A Ti / Fe2O3@Co-MOF composite photoelectrode and its preparation and application
The Ti/Fe2O3@Co-MOF composite photoelectrode, which is doped with Ti and modified with Co-MOF, solves the problems of poor conductivity and slow migration of photogenerated carriers in iron oxide photoelectrodes, improves photoelectrocatalytic performance, and realizes efficient photoelectrochemical water splitting for hydrogen production.
Patent Information
- Application Number
- CN202310656541.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-05
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-06-05
AI Technical Summary
Existing iron oxide photoelectrode materials have poor conductivity, high recombination rate of photogenerated electron-hole pairs, and slow migration rate of photogenerated charge carriers, resulting in low photoelectric conversion efficiency and difficulty in effectively utilizing solar energy for hydrogen production.
The Ti/Fe2O3@Co-MOF composite photoelectrode was prepared by growing Ti-doped FeOOH on FTO conductive glass via hydrothermal method, followed by calcination to form a Ti/Fe2O3 photoelectrode, and then modifying its surface with a Co-MOF cocatalyst layer to form a Ti/Fe2O3@Co-MOF composite photoelectrode.
This improved the absorption band of the photoelectrode to sunlight, enhanced its conductivity and carrier conduction rate, lowered the interfacial charge migration barrier, increased the photocurrent density, and reduced the reaction overpotential, thus achieving highly efficient photoelectrocatalytic water splitting for hydrogen production.
Smart Images

Figure CN116716631B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of photoelectrocatalytic materials technology, specifically relating to a Ti / Fe2O3@Co-MOF composite photoelectrode, its preparation method, and its application. Background Technology
[0002] Energy is the material foundation upon which human society depends for survival and development. With the rapid development of the global economy and human society, the demand for energy has increased exponentially. Currently, the world's energy supply mainly relies on traditional fossil fuels such as coal, oil, and natural gas. However, these fossil fuels are non-renewable and have limited reserves. The overexploitation and utilization of fossil fuels has also brought about a series of serious environmental problems, threatening the sustainable development of human society. Therefore, developing clean and renewable energy is of great strategic significance. Solar energy is a sustainable and clean energy source. Photoelectrochemical hydrogen production is an important method for effectively utilizing solar energy. It can convert solar energy into hydrogen energy for storage and utilization, effectively solving the current energy crisis and environmental pollution problems. In the photoelectrochemical water splitting hydrogen production system, the photoelectrode material is the key factor determining the solar energy conversion efficiency and hydrogen production rate. Developing high-performance photoelectrode materials and improving their photoelectrocatalytic performance is of great significance.
[0003] Among numerous photoelectrocatalytic materials, iron oxide (α-Fe₂O₃) has become a very promising photoelectrocatalytic material due to its narrow band gap (1.9–2.2 eV), wide light absorption range, high catalytic activity, stable chemical properties, abundant, inexpensive, and non-toxic sources. Theoretically, its photocurrent density can reach up to 12.6 mA / cm². 2Iron oxide has an efficiency of up to 6% in converting sunlight into hydrogen energy. However, iron oxide itself also has certain defects: poor conductivity, high recombination rate of photogenerated electron-hole pairs, and slow migration rate of photogenerated charge carriers, which leads to its photoelectric conversion efficiency being far lower than the theoretical value. Doping with n-type dopants (such as Ti, Sn, Mn, and Cr) is a widely used and effective method to improve the conductivity and charge separation efficiency of iron oxide. Among the many element doping methods, Ti doping significantly improves the performance of iron oxide and can greatly increase its photocurrent density; however, Ti doping does not reduce the onset voltage of photocatalysis, and its improvement on the hydrogen production rate is also very limited. Metal-organic frameworks (MOFs) composed of metal ions or clusters coordinated with organic ligands, due to their large specific surface area, tunable structure, and certain photocatalytic activity, can be selected as a co-catalyst to be combined with photoelectrode materials or surface modified to reduce the activation energy required for photocatalytic water splitting, promote the separation of photogenerated electron-hole pairs, accelerate the migration rate of photogenerated charge carriers, increase the rate of surface chemical reactions, and reduce the onset voltage of photocurrent. If the advantages of the above methods can be combined to synergistically improve the catalytic performance of iron oxide, the efficiency of photoelectric water splitting for hydrogen production will be significantly enhanced, which has profound research significance. Summary of the Invention
[0004] The purpose of this invention is to provide a method for preparing a high-performance Ti / Fe2O3@Co-MOF composite photoelectrode and its application. This method not only increases the photocurrent density of hydrogen production through photoelectrocatalytic water splitting but also reduces the overpotential of the reaction, accelerates the migration rate of photogenerated carriers, and improves surface reaction kinetics. This significantly improves the photoelectrocatalytic hydrogen production performance of the electrode material, achieving efficient conversion of solar energy to hydrogen energy. This method has the advantages of simple operation, good repeatability, high conversion efficiency, and wide applicability.
[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0006] A method for preparing a Ti / Fe2O3@Co-MOF composite photoelectrode includes the following steps:
[0007] (1) Place the FTO conductive glass in acetone, anhydrous ethanol and deionized water in sequence for ultrasonic cleaning for 5~40 min, and then place it in an oven at 40~90 ℃ to dry for later use;
[0008] (2) Add anhydrous ferric chloride and sodium nitrate to deionized water and stir until completely dissolved to obtain a mixed solution, thus obtaining the Fe2O3 reaction precursor solution;
[0009] (3) Add titanium source to the mixed solution in step (2) and stir until the mixture is uniform to obtain Ti-doped Fe2O3 reaction precursor solution;
[0010] (4) Place the cleaned FTO conductive glass in step (1) with the conductive surface facing down in the lining of the reactor, and add the reaction precursor liquid prepared in step (2) and (3) into the reactor. Seal the hydrothermal reactor and place it in a forced-air drying oven for hydrothermal reaction. After the reaction is completed, allow it to cool naturally to room temperature.
[0011] (5) Open the reactor, take out the FTO conductive glass, rinse the glass surface repeatedly with deionized water, and put it in a forced-air drying oven at 40~90 ℃ for 1~3 h to obtain FeOOH substrate and Ti / FeOOH substrate conductive glass;
[0012] (6) The FeOOH substrate and Ti / FeOOH substrate conductive glass obtained in step (5) are placed in a muffle furnace and calcined at high temperature to obtain Fe2O3 and Ti / Fe2O3 photoelectrodes;
[0013] (7) Cobalt chloride hexahydrate and 2-mercaptoisonicotinic acid were dissolved in a mixed solvent of 15-30 mL of deionized water and acetonitrile. The mixed solution was sealed in a polytetrafluoroethylene reactor for hydrothermal reaction. After cooling to room temperature and standing for a period of time, orange crystals were obtained. The orange crystals were ground into fine powder, and an appropriate amount of the fine powder was added to anhydrous ethanol and ultrasonically treated for 30-90 min to prepare a Co-MOF suspension.
[0014] (8) Immerse the Ti / Fe2O3 photoelectrode in the Co-MOF suspension in step (7) and let it stand. Then take it out and dry it in a forced-air drying oven at 40~80 ℃ for 5~20 min to finally obtain the Ti / Fe2O3@Co-MOF composite photoelectrode.
[0015] Preferably, in the Fe2O3 reaction precursor solution obtained in step (2), the concentration of anhydrous ferric chloride is 0.01~0.3 mol / L and the concentration of sodium nitrate is 0.5~2 mol / L.
[0016] Preferably, the titanium source in step (3) is TiCl4, and the amount used is 0.2~6.5 μL.
[0017] Preferably, the amount of the reaction precursor liquid added to the reactor in step (4) is 5 to 20 mL.
[0018] Preferably, the hydrothermal reaction temperature in step (4) is 90~150 ℃ and the reaction time is 2~10 h.
[0019] Preferably, the high-temperature calcination procedure in step (6) is a step-by-step calcination. First, the temperature is raised from room temperature to 400-600 ℃ at a heating rate of 2-10 ℃ / min and calcined for 1-2 h. Then, the temperature is raised to 700-800 ℃ at a heating rate of 5-15 ℃ / min and calcined for 10-20 min.
[0020] Preferably, in the mixed solution prepared in step (7), the mass of cobalt chloride hexahydrate is 0.1~0.4 mmol, the mass of 2-mercaptoisonicotinic acid is 0.2~0.6 mmol, the hydrothermal reaction temperature is 130~180 ℃, the reaction time is 1~5 days, and the standing time is 1~3 days.
[0021] Preferably, the concentration of the Co-MOF suspension in step (8) is 0.2~3 mg / mL.
[0022] Preferably, the immersion method described in step (8) is as follows: first, immerse the Ti / Fe2O3 photoelectrode in Co-MOF suspension for 3~12 min, then dry it at 60~80℃ for 5~20 min, and then repeat the above steps 1~6 times after drying the photoelectrode.
[0023] This invention also provides an application of a Ti / Fe2O3@Co-MOF composite photoelectrode in the field of photoelectrocatalytic water splitting. The Ti / Fe2O3@Co-MOF composite photoelectrode is prepared using the method described above. The application method is as follows: A three-electrode system is used, with the Ti / Fe2O3@Co-MOF composite electrode as the working electrode, a Pt sheet as the counter electrode, and a saturated Ag / AgCl electrode as the reference electrode. The electrode is immersed in a 1 mol / L NaOH electrolyte, and under a certain applied voltage, it is irradiated with simulated sunlight using a xenon lamp to perform photoelectrocatalytic water splitting.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) In this invention, Ti-doped FeOOH is grown on the surface of FTO conductive glass using a hydrothermal method, followed by calcination to obtain Ti-doped Fe2O3. A Co-MOF co-catalyst layer is then added to the Ti / Fe2O3 surface using an immersion method to prepare a Ti / Fe2O3@Co-MOF photoelectrode. Compared to Fe2O3 alone, Ti doping broadens the absorption band of the electrode to sunlight, introduces more oxygen vacancies, and results in higher conductivity and increased carrier conduction rate. The Co-MOF co-catalyst modification on the Ti / Fe2O3 surface lowers the interfacial charge migration barrier and improves the kinetics of the water oxidation reaction. The synergistic effect of these two factors accelerates the separation of charges on the electrode surface, thereby increasing the photocurrent density and reducing the reaction overpotential, demonstrating excellent photoelectrocatalytic performance.
[0026] (2) The present invention uses the immersion method to modify the Co-MOF cocatalyst on the Ti / Fe2O3 surface. No special instruments or equipment are needed, and no complicated operation procedures are required. By controlling the immersion time and the number of immersions, the thickness of the Co-MOF cocatalyst layer can be easily controlled. The composite of porous Co-MOF gives the electrode a larger specific surface area and more active catalytic sites, thereby inhibiting the recombination of charge carriers, promoting the separation of electron-hole pairs, and accelerating the reaction rate of hydrogen and oxygen production in water electrolysis.
[0027] (3) The materials used in this invention are inexpensive and abundant, the preparation process is simple and highly controllable, the equipment requirements are low and the preparation cycle is short; the prepared electrodes have excellent chemical stability, good repeatability and high photoelectrocatalytic efficiency, and can be mass-produced industrially, and have a very broad application prospect in the field of photoelectrocatalysis.
[0028] (4) The MOF used in this invention employs ligands containing three different atoms—sulfur, nitrogen, and oxygen—as coordination sites, which can form stable chelated cobalt ion complex structures in various forms. Furthermore, this MOF uses pentanuclear cobalt clusters as building blocks, which can further improve the stability of the MOF structure compared to MOFs with mononuclear metal nodes. Therefore, the MOF composite material in this invention has excellent stability during the PEC water splitting process and can still maintain 95% activity after 10 hours. Attached Figure Description
[0029] Figure 1 SEM images of the photoanodes prepared in Example 2 and Comparative Example 1;
[0030] Figure 2 The XRD patterns are of the photoanodes prepared in Example 2 and Comparative Example 1.
[0031] Figure 3 The UV-Vis diffuse reflectance spectra of the photoanodes prepared in Example 2 and Comparative Example 1 are shown.
[0032] Figure 4 for Figure 3 Kubelka-Munk transform reflectance spectrum;
[0033] Figure 5 The LSV curves of the photoanodes prepared in Example 2 and Comparative Example 1 under illumination and darkness are shown respectively.
[0034] Figure 6 The image shows the light on / off cycle It curves of the photoanodes prepared in Example 2 and Comparative Example 1.
[0035] Figure 7 The ABPE curves of the photoanodic light prepared in Example 2 and Comparative Example 1 are shown.
[0036] Figure 8 The photoanode IPCE spectra prepared in Example 2 and Comparative Example 1 are shown.
[0037] Figure 9 The EIS curves of the photoanodes prepared in Example 2 and Comparative Example 1 under illumination are shown.
[0038] Figure 10 The graphs show the photoelectrochemical stability of the photoanodes prepared in Example 2 and Comparative Example 1. Detailed Implementation
[0039] To make the content of this invention easier to understand, the invention will be further described in detail below with reference to specific embodiments.
[0040] Example 1
[0041] (I) Preparation of Ti / Fe2O3 electrode
[0042] (1) The FTO conductive glass was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 15 min in sequence, and then dried in an oven at 60 ℃ for later use.
[0043] (2) Add 0.01 mol of anhydrous ferric chloride and 0.15 mol of sodium nitrate to 100 mL of deionized water and stir until completely dissolved to obtain Fe2O3 reaction precursor solution; then take 15 mL of the mixed solution and dispense it into a 25 mL polytetrafluoroethylene reactor liner, then add 0.5 μL of TiCl4 into the reactor liner and stir until evenly mixed to obtain Ti-doped Fe2O3 reaction precursor solution;
[0044] (3) Place the cleaned FTO conductive glass from step (1) with its conductive surface facing down into the lining of the reactor containing the Ti-doped Fe2O3 reaction precursor solution, seal the hydrothermal reactor, and place it in a forced-air drying oven for hydrothermal reaction at 120 °C for 6 h. After the reaction is complete, allow it to cool naturally to room temperature. Open the reactor, remove the FTO conductive glass, rinse the glass surface repeatedly with deionized water, and place it in a forced-air drying oven at 60 °C for 1 h to obtain the conductive glass supported on the Ti / FeOOH substrate.
[0045] (4) The conductive glass with Ti / FeOOH substrate obtained in step (3) is placed in a muffle furnace and heated from room temperature to 500 ℃ at a heating rate of 5 ℃ / min, held for 2 h, and then heated from 500 ℃ to 700 ℃ at a heating rate of 10 ℃ / min, and calcined for 15 min to finally obtain Ti / Fe2O3 photoelectrode.
[0046] (II) Preparation of Co-MOF materials
[0047] 59.46 mg of CoCl₂·6H₂O and 77.5 mg of 2-mercaptoisonicotinic acid were dissolved in a mixed solution of 12.5 mL of deionized water and acetonitrile. The mixture was sealed in a 25 mL polytetrafluoroethylene reactor for hydrothermal reaction at 130 °C for 1 day. After cooling to room temperature and standing for 2 days, orange crystals were obtained. The orange crystals were ground into a fine powder and then sonicated with anhydrous ethanol for 30 min to prepare a 2 mg / mL Co-MOF suspension.
[0048] (III) Preparation of Ti / Fe2O3@Co-MOF composite photoelectrode
[0049] The Ti / Fe2O3 photoelectrode was immersed in a 2 mg / mL Co-MOF suspension for 5 min, and then dried in a forced-air drying oven at 60 ℃ for 5 min to finally obtain the Ti / Fe2O3@Co-MOF composite photoelectrode.
[0050] (iv) Performance test of photoelectrochemical catalytic water splitting of Ti / Fe2O3@Co-MOF composite photoelectrode
[0051] A three-electrode testing system was used, with the Ti / Fe2O3@Co-MOF composite electrode prepared in Example 1 as the working electrode, a Pt sheet as the counter electrode, saturated Ag / AgCl as the reference electrode, and 1 mol / L NaOH as the electrolyte, to assemble a photoelectrochemical reactor. The illumination area of the working electrode was limited to 1 square centimeter. A 300 W xenon lamp with an AM1.5 filter was used to obtain simulated sunlight. The light intensity at the location of the working electrode in the reactor was corrected to 100 mW / cm² using a power meter. 2 .
[0052] Example 2
[0053] (I) Preparation of Ti / Fe2O3 electrode
[0054] (1) The FTO conductive glass was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 15 min in sequence, and then dried in an oven at 60 ℃ for later use.
[0055] (2) Add 0.015 mol of anhydrous ferric chloride and 0.1 mol of sodium nitrate to 100 mL of deionized water and stir until completely dissolved to obtain Fe2O3 reaction precursor solution; then take 15 mL of the mixed solution and dispense it into a 25 mL polytetrafluoroethylene reactor liner, then add 1 μL of TiCl4 to the reactor liner and stir until evenly mixed to obtain Ti-doped Fe2O3 reaction precursor solution;
[0056] (3) Place the cleaned FTO conductive glass from step (1) with its conductive surface facing down into the lining of the reactor containing the Ti-doped Fe2O3 reaction precursor solution, seal the hydrothermal reactor, and place it in a forced-air drying oven at 95 ℃ for hydrothermal reaction for 4 h. After the reaction is completed, allow it to cool naturally to room temperature. Open the reactor, remove the FTO conductive glass, rinse the glass surface repeatedly with deionized water, and place it in a forced-air drying oven at 60 ℃ for 1 h to obtain the conductive glass supported on the Ti / FeOOH substrate.
[0057] (4) The conductive glass with Ti / FeOOH substrate obtained in step (3) is placed in a muffle furnace and heated from room temperature to 550 ℃ at a heating rate of 5 ℃ / min, held for 2 h, and then heated from 550 ℃ to 770 ℃ at a heating rate of 10 ℃ / min, and calcined for 15 min to finally obtain Ti / Fe2O3 photoelectrode.
[0058] (II) Preparation of Co-MOF materials (same as Example 1)
[0059] (III) Preparation of Ti / Fe2O3@Co-MOF composite photoelectrode
[0060] The Ti / Fe2O3 photoelectrode was immersed in a 2 mg / mL Co-MOF suspension for 5 min, then removed and dried in a forced-air drying oven at 60 ℃ for 5 min. The dried electrode was then removed and the above steps were repeated to finally obtain the Ti / Fe2O3@Co-MOF composite photoelectrode.
[0061] (iv) Test of photoelectrocatalytic water splitting performance of Ti / Fe2O3@Co-MOF composite photoelectrode (same as Example 1, but the working electrode is changed to the electrode prepared in Example 2)
[0062] Example 3
[0063] (I) Preparation of Ti / Fe2O3 electrode
[0064] (1) The FTO conductive glass was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 30 min in sequence, and then dried in an oven at 60 ℃ for later use.
[0065] (2) Add 0.02 mol of anhydrous ferric chloride and 0.15 mol of sodium nitrate to 100 mL of deionized water and stir until completely dissolved to obtain Fe2O3 reaction precursor solution; then take 15 mL of the mixed solution and dispense it into a 25 mL polytetrafluoroethylene reactor liner, then add 1.5 μL of TiCl4 into the reactor liner and stir until evenly mixed to obtain Ti-doped Fe2O3 reaction precursor solution;
[0066] (3) Place the cleaned FTO conductive glass from step (1) with its conductive surface facing down into the lining of the reactor containing the Ti-doped Fe2O3 reaction precursor solution, seal the hydrothermal reactor, and place it in a forced-air drying oven for hydrothermal reaction at 100 ℃ for 5 h. After the reaction is completed, allow it to cool naturally to room temperature. Open the reactor, remove the FTO conductive glass, rinse the glass surface repeatedly with deionized water, and place it in a forced-air drying oven at 60 ℃ for 1 h to obtain the conductive glass supported on the Ti / FeOOH substrate.
[0067] (4) The conductive glass with Ti / FeOOH substrate obtained in step (3) is placed in a muffle furnace and heated from room temperature to 550 ℃ at a heating rate of 5 ℃ / min, held for 3 h, and then heated from 550 ℃ to 750 ℃ at a heating rate of 10 ℃ / min, and calcined for 20 min to finally obtain Ti / Fe2O3 photoelectrode.
[0068] (II) Preparation of Co-MOF materials (same as Example 1)
[0069] (III) Preparation of Ti / Fe2O3@Co-MOF composite photoelectrode
[0070] The Ti / Fe2O3 photoelectrode was immersed in a 2 mg / mL Co-MOF suspension for 5 min, then removed and dried in a forced-air drying oven at 60 ℃ for 5 min. The dried electrode was then removed and the above steps were repeated to finally obtain the Ti / Fe2O3@Co-MOF composite photoelectrode.
[0071] (iv) Performance test of photoelectrocatalytic water splitting of Ti / Fe2O3@Co-MOF composite photoelectrode (same as Example 1, except that the working electrode is replaced with the electrode prepared in Example 3)
[0072] Comparative Example 1
[0073] A Fe2O3 photoanode is prepared by the following steps: the steps are the same as steps (1) to (4) in Example 2, but TiCl4 is not added.
[0074] Test case
[0075] I. Characterization Analysis
[0076] 1. The Ti / Fe2O3, Ti / Fe2O3@Co-MOF photoanodes prepared in Example 2 and the Fe2O3 photoanode prepared in the comparative example were analyzed by scanning electron microscopy (SEM). The results are shown in the figure. Figure 1 (Where a is Fe2O3, b is Ti / Fe2O3, and c is Ti / Fe2O3@Co-MOF). From Figure 1It can be seen that Fe2O3 grows vertically on FTO to form a nanorod array; after doping with titanium ions, a thin film is formed on the surface of the nanorod array, and further Co-MOF modification will not change the basic morphology of Ti / Fe2O3.
[0077] 2. The Ti / Fe2O3, Ti / Fe2O3@Co-MOF photoanodes prepared in Example 2, and the Fe2O3 photoanode prepared in the comparative example were subjected to crystal structure analysis by X-ray diffraction (XRD). The results are shown in [Figure 1]. Figure 2 .Depend on Figure 2 It can be seen that the XRD patterns of Fe2O3, Ti / Fe2O3, and Ti / Fe2O3@Co-MOF samples have the same crystal structure as hematite (αα-x2O3, JCPDS 33-0664). Titanium doping did not cause a peak shift, and the crystal structure of hematite did not change significantly. This indicates that Ti was doped into the Fe2O3 lattice rather than forming an oxide. The lack of peak shift may also be due to the identical covalent radii (140 pm) of Fe and Ti. No peaks were observed in the Co-MOF layer, which is attributed to the low Co-MOF content.
[0078] 3. The light absorption capacity of the Ti / Fe2O3 and Ti / Fe2O3@Co-MOF photoanodes prepared in Example 2 and the Fe2O3 photoanode prepared in the comparative example was evaluated by ultraviolet-visible diffuse reflectance (UV-vis DRS). The results are shown in [Figure 1]. Figure 3 .Depend on Figure 3 It can be seen that all photoanodes exhibit strong absorption in the 400-600 nm region, with the absorption band edge at 600 nm; through Figure 4 The Kubelka-Munk plot estimated the corresponding band gap values for Fe2O3, Ti / Fe2O3, and Ti / Fe2O3@Co-MOF photoanodes to be 2.03 eV, 1.99 eV, and 1.96 eV, respectively.
[0079] II. Photoelectrochemical Performance Analysis
[0080] 1. The Ti / Fe2O3 and Ti / Fe2O3@Co-MOF photoanodes prepared in Example 2, and the Fe2O3 photoanode prepared in the comparative example, were subjected to PEC performance analysis. The specific method was as follows: a three-electrode system was used for testing, with the photoanode as the working electrode, a Pt sheet as the auxiliary electrode, Ag / AgCl as the reference electrode, and 1 mol / L sodium hydroxide (pH=13.4) as the electrolyte; the light source was configured as simulated AM1.5G sunlight (Beijing Pofila) equipped with a 300W xenon lamp, with a light intensity of 1 solar term (i.e., 100 mW / cm²). -2The test parameters were recorded using a Chenhua CHI660E electrochemical workstation. All measurements were performed with Ag / AgCl as the reference electrode. The final test potential was converted to a reversible standard hydrogen electrode (RHE) according to the formula: E(vs. RHE) = E(vs. Ag / AgCl) + E Ag / AgCl (reference) + 0.0591V × pH.
[0081] 1.1. The linear sweep voltammetry (LSV) curve was measured under AM1.5G illumination at a scan rate of 10 mV / s. The results are shown in [Figure 1]. Figure 5 .
[0082] Depend on Figure 5 It can be seen that the Ti / Fe2O3 and Ti / Fe2O3@Co-MOF photoanodes prepared in Example 2, and the Fe2O3 photoanode prepared in the comparative example, have a current density of 1.55 mA·cm at 1.23 V (vs. RHE). -2 1.8 mA·cm -2 and 0.59 mA·cm -2 The onset potential follows the order Fe₂O₃ (0.83 V) < Ti / Fe₂O₃@Co-MOF (0.86 V) < Ti / Fe₂O₃ (0.967 V). Therefore, the Co-MOF ultrathin layer can negatively change the onset potential by 10⁷ mV. LSV results show that the Co-MOF ultrathin layer, as a co-catalyst, can effectively improve the PEC activity of the photoanode, including the onset potential and photocurrent density.
[0083] 1.2. Photocurrent response analysis was performed using the instantaneous photocurrent (It) curve under optical switching cycles. The results are shown in [Figure Number]. Figure 6 .
[0084] Depend on Figure 6 It can be seen that Fe2O3, Ti / Fe2O3, and Ti / Fe2O3@Co-MOF photoanodes can all reach a stable current within 0.1s, exhibiting excellent photocurrent response characteristics, and the photocurrent density is consistent with... Figure 5 The LSV results are consistent.
[0085] 1.3. Photoelectrochemical characterization was performed using ABPE curves, and the results are shown in [Figure number missing]. Figure 7 .
[0086] Depend on Figure 7It can be seen that the Ti / Fe2O3@Co-MOF photoanode prepared in Example 2 achieved a maximum ABPE value of 0.18% at 1.04 V (vs. RHE). In contrast, the Fe2O3 photoanode prepared in Comparative Example 1 and the Ti / Fe2O3 photoanode prepared in Example 2 have ABPE values of 0.062% at 1.04 V (vs. RHE) and 0.11% at 1.09 V (vs. RHE), respectively, which are both lower than the Ti / Fe2O3@Co-MOF photoanode prepared in this invention.
[0087] 1.4. Photoelectrochemical characterization was performed using IPCE curves, and the results are shown in [Figure number missing]. Figure 8 .
[0088] Depend on Figure 8 It can be seen that the IPCE values of Fe2O3, Ti / Fe2O3 and Ti / Fe2O3@Co-MOF photoanodes at 400 nm are 2.6%, 21% and 38%, respectively, indicating that the superior IPCE of Ti / Fe2O3@Co-MOF photoanode is attributed to titanium ion doping and Co-MOF modification, which improves the charge transfer efficiency at the photoanode / electrolyte interface.
[0089] 1.5. Charge transfer capability was measured by electrochemical impedance spectroscopy (EIS) curves, and the results are shown in [Figure number missing]. Figure 9 .
[0090] Depend on Figure 9 It can be seen that the R of Fe2O3, Ti / Fe2O3 and Ti / Fe2O3@Co-MOF photoanodes ct The values are 1047 Ω, 310 Ω, and 289 Ω, respectively, indicating that the surface state of Fe2O3 after titanium doping and Co-MOF modification is conducive to improving the charge transfer efficiency at the photoanode / electrolyte interface. The faster the carrier transport rate of the electrode material, the lower the recombination rate of photogenerated electrons and holes.
[0091] 1.6 The performance of the photoanode PEC was evaluated using optical stability curves. The results are shown in [Figure number missing]. Figure 10 .
[0092] Depend on Figure 10 It can be seen that after continuous testing at 1.23 V (vs. RHE) for 10 h, the photocurrent density retention rates of Fe2O3, Ti / Fe2O3 and Ti / Fe2O3@Co-MOF photoanodes were 80%, 84% and 95%, respectively, indicating that Ti / Fe2O3@Co-MOF photoanodes have good photochemical stability.
[0093] The above description is only the preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing a Ti / Fe2O3@Co-MOF composite photoelectrode for photoelectrocatalytic water splitting, characterized in that, Includes the following steps: (1) Place the FTO conductive glass in acetone, anhydrous ethanol and deionized water in sequence for ultrasonic cleaning for 5-40 min, and then place it in an oven at 40~90 ℃ to dry for later use. (2) Add anhydrous ferric chloride and sodium nitrate to deionized water and stir until completely dissolved to obtain a mixed solution, thus obtaining the Fe2O3 reaction precursor solution; (3) Add titanium source to the mixed solution in step (2) and stir until the mixture is uniform to obtain Ti-doped Fe2O3 reaction precursor solution; (4) Place the cleaned FTO conductive glass in step (1) with the conductive surface facing down in the lining of the reactor, add the reaction precursor liquid prepared in step (3) into the reactor, seal the hydrothermal reactor, put it into the drying oven for hydrothermal reaction, and cool it naturally to room temperature after the reaction is completed. (5) Open the reactor, take out the FTO conductive glass, rinse the glass surface repeatedly with deionized water, and put it in a forced-air drying oven at 40~90 ℃ for 1~3 h to obtain the Ti / FeOOH substrate conductive glass; (6) The conductive glass on the Ti / FeOOH substrate obtained in step (5) is placed in a muffle furnace and calcined at high temperature to obtain a Ti / Fe2O3 photoelectrode; (7) Dissolve cobalt chloride hexahydrate and 2-mercaptoisonicotinic acid in a mixed solvent of 15-30 mL deionized water and acetonitrile. Seal the mixed solution in a polytetrafluoroethylene reactor for hydrothermal reaction. Cool to room temperature and let stand for a certain time to obtain orange crystals. Grind the orange crystals into fine powder. Then take an appropriate amount of fine powder and add anhydrous ethanol. Ultrasonic treatment for 30-90 min is used to prepare Co-MOF suspension. (8) Immerse the Ti / Fe2O3 photoelectrode in the Co-MOF suspension in step (7), let it stand, then take it out and dry it in a forced-air drying oven at 40~80 ℃ for 5~20 min to finally obtain the Ti / Fe2O3@Co-MOF composite photoelectrode.
2. The preparation method according to claim 1, characterized in that, In the Fe2O3 reaction precursor solution obtained in step (2), the concentration of anhydrous ferric chloride is 0.01~0.3 mol / L and the concentration of sodium nitrate is 0.5~2 mol / L.
3. The preparation method according to claim 1, characterized in that, The titanium source mentioned in step (3) is TiCl4, and its amount is 0.2~6.5 μL.
4. The preparation method according to claim 1, characterized in that, In step (4), the amount of precursor solution used is 5~20mL; the hydrothermal reaction temperature is 90~150℃, and the reaction time is 2~10h.
5. The preparation method according to claim 1, characterized in that, The high-temperature calcination process described in step (6) is a step-by-step calcination. First, the temperature is raised from room temperature to 400-600 ℃ at a heating rate of 2-10 ℃ / min and calcined for 1-2 h. Then, the temperature is raised to 700-800 ℃ at a heating rate of 5-15 ℃ / min and calcined for 10-20 min.
6. The preparation method according to claim 1, characterized in that, In the mixed solution prepared in step (7), the mass of cobalt chloride hexahydrate is 0.1~0.4 mmol, the mass of 2-mercaptoisonicotinic acid is 0.2~0.6 mmol, the hydrothermal reaction temperature is 130~180℃, the reaction time is 1~5 days, and the standing time is 1~3 days.
7. The preparation method according to claim 1, characterized in that, The concentration of the Co-MOF suspension mentioned in step (8) is 0.2~3 mg / mL.
8. The preparation method according to claim 1, characterized in that, The immersion method described in step (8) is as follows: first, immerse the Ti / Fe2O3 photoelectrode in Co-MOF suspension for 3~12 min, then dry it at 60~80 ℃ for 5~20 min, and then repeat the above steps 1~6 times after drying.
Citation Information
Patent Citations
Fe2-xTixO3 / FTO photo-anode preparing technology and treatment method capable of improving photocurrent density of photo-anode