating resistant to strong alkali cleaning comprises a glass substrate, on which a silicon dioxide coating, a titanium pentoxide, a silicon dioxide coating, a titanium pentoxide, a silicon dioxide coating, a titanium pentoxide, a silicon dioxide coating, a titanium pentoxide, a silicon dioxide, a praseodymium-tantalum-titanium mixed layer, a silicon dioxide and a lanthanide material coating are sequentially arranged.

[0037] Example 4

[0038] A coating resistant to strong alkali cleaning comprises a glass substrate, on which a silicon dioxide coating, a titanium pentoxide, a silicon dioxide coating, a titanium pentoxide, a silicon dioxide coating, a titanium pentoxide, a silicon dioxide coating, a titanium pentoxide, a silicon dioxide, a europium tantalum titanium mixed layer, a silicon dioxide and a lanthanide material coating are sequentially arranged.

[0039] Example 5

[0040] A coating method for a strong alkali-resistant coating, comprising the following steps:

[0041] S1: providing a glass substrate;

[0042] S2: Vacuum the coating sputtering machine to 5.00*10 -3 PA;

[0043] S3: Pre-melting of materials. Three groups of cathode targets are fixed in the cavity. Solid titanium pentoxide is taken and pre-melted and heated to liquid by setting the current intensity of the equipment to 440MA. The pre-melting temperature is 1800℃. Lanthanide materials in solid powder form are matched with titanium dioxide target and tantalum pentoxide. Lanthanide metal materials, titanium dioxide and tantalum pentoxide are also melted and mixed at this temperature. The current intensity of the equipment is set to 480MA and pre-melted and heated to liquid. The lanthanide materials are mixed with titanium and tantalum elements. After cooling down, solid cathode targets are formed. Silicon dioxide is used as the third group of cathode targets.

[0044] S4: Material evaporation, followed by injection of oxygen and argon, the oxygen and argon injection amounts are 1% and 0.8% of the cavity, and the ratios of oxygen and argon are 1:3 and 2:5; argon is ionized by sputtering equipment, and ions bombard the cathode target material. The cathode target material rotates through the turntable inside the sputtering equipment, and the position of the cathode target can be adjusted. The sputtering is carried out in the order of silicon dioxide, titanium pentoxide, silicon dioxide, titanium pentoxide, silicon dioxide, titanium pentoxide, silicon dioxide, lanthanide material coating, silicon dioxide, and lanthanide material coating. When sputtering the lanthanide material mixed coating, the gas injection amount is 0.4%, and the obtained titanium pentoxide coating thickness is 450nm. The current used is: 420MA, and the rate is: The thickness of silicon dioxide coating is 418nm, the current is 180MA, and the rate is The coating thickness of the lanthanide material mixture is 53nm, the current is 460MA, and the rate is

[0045] S5: Maintain pressure for 30 minutes;

[0046] S6: Perform deflation operation;

[0047] S7: Alkali resistance cleaning measurement spectrum inspection packaging process.

[0048] Adjust the ratio of argon and oxygen. The increase of argon ratio can increase the power of particles, which can make the density of coating higher, so as to increase acid and alkali resistance and enhance weather resistance. Increasing the amount of gas can increase the film thickness. Due to the adjustment of gas injection amount between different layers, the proportion of oxygen also changes, the film thickness is different, and due to the change of oxygen amount, the stress inside the film is reduced, which improves the strength of the film.

[0049] Comparative Example

[0050] Take a glass substrate, and sequentially coat the glass substrate with a silicon dioxide coating, a titanium pentoxide, a silicon dioxide coating, a titanium pentoxide, a silicon dioxide coating, a titanium pentoxide, and a silicon dioxide.

[0051] The coating process is:

[0052] S1: providing a glass substrate;

[0053] S2: Vacuum the coating sputtering machine to 5.00*10 -3 PA;

[0054] S3: Pre-melting of materials. Fix two groups of cathode targets in the chamber. Take solid titanium pentoxide and pre-melt it to liquid by setting the current intensity of the equipment to 440MA. The pre-melting temperature is 1800℃. Take silicon dioxide as the cathode target. After cooling down, each of them forms a solid cathode target.

[0055] S4: material evaporation, followed by injection of oxygen and argon, the amount of oxygen and argon injected is 1% of the cavity, and the ratio of oxygen to argon is 1:3; argon is ionized by sputtering equipment, and ions bombard the cathode target material. The cathode target material rotates through the turntable inside the sputtering equipment, and the position of the cathode target can be adjusted in the order of silicon dioxide, titanium pentoxide, silicon dioxide, titanium pentoxide, silicon dioxide, titanium pentoxide, silicon dioxide, S5: pressure maintenance for 30 minutes;

[0056] S6: Perform deflation operation;

[0057] S7: Alkali resistance cleaning measurement spectrum inspection packaging process.

[0058] The following tests were performed on the products in the above embodiments and the coatings prepared in the comparative examples:

[0059] Coating spectrophotometry test: Perform spectrophotometry test on the coated product, output the spectrum curve, and judge whether the spectrum meets the specification requirements; the results are detailed in Figure 5

[0060] Cleaning spectrophotometry test: The product after cleaning with a high pH solution is subjected to spectrophotometry test, and the spectrum curve is output. The spectrum meets the specification requirements. See Table 6 for the results.

[0061] High temperature and high humidity storage: ① Set the constant temperature box to 85℃±3℃ and the relative humidity to 85%±5%; ② Place the test sample in the constant temperature box for 1000h; ③ Allow the sample to recover at room temperature (25℃±5℃) for 24h, and perform spectrometry, appearance, and film strength; see Table 7 for the results.

[0062] Thermal shock: ① Cycle 1000 hours in a storage environment with a cycle of (low temperature -40℃±2℃ (30 minutes) and high temperature 85℃±3℃ (30 minutes)); Temperature exchange time: 5 minutes ② The sample is restored at room temperature (25℃±5℃) for 24 hours, and then the spectroscopic, appearance and film strength tests are carried out; the results are shown in Table 8

[0063] High temperature storage: ① Set the temperature of the thermostat to 105℃±3℃ and place it in the thermostat for 1000h ② Let the sample recover at room temperature (25℃±5℃) for 24h, and then perform spectroscopic, appearance and film strength tests. The results are shown in Table 9

[0064] Low temperature storage: ① Set the thermostat temperature to -40℃±3℃ and place it in the thermostat for 1000h; ② Let the sample recover at room temperature (25℃±5℃) for 24h, and then perform spectrometry, appearance and film strength tests. The results are shown in Table 10

[0065] In the above test, the products in Examples 1-4 all meet the requirements, and the products prepared by the method of Example 5 all meet the requirements. However, after the comparative example was soaked in a high pH solution and then subjected to the above test, obvious defects occurred on the surface, and it was not suitable for use.

[0066] This product, by adding lanthanide materials to the coating layer, and mixing tantalum and titanium elements, the sizes of different ions are different, and the gap between the film layers is reduced after coating, which can be seen in Figure 1 and Figure 2 The microscopic image after coating in this embodiment greatly improves the coating density, thereby improving the corrosion resistance. Another factor that increases the coating density also includes coordinating the coating process. In the coating process, by adjusting the ratio of argon and oxygen, the increase in the amount of argon increases the power of ions, thereby increasing the density of the coating. At the same time, different coatings are carried out in the same cavity and different amounts of oxygen are injected. The change in the amount of oxygen reduces the coating stress between different layers and improves the strength of the coating.

Claims

1. A coating method for a strong alkali-resistant coating, characterized in that: The following steps are involved: S1: providing a glass substrate; S2: Vacuum the coating sputtering machine to 5.00*10 -3 Pa; S3: Pre-melting of materials: Fix three sets of cathode targets in the chamber. Take solid titanium pentoxide and pre-melt it to liquid by setting the current intensity of the equipment to 440MA. Take solid powdered lanthanide material, mix it with titanium dioxide target and tantalum pentoxide, and pre-melt it to liquid by setting the current intensity of the equipment to 480MA. Mix the lanthanide material with titanium and tantalum elements, and form solid cathode targets after cooling. Silicon dioxide serves as the third set of cathode targets. S4: Material evaporation, followed by injection of oxygen and argon, with the ratio of oxygen to argon being 1:3~5; argon is ionized by sputtering equipment, and the ions bombard the cathode target, and the sputtering is carried out in the order of silicon dioxide, titanium pentoxide, silicon dioxide, titanium pentoxide, silicon dioxide, titanium pentoxide, silicon dioxide, lanthanide material coating, silicon dioxide, and lanthanide material coating. The obtained titanium pentoxide coating has a thickness of 450nm, using a current of 420MA and a rate of 3.5Å / sec; the silicon dioxide coating has a thickness of 418nm, using a current of 180MA and a rate of 8.0Å / sec; the lanthanide material mixture coating has a thickness of 53nm, using a current of 460MA and a rate of 2.5Å / sec; S5: Maintain pressure for 30 minutes; S6: perform deflation operation; S7: Alkali resistance cleaning measurement spectrum inspection packaging process.

2. The coating film resistant to strong alkali cleaning according to claim 1, characterized in that: The ratio and amount of argon and oxygen are adjusted during the evaporation process. When coating silicon dioxide and titanium pentoxide, the total injection amount is 1% and 0.8% respectively, and the injection ratio of oxygen and argon is 1:3 and 2:

5. When coating lanthanide materials, the total injection amount is 0.4%, and the injection ratio of oxygen and argon is 1:

5.

3. The coating film resistant to strong alkali cleaning according to claim 1, characterized in that: The pre-melting temperature is 1800℃-2000℃.