A nano-silver graphene composite antibacterial coating material and preparation method thereof
By adding nano-silver graphene composite filler to the epoxy resin and modifying it, coating materials with antibacterial and flame retardant properties were prepared, which solved the problem of the lack of antibacterial properties of existing epoxy resin-based coatings, and achieved bacterial control Effective suppression and improvement of flame retardant performance are suitable for applications in various places.
Patent Information
- Application Number
- CN202310756464.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-06-26
AI Technical Summary
Existing epoxy resin-based insulating powder coatings lack antibacterial properties and are difficult to provide effective bacterial inhibition in hospitals, schools and other places.
Add nano silver graphene composite filler to the epoxy resin and modify the modification composition to prepare nano silver graphene composite antibacterial coating material, combined with curing agent and leveling agent, extrusion and grinding through twin screws The powder process produces coating materials with antibacterial and flame retardant properties.
实现了涂层材料的抗菌性能和阻燃性能的提升,尤其通过改性纳米银石墨烯复合填料的使用,显著提高了阻燃性能,能够对大肠杆菌和金黄色黄葡萄球菌的抑菌率达到99.99%,氧指数达到57%,适用于多种场所的应用。
Smart Images

Figure BDA0004302965860000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coating preparation, and in particular to a nano silver graphene composite antibacterial coating material and a preparation method thereof. Background Art
[0002] Antibacterial coatings refer to coatings that have antibacterial effects on bacteria; they are widely used in hospitals, schools and other places, as well as bank ATMs, communication equipment and public transportation equipment; they achieve their antibacterial effects by adding antibacterial agents to the coatings. Nanosilver antibacterial is a metallic silver element with a particle size of nanometers, which has antibacterial and bactericidal properties; it is usually used as an antibacterial agent added to coatings.
[0003] Chinese invention patent 201910989713.8 discloses an insulating powder coating. The insulating powder coating comprises the following raw material components by weight: 60-80 parts of epoxy resin; 20-30 parts of silicon powder; 5-10 parts of calcium silicate; 3-5 parts of ammonium polyphosphate; 1-3 parts of benzoin; 20-40 parts of curing agent; 1-5 parts of accelerator; 1-5 parts of leveling agent; and has good insulating properties.
[0004] The powder coating is prepared with epoxy resin as raw material; the technical problem it aims to solve is insulation; it does not have antibacterial effect. Therefore, it is of great application value to develop a coating material with antibacterial effect using epoxy resin as raw material. Summary of the invention
[0005] In order to overcome at least one of the technical problems existing in the prior art, the present invention provides a nano silver graphene composite antibacterial coating material.
[0006] The technical solution of the present invention is as follows:
[0007] A nano silver graphene composite antibacterial coating material comprises the following raw material components in parts by weight:
[0008] 80-120 parts of epoxy resin; 20-40 parts of nano silver graphene composite filler; 5-10 parts of curing agent; 1-5 parts of leveling agent.
[0009] The invention uses epoxy resin as a raw material, and by adding nano silver graphene composite filler therein, the prepared nano silver graphene composite antibacterial coating material has antibacterial performance and also has certain flame retardant performance.
[0010] Preferably, the nano silver graphene composite antibacterial coating material comprises the following raw material components in parts by weight: 90-110 parts of epoxy resin; 30-40 parts of nano silver graphene composite filler; 6-8 parts of curing agent; and 2-3 parts of leveling agent.
[0011] Most preferably, the nano silver graphene composite antibacterial coating material comprises the following raw material components in parts by weight: 100 parts of epoxy resin; 30 parts of nano silver graphene composite filler; 7 parts of curing agent; and 3 parts of leveling agent.
[0012] Preferably, the nano-silver-graphene composite filler is a mixture of nano-silver and graphene in a weight ratio of 1:2-4.
[0013] Most preferably, the nano-silver-graphene composite filler is a mixture of nano-silver and graphene in a weight ratio of 1:3.
[0014] Preferably, the nano silver graphene composite filler is a modified nano silver graphene composite filler;
[0015] The modified nano silver graphene composite filler is prepared by the following method:
[0016] (1) mixing nano silver and graphene to obtain a mixture raw material;
[0017] (2) adding the mixture raw material into the solvent and mixing to obtain a first mixed solution;
[0018] (3) adding the modified composition to the first mixed solution, heating to 60-80° C. and stirring for 3-6 hours to obtain a second mixed solution;
[0019] (4) separating the solid from the second mixed liquid, and drying to obtain the modified nano-silver graphene composite filler. The inventors surprisingly found in a large number of experiments that adding the modified nano-silver graphene composite filler prepared by the above method to the nano-silver graphene composite antibacterial coating material can further significantly improve the flame retardant properties of the nano-silver graphene composite antibacterial coating material compared to adding the unmodified nano-silver graphene composite filler.
[0020] Further preferably, in step (1), the weight ratio of nanosilver to graphene is 1:2-4.
[0021] Most preferably, the weight ratio of nanosilver to graphene in step (1) is 1:3.
[0022] Most preferably, the solvent in step (1) is water.
[0023] Further preferably, in step (2), the ratio of the mixture raw material to the solvent is 1 kg: 6 to 10 L.
[0024] Most preferably, the ratio of the mixture raw material to the solvent in step (2) is 1 kg:8 L.
[0025] More preferably, in step (3), the ratio of the first mixed solution to the modified composition is 1 L: 40-60 g.
[0026] Most preferably, in step (3), the ratio of the first mixed solution to the modified composition is 1 L:50 g.
[0027] Further preferably, the modified composition in step (3) consists of polyglycerol-10 diisostearate and potassium lauryl ether phosphate.
[0028] The inventors need to emphasize here that in the preparation process of modified nano-silver graphene composite fillers, the modified composition is very critical; the modified nano-silver graphene composite filler obtained by modifying with a single polyglycerol-10 diisostearate or a single potassium lauryl ether phosphate cannot significantly improve the flame retardant properties of the nano-silver graphene composite antibacterial coating material compared with the unmodified nano-silver graphene composite filler; the modified nano-silver graphene composite filler obtained by modifying with a modified composition composed of polyglycerol-10 diisostearate and potassium lauryl ether phosphate must be selected at the same time, compared with the unmodified nano-silver graphene composite filler, to significantly improve the flame retardant properties of the nano-silver graphene composite antibacterial coating material.
[0029] Preferably, the weight ratio of polyglyceryl-10 diisostearate to potassium laureth phosphate is 2 to 4:1 to 3. Most preferably, the weight ratio of polyglyceryl-10 diisostearate to potassium laureth phosphate is 3:2.
[0030] The present invention also provides a method for preparing the above-mentioned nano silver graphene composite antibacterial coating material, which comprises the following steps:
[0031] The epoxy resin, nano silver graphene composite filler or modified nano silver graphene composite filler, curing agent and leveling agent are uniformly mixed, extruded through a twin-screw extruder, crushed by tabletting, and then pulverized by a grinder to obtain the nano silver graphene composite antibacterial coating material.
[0032] Beneficial effects: The present invention provides a new nano-silver graphene composite antibacterial coating material; the epoxy resin is used as a raw material, and by adding a nano-silver graphene composite filler therein, the prepared nano-silver graphene composite antibacterial coating material has antibacterial properties; and also has certain flame retardant properties. In addition, adding the modified nano-silver graphene composite filler prepared by the method of the present invention to the nano-silver graphene composite antibacterial coating material can further significantly improve the flame retardant properties of the nano-silver graphene composite antibacterial coating material compared to adding an unmodified nano-silver graphene composite filler. DETAILED DESCRIPTION
[0033] The present invention is further explained below in conjunction with specific examples, but the examples do not limit the present invention in any form.
[0034] The epoxy resin used in the following examples is E-12 (604) epoxy resin; the remaining raw materials whose sources are not indicated are conventional raw materials that can be purchased by those skilled in the art through conventional purchasing channels; the sources of the above raw materials of the present invention do not limit the scope of protection of the present invention.
[0035] Example 1 Preparation of Nano-Silver Graphene Composite Antibacterial Coating Material
[0036] Raw materials by weight: 100 parts of epoxy resin; 30 parts of nano silver graphene composite filler; 7 parts of curing agent (adipic acid dihydrazide); 3 parts of leveling agent (leveling agent PV88);
[0037] The nano silver graphene composite filler is formed by mixing nano silver and graphene in a weight ratio of 1:3.
[0038] Preparation method: epoxy resin, nano silver graphene composite filler, curing agent and leveling agent are uniformly mixed, extruded through a twin-screw extruder, crushed by tabletting, and then pulverized by a grinder to obtain the nano silver graphene composite antibacterial coating material.
[0039] Example 2 Preparation of Nano-Silver Graphene Composite Antibacterial Coating Material
[0040] Raw materials are composed by weight: 100 parts of epoxy resin; 30 parts of modified nano silver graphene composite filler; 7 parts of curing agent (adipic acid dihydrazide); 3 parts of leveling agent (leveling agent PV88);
[0041] The modified nano silver graphene composite filler is prepared by the following method:
[0042] (1) mixing nanosilver and graphene in a weight ratio of 1:3 to obtain a mixture raw material;
[0043] (2) adding the mixture raw material into water to obtain a first mixed solution; wherein the ratio of the mixture raw material to water is 1 kg:8 L;
[0044] (3) adding the modified composition to the first mixed solution, heating to 70° C. and stirring for 4 hours to obtain a second mixed solution; wherein the amount ratio of the first mixed solution to the modified composition is 1L:50g; the modified composition is composed of polyglycerol-10 diisostearate and potassium lauryl ether phosphate in a weight ratio of 3:2;
[0045] (4) Separating the solid from the second mixed liquid and drying it to obtain the modified nano silver graphene composite filler.
[0046] Preparation method: epoxy resin, modified nano silver graphene composite filler, curing agent and leveling agent are uniformly mixed, extruded through a twin-screw extruder, crushed by tabletting, and then pulverized by a grinder to obtain the nano silver graphene composite antibacterial coating material.
[0047] Example 3 Preparation of Nano-Silver Graphene Composite Antibacterial Coating Material
[0048] Raw materials by weight: 80 parts of epoxy resin; 20 parts of modified nano silver graphene composite filler; 5 parts of curing agent (adipic acid dihydrazide); 5 parts of leveling agent (leveling agent PV88);
[0049] The modified nano silver graphene composite filler is prepared by the following method:
[0050] (1) mixing nanosilver and graphene in a weight ratio of 1:2 to obtain a mixture raw material;
[0051] (2) adding the mixture raw material into water to obtain a first mixed solution; wherein the ratio of the mixture raw material to water is 1 kg:6 L;
[0052] (3) adding the modified composition to the first mixed solution, heating to 60° C. and stirring for 6 hours to obtain a second mixed solution; wherein the amount ratio of the first mixed solution to the modified composition is 1L:40g; the modified composition is composed of polyglycerol-10 diisostearate and potassium lauryl ether phosphate in a weight ratio of 2:1;
[0053] (4) Separating the solid from the second mixed liquid and drying it to obtain the modified nano silver graphene composite filler.
[0054] Preparation method: epoxy resin, modified nano silver graphene composite filler, curing agent and leveling agent are uniformly mixed, extruded through a twin-screw extruder, crushed by tabletting, and then pulverized by a grinder to obtain the nano silver graphene composite antibacterial coating material.
[0055] Example 4 Preparation of Nano-Silver Graphene Composite Antibacterial Coating Material
[0056] Raw materials by weight: 120 parts of epoxy resin; 40 parts of modified nano silver graphene composite filler; 10 parts of curing agent (adipic acid dihydrazide); 1 part of leveling agent (leveling agent PV88);
[0057] The modified nano silver graphene composite filler is prepared by the following method:
[0058] (1) mixing nanosilver and graphene in a weight ratio of 1:4 to obtain a mixture raw material;
[0059] (2) adding the mixture raw material into water to obtain a first mixed solution; wherein the ratio of the mixture raw material to water is 1 kg:10 L;
[0060] (3) adding the modified composition to the first mixed solution, heating to 80° C. and stirring for 3 hours to obtain a second mixed solution; wherein the amount ratio of the first mixed solution to the modified composition is 1L:60g; the modified composition is composed of polyglycerol-10 diisostearate and potassium lauryl ether phosphate in a weight ratio of 4:3;
[0061] (4) Separating the solid from the second mixed liquid and drying it to obtain the modified nano silver graphene composite filler.
[0062] Preparation method: epoxy resin, modified nano silver graphene composite filler, curing agent and leveling agent are uniformly mixed, extruded through a twin-screw extruder, crushed by tabletting, and then pulverized by a grinder to obtain the nano silver graphene composite antibacterial coating material.
[0063] Comparative Example 1 Preparation of Nano-Silver Graphene Composite Antibacterial Coating Material
[0064] Raw materials are composed by weight: 100 parts of epoxy resin; 30 parts of modified nano silver graphene composite filler; 7 parts of curing agent (adipic acid dihydrazide); 3 parts of leveling agent (leveling agent PV88);
[0065] The modified nano silver graphene composite filler is prepared by the following method:
[0066] (1) mixing nanosilver and graphene in a weight ratio of 1:3 to obtain a mixture raw material;
[0067] (2) adding the mixture raw material into water to obtain a first mixed solution; wherein the ratio of the mixture raw material to water is 1 kg:8 L;
[0068] (3) adding the modifier to the first mixed solution, heating to 70° C. and stirring for 4 hours to obtain a second mixed solution; wherein the amount ratio of the first mixed solution to the modifier is 1L:50g; and the modifier is polyglycerol-10 diisostearate;
[0069] (4) Separating the solid from the second mixed liquid and drying it to obtain the modified nano silver graphene composite filler.
[0070] Preparation method: epoxy resin, modified nano silver graphene composite filler, curing agent and leveling agent are uniformly mixed, extruded through a twin-screw extruder, crushed by tabletting, and then pulverized by a grinder to obtain the nano silver graphene composite antibacterial coating material.
[0071] The difference between Comparative Example 1 and Example 2 is that Comparative Example 1 only uses polyglycerol-10 diisostearate for modification to prepare the modified nano-silver graphene composite filler; while Example 2 uses both polyglycerol-10 diisostearate and potassium lauryl ether phosphate for modification to prepare the modified nano-silver graphene composite filler.
[0072] Comparative Example 2 Preparation of Nano-Silver Graphene Composite Antibacterial Coating Material
[0073] Raw materials are composed by weight: 100 parts of epoxy resin; 30 parts of modified nano silver graphene composite filler; 7 parts of curing agent (adipic acid dihydrazide); 3 parts of leveling agent (leveling agent PV88);
[0074] The modified nano silver graphene composite filler is prepared by the following method:
[0075] (1) mixing nanosilver and graphene in a weight ratio of 1:3 to obtain a mixture raw material;
[0076] (2) adding the mixture raw material into water to obtain a first mixed solution; wherein the ratio of the mixture raw material to water is 1 kg:8 L;
[0077] (3) adding the modifier to the first mixed solution, heating to 70° C. and stirring for 4 hours to obtain a second mixed solution; wherein the amount ratio of the first mixed solution to the modifier is 1L:50g; the modifier is potassium lauryl ether phosphate; (4) separating the solid from the second mixed solution, and obtaining the modified nano-silver graphene composite filler after drying.
[0078] Preparation method: epoxy resin, modified nano silver graphene composite filler, curing agent and leveling agent are uniformly mixed, extruded through a twin-screw extruder, crushed by tabletting, and then pulverized by a grinder to obtain the nano silver graphene composite antibacterial coating material.
[0079] The difference between Comparative Example 2 and Example 2 is that Comparative Example 2 only uses potassium lauryl ether phosphate to modify and prepare the modified nano-silver graphene composite filler; while Example 2 uses both polyglycerol-10 diisostearate and potassium lauryl ether phosphate to modify and prepare the modified nano-silver graphene composite filler.
[0080] The nano silver graphene composite antibacterial coating materials prepared in Examples 1 to 4 and Comparative Examples 1 and 2 were sprayed on steel plates using an electrostatic spray gun, and after the coating was cured; the oxygen index was tested according to the method in GB 8624-2012; the antibacterial performance was tested according to the method in GB / T21866-2008; the test results are shown in Table 1.
[0081] Table 1.
[0082]
[0083] It can be seen from the experimental data in Table 1 that the nano-silver graphene composite antibacterial coating materials prepared in Examples 1 to 4 have an antibacterial rate of 99.99% against Escherichia coli and Staphylococcus aureus; this shows that the nano-silver graphene composite antibacterial coating material of the present invention has excellent antibacterial properties.
[0084] It can be seen from the experimental data in Table 1 that the nano silver graphene composite antibacterial coating material prepared in Example 1 has an oxygen index of 35%, which indicates that the nano silver graphene composite antibacterial coating material of the present invention also has certain flame retardant properties.
[0085] It can be seen from the experimental data in Table 1 that the oxygen index of the nano-silver graphene composite antibacterial coating material prepared in Example 2 reaches 57%, which is significantly higher than that of the nano-silver graphene composite antibacterial coating material prepared in Example 1; this shows that adding the modified nano-silver graphene composite filler prepared by the method of the present invention to the nano-silver graphene composite antibacterial coating material can further significantly improve the flame retardant properties of the nano-silver graphene composite antibacterial coating material compared to adding unmodified nano-silver graphene composite filler.
[0086] It can be seen from the experimental data in Table 1 that the oxygen index of the nano silver graphene composite antibacterial coating materials prepared in Comparative Examples 1 and 2 is improved compared with that in Example 1, but the improvement is not large, and the improvement is much smaller than that of the nano silver graphene composite antibacterial coating material prepared in Example 2; this shows that: in the preparation process of the modified nano silver graphene composite filler, the modified composition is very critical; the modified nano silver graphene composite filler obtained by modifying with a single polyglycerol-10 diisostearate or a single potassium lauryl ether phosphate cannot significantly improve the flame retardant properties of the nano silver graphene composite antibacterial coating material compared with the unmodified nano silver graphene composite filler; the modified nano silver graphene composite filler obtained by modifying with a modified composition composed of polyglycerol-10 diisostearate and potassium lauryl ether phosphate must be selected at the same time, compared with the unmodified nano silver graphene composite filler, to significantly improve the flame retardant properties of the nano silver graphene composite antibacterial coating material.
Claims
1. A nano silver graphene composite antibacterial coating material, It is characterized in that Contains the following parts by weight Raw material components: Epoxy resin 80~120 parts; Nano silver graphene composite filler 20~40 parts; Curing agent 5~10 1~5 parts of leveling agent; The nano silver graphene composite filler is a modified nano silver graphene composite filler; The modified nano silver graphene composite filler is prepared by the following method: (1) Mixing nanosilver and graphene to obtain a mixture raw material; (2) adding the mixed raw material into the solvent to obtain a first mixed liquid; (3) Adding the modified composition to the first mixed solution, heating to 60-80° C. and stirring for 3-6 hours to obtain a second mixed solution; (4) separating the solid from the second mixed liquid, and obtaining the modified nano-silver graphene composite filler after drying; The modified composition described in step (3) consists of polyglycerol-10 diisostearate and potassium lauryl ether phosphate.
2. The nano silver graphene composite antibacterial coating material according to claim 1, It is characterized in that The raw material components include the following parts by weight: 90-110 parts of epoxy resin; 30-40 parts of nano silver graphene composite filler; 6-8 parts of curing agent; 2-3 parts of leveling agent.
3. The nano silver graphene composite antibacterial coating material according to claim 1, It is characterized in that The raw material components include the following parts by weight: 100 parts of epoxy resin; 30 parts of nano silver graphene composite filler; 7 parts of curing agent; 3 parts of leveling agent.
4. The nano silver graphene composite antibacterial coating material according to claim 1, wherein in step (1) The weight ratio of silver to graphene is 1:2~4.
5. The nano silver graphene composite antibacterial coating material according to claim 4, It is characterized in that The weight ratio of nanosilver to graphene in step (1) is 1:
3.
6. The nano silver graphene composite antibacterial coating material according to claim 1, It is characterized in that In step (2), the ratio of the mixture raw material to the solvent is 1 kg: 6-10 L.
7. The nano silver graphene composite antibacterial coating material according to claim 6, It is characterized in that In step (2), the ratio of the mixture raw material to the solvent is 1 kg:8 L.
8. The nano silver graphene composite antibacterial coating material according to claim 1, It is characterized in that In step (3), the ratio of the first mixed solution to the modified composition is 1L: 40-60g.
9. The nano silver graphene composite antibacterial coating material according to claim 8, It is characterized in that In step (3), the ratio of the first mixed liquid to the modified composition is 1L:50g.
10. The method for preparing the nano silver graphene composite antibacterial coating material according to any one of claims 1 to 9, It is characterized in that The following steps are included: The epoxy resin, modified nano silver graphene composite filler, curing agent and leveling agent are mixed evenly and then The nano silver graphene composite antibacterial coating material is obtained by extruding with a twin screw extruder, tabletting and crushing, and then grinding with a grinder.
Citation Information
Patent Citations
An insulating powder coating
CN110698950B
Nanofiller-containing epoxy resins and stable aqueous dispersions thereof
CN101688000A
Graphene nano-silver antibacterial coating and preparation method thereof
CN105419530A
Composite pigment containing organic and inorganic pigment and preparation method thereof
CN107722709A
Graphene-modified antibacterial anticorrosive paint
CN109777262A