Preparation method of Fe3O4@C composite material derived from multi-sized octahedral MIL-88B (Fe)

Multi-sized octahedral MIL-88B(Fe) is prepared by solvothermal method and carbonized and graphitized to form Fe3O4@C composite material, which solves the problems of single size and small specific surface area of ​​the material in the existing technology, and achieves efficient removal of heavy metal ions. effect.

CN116726882BActive Publication Date: 2024-10-22TIANJIN RIGGS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310635343.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-10-22
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

It is difficult to prepare multi-sized octahedral MIL-88B (Fe) materials with existing technology, and its specific surface area is small, the preparation process is complex, and heavy metal ions cannot be effectively removed.

Method used

Multi-size octahedral MIL-88B(Fe) was prepared by solvothermal method, and carbonized and graphitized under N2 to form Fe3O4@C composite material, retaining the morphology and mesoporous structure of the original material, increasing the specific surface area, Paramagnetic for efficient separation.

Benefits of technology

It achieves the efficient removal of adsorbed heavy metal ion Pb2+, has good material stability and low separation energy consumption, and has great application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116726882B_ABST
    Figure CN116726882B_ABST
Patent Text Reader

Abstract

The invention discloses a Fe3O4@C composite material derived from multi-sized octahedral MIL-88B(Fe) and a preparation method thereof. First, the multi-sized octahedral MIL-88B(Fe) is obtained by changing the concentration of metal salt and organic ligand and the filling degree of solution; then, the multi-sized octahedral MIL-88B(Fe) is used as a precursor and calcined in a N2 step to obtain a magnetic Fe3O4 composite material wrapped in mesoporous carbon. The composite material retains the morphology of the precursor, and the preparation method is simple, green and environmentally friendly, and low in cost. The Fe3O4@C composite material prepared by the method disclosed in the invention has good stability, a mesoporous structure, a large specific surface area, and paramagnetism. It can be used as an adsorbent material in the field of heavy metal ion removal, with high removal efficiency and low energy consumption, and has certain practical application potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal organic framework compound MOF materials, in particular to a method for preparing a Fe3O4@C composite material derived from multi-sized octahedral MIL-88B (Fe). Background Art

[0002] With the rapid development of my country's industry, heavy metal wastewater generated in the production process of mining, machinery manufacturing, chemical industry and other industries has become one of the most serious water pollution and ecologically harmful industrial wastewaters. Heavy metal ions in wastewater cannot be decomposed and destroyed by common water treatment methods, and they cannot be biodegraded after entering the environment. They can only participate in the food chain cycle and accumulate in organisms by changing their physical and chemical states or being transferred and diluted, eventually destroying the normal physiological metabolic activities of organisms and endangering human health.

[0003] The methods commonly used for heavy metal wastewater treatment mainly include chemical method, ion exchange method, electrolysis method, adsorption method, etc. Among them, the adsorption method has the advantages of easy operation and high efficiency, but at the same time there are bottleneck problems such as high treatment cost and difficult separation of adsorbent materials. Therefore, it is urgent to find a new adsorbent material that is simple to synthesize, green, efficient and easy to separate for the adsorption of Pb in wastewater. 2+ And other heavy metal ions.

[0004] The currently reported synthesis methods of MIL-88B(Fe) include hydrothermal, solvent thermal, and oil bath. The resulting morphologies are mostly regular octahedrons or spindles. They have a single size and cannot have multiple scales at the same time. They lack nanoscale sizes of around 100 nm, have a small specific surface area, and have a complicated preparation process. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a Fe3O4@C composite material derived from multi-sized octahedral MIL-88B (Fe). The material retains the basic morphology of the original MIL-88B (Fe) material, has good stability, a mesoporous structure, a large specific surface area, and paramagnetism, and can be used as an adsorption material in the field of heavy metal ion removal.

[0006] The technical solution adopted by the present invention to solve the technical problem is:

[0007] The first aspect of the present invention provides a method for preparing a Fe3O4@C composite material derived from a multi-sized octahedral MIL-88B (Fe), the preparation method comprising the following steps:

[0008] (1) dissolving ferric chloride hexahydrate in N,N-dimethylformamide solvent, and stirring magnetically until the solution is uniform and transparent, thereby obtaining solution A, wherein the concentration of ferric chloride hexahydrate in solution A is 0.092 to 0.138 mol / L; dissolving terephthalic acid in N,N-dimethylformamide solvent, and stirring magnetically until the solution is uniform and transparent, thereby obtaining solution B;

[0009] (2) adding solution A dropwise into solution B while continuously stirring under magnetic stirring, wherein the molar ratio of ferric chloride hexahydrate to terephthalic acid is 1-2:1-2, and after complete addition, continuing magnetic stirring until the solution is uniform, thereby obtaining solution C;

[0010] (3) Solvent thermal reaction of solution C, after the reaction, centrifugation to separate the solid, washing and drying to obtain a pink powder, i.e., MIL-88B (Fe);

[0011] (4) Using the MIL-88B(Fe) prepared in step (3) as a precursor, calcining under N2 to undergo carbonization and graphitization, ultimately obtaining a multi-sized octahedral MIL-88B(Fe)-derived Fe3O4@C composite material.

[0012] The organic ligand terephthalic acid is used as a carbon source to carbonize to form amorphous carbon, Fe 3+ It is reduced and combines with the oxygen element in the organic ligand to form Fe3O4, and then part of the amorphous carbon undergoes graphitization under the catalytic action of Fe3O4.

[0013] Furthermore, the concentration of the ferric chloride hexahydrate in step (1) is 0.092-0.11 mol / L

[0014] Furthermore, in step (2), the molar ratio of ferric chloride hexahydrate to terephthalic acid is 1-1.5:1-1.5.

[0015] Furthermore, in step (2), after the solution A is added dropwise to the solution B, the magnetic stirring is continued for 30 to 40 minutes.

[0016] Furthermore, the solvent thermal reaction temperature in step (3) is 100-120°C, and the reaction time is 20-30 hours. More preferably, the reaction temperature is 105-115°C, and the reaction time is 23-25 ​​hours.

[0017] Furthermore, after the solvothermal reaction in step (3), the centrifugal speed is 2000-5000 r / min, and the product is washed with DMF and anhydrous ethanol 2-3 times respectively.

[0018] Furthermore, the drying in step (3) is vacuum drying, the drying temperature is 50-70°C, and the drying time is 12-24 hours. More preferably, the drying temperature is 55-65°C, and the drying time is 16-20 hours.

[0019] Furthermore, the calcination in step (4) is carried out in a quartz tube furnace, the heating rate during calcination is 2-10°C / min, the calcination temperature is 700-900°C, and the time is 0.5-2h. Further preferably, the heating rate is 4-8°C / min, the calcination temperature is 700-800°C, and the calcination time is 0.5-1h.

[0020] The second aspect of the present invention is to provide a multi-sized octahedral MIL-88B (Fe)-derived Fe3O4@C composite material prepared by the above method, the size of which is shrunk compared to the precursor MIL-88B (Fe), but the overall shape is still octahedral, with an edge length in the range of 40 to 900 nm, and the main size is concentrated in the range of 400 to 700 nm.

[0021] The third aspect of the present invention is to provide the above composite material for adsorbing heavy metal ions Pb in the comprehensive wastewater of garbage power plant 2+ Application as adsorbent.

[0022] The present invention uses a multi-sized octahedral MIL-88B (Fe) prepared by a solvothermal method, and a MIL-88B (Fe)-derived Fe3O4@C composite material prepared by calcining (carbonization, graphitization) in a N2 step. It is mainly Fe3O4, and a layer of porous carbon mixed with amorphous carbon and graphite carbon is coated on the surface. This coating structure retains the basic morphology of the original MIL-88B (Fe) material, has a mesoporous structure, and has the characteristics of a large specific surface area; it has superparamagnetism, and can achieve efficient separation of adsorption materials under the action of an external magnetic field, greatly reducing separation energy consumption, and can be used as an adsorption material to achieve heavy metal ions Pb in the comprehensive wastewater of garbage power plants. 2+ Rapid removal has great application potential.

[0023] The advantages and positive effects of the present invention are:

[0024] The present invention obtains multi-sized octahedron MIL-88B (Fe) by setting the concentration of metal salt and organic ligand and the filling degree of solution; then it is used as a precursor and calcined in N2 in one step to obtain a magnetic Fe3O4 composite material wrapped by mesoporous carbon. The small size effect of nano-scale materials is conducive to increasing the specific surface area of ​​the material and promoting the full contact between the material and the comprehensive wastewater of the garbage power plant. The large-sized octahedron of micron size can provide more pores to adsorb heavy metal ions. In summary, multi-sized particles cooperate with each other and can greatly promote the adsorption of heavy metal ions in the comprehensive wastewater of the garbage power plant by the material. The composite material retains the morphology of the precursor, and the preparation method is simple, green and environmentally friendly, and low in cost. The Fe3O4@C composite material prepared by the method disclosed in the present invention has good stability, a mesoporous structure, a large specific surface, and paramagnetism. It can be used as an adsorption material in the field of heavy metal ion removal, with high removal efficiency and low energy consumption, and has certain practical application potential. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a low-resolution SEM image of MIL-88B (Fe) prepared in Example 1 of the present invention;

[0026] Figure 2 This is a high-resolution SEM image of MIL-88B (Fe) prepared in Example 1 of the present invention;

[0027] Figure 3 This is a SEM image of MIL-88B (Fe) prepared in Comparative Example 1 of the present invention;

[0028] Figure 4 This is the XRD pattern of Fe3O4@C prepared in Example 1 of the present invention;

[0029] Figure 5 This is a N2 adsorption-desorption isotherm curve of Fe3O4@C prepared in Example 1 of the present invention;

[0030] Figure 6 This is a pore size distribution diagram of Fe3O4@C prepared in Example 1 of the present invention;

[0031] Figure 7 This is a graph showing the adsorption capacity of Fe3O4@C prepared in Example 1 of the present invention at different pH values;

[0032] Figure 8 This is a graph showing the removal rate of Fe3O4@C obtained in Example 1 of the present invention after five cycles at pH=5;

[0033] Fig. 9 This is a graph of the adsorption capacity of Fe3O4@C prepared in Example 2 of the present invention at different pH values;

[0034] Fig.10This is a graph showing the removal rate of Fe3O4@C obtained in Example 2 of the present invention after five cycles at pH=6;

[0035] Fig.11 This is a graph showing the adsorption capacity of Fe3O4@C prepared in Example 3 of the present invention at different pH values;

[0036] Fig.12 This is a graph showing the removal rate of Fe3O4@C obtained in Example 3 of the present invention after five cycles at pH=5;

[0037] Fig.13 This is a graph of the adsorption capacity of Fe3O4@C prepared in Comparative Example 1 of the present invention at different pH values;

[0038] Fig.14 This is a graph of the adsorption capacity of Fe3O4@C prepared in Comparative Example 2 of the present invention at different pH values;

[0039] Fig.15 This is a graph showing the removal rate of Fe3O4@C obtained in Comparative Example 2 of the present invention after five cycles at pH=5;

[0040] Fig.16 This is a graph of the adsorption capacity of Fe3O4@C prepared in Comparative Example 3 of the present invention at different pH values;

[0041] Fig.17 This is a graph showing the removal rate of Fe3O4@C obtained in Comparative Example 3 of the present invention after five cycles at pH=5; DETAILED DESCRIPTION

[0042] The present invention is further described in detail below through specific examples. The following examples are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.

[0043] In the following examples, all reagents used were of analytical grade and commercially available chemical reagents unless otherwise specified.

[0044] Filling degree refers to the percentage of total solvent volume to the total volume of the solvothermal reactor.

[0045] Example 1

[0046] A method for preparing a Fe3O4@C composite material derived from multi-sized octahedral MIL-88B (Fe), comprising the following steps:

[0047] 1) Weigh 622 mg (2.3 mmol) of ferric chloride hexahydrate, dissolve it in 25 mL of DMF solvent, and stir it evenly with a magnetic force to obtain solution A; weigh 382 mg (2.3 mmol) of terephthalic acid, dissolve it in 25 mL of DMF solvent, and stir it evenly with a magnetic force to obtain solution B, with a filling degree of 50%;

[0048] 2) Add solution A dropwise into solution B during continuous ultrasonication, and continue magnetic stirring for 30 minutes after complete addition until uniform, to obtain solution C;

[0049] 3) The mixed solution C was transferred to a 100 mL polytetrafluoroethylene-lined stainless steel reactor, sealed, and subjected to solvent thermal reaction at 110° C. in a forced air drying oven for 24 h. After the reaction was completed, it was naturally cooled to room temperature, washed by centrifugation with DMF and anhydrous ethanol for 3 times, and finally dried in a vacuum drying oven at 60° C. for 10 h to obtain the final product MIL-88B(Fe);

[0050] 4) Take 200 mg of the obtained MIL-88B(Fe) pink powder and spread it evenly in a porcelain boat, place it in a tube furnace, and heat it from room temperature to 700°C under N2 atmosphere at a heating rate of 5°C / min. Keep it at 700°C for 0.5 h, and then cool it naturally to room temperature. The obtained black powder is the Fe3O4@C composite material derived from MIL-88B(Fe).

[0051] The low-resolution SEM results of the precursor MIL-88B (Fe) prepared in step 3) of this embodiment are as follows: Figure 1 As shown, the morphology is regular, all are regular octahedrons, and the side lengths are in the range of 50 to 1500 nm, with the main dimensions concentrated in the range of 700 to 1300 nm.

[0052] The high-resolution SEM results of the precursor MIL-88B (Fe) prepared in step 3) of this embodiment are as follows Figure 2 As shown, octahedral particles within 100 nm can be clearly seen.

[0053] The XRD results of the Fe3O4@C composite material prepared in step 4) of this embodiment are as follows Figure 4 The diffraction peaks in the figure can be attributed to Fe3O4 (JCPDS#88-0315) and graphite carbon (JCPDS#34-0567), respectively, indicating that the prepared MIL-88B(Fe) derivative is a Fe3O4@C composite material.

[0054] The N2 adsorption-desorption isotherm curve of the Fe3O4@C composite material prepared in step 4) of this embodiment is as follows Figure 5 As shown in the figure, this curve is the characteristic curve of a typical type IV mesoporous material, and the BET specific surface area is calculated to be 295 m 2 / g.

[0055] The pore size distribution results of the Fe3O4@C composite material prepared in step 4) of this embodiment are as follows Figure 6As shown in the figure, the extreme peak at 3.8nm is a false peak caused by the hysteresis loop of the desorption curve. The real pore size of the material is mostly concentrated at 6.9nm, proving that the Fe3O4@C composite material is a typical mesoporous material.

[0056] Fe3O4@C composite materials for adsorption of heavy metal ions Pb 2+ The application of the field includes the following steps:

[0057] Add 10 mL of waste-to-energy plant wastewater (COD Cr ≤170mg / L; SS≤480mg / L; pH 6.5~8.5; Cl - Concentration ≤330mg / L; Pb 2+ Concentration ≤110mg / L), use 0.1M NaOH or HCl solution to adjust Pb 2+ The initial pH of the solution was 1, 3, 5, 7, 9, 11 and 13, 1 g / L Fe3O4@C was added as adsorbent, mechanically stirred at room temperature for 30 min, centrifuged at 2000 r / min for 10 min (or under the action of an external magnetic field), the supernatant was taken and appropriately diluted, and the residual heavy metal ion concentration in the solution was determined by atomic absorption spectrophotometer. The results are shown in Figure 7 As shown, the prepared Fe3O4@C can be effectively adsorbed in a wide pH range.

[0058] According to the above experimental method, after the adsorption experiment is completed, the solid adsorbent is separated and desorbed with 0.1 mol / L HCl solution for 2 hours, washed with ultrapure water for 3 times, and then fully dried. Under the condition of pH = 5, the adsorbent is tested for recycling according to the above experimental method. The results are as follows Figure 8 As shown. Heavy metal ion Pb after 5 cycles of adsorbent 2+ The removal rate remains above 99%.

[0059] Example 2

[0060] The preparation method is the same as that of Example 1, except that the concentration of ferric chloride hexahydrate is 0.11 mol / L and the calcination (carbonization, graphitization) temperature is 900°C. 2+ Pollutant adsorption is effective over a wide pH range (e.g. Fig. 9 ), and the adsorbent can be recycled for many times. After 5 cycles, the adsorbent can absorb heavy metal ions Pb at pH = 6. 2+ The removal rate is still higher than 90% (such as Fig.10 ).

[0061] Example 3

[0062] The preparation method is the same as that of Example 1, except that the calcination (carbonization, graphitization) time is 1 h. 2+ Pollutant adsorption is effective over a wide pH range (e.g. Fig.11 ), and the heavy metal ion Pb after 5 cycles under pH=5 2+ The removal rate is still higher than 89% (such as Fig.12 ).

[0063] Comparative Example 1

[0064] The preparation method is the same as that of Example 1, except that the concentration of ferric chloride hexahydrate is 0.023 mol / L and the filling degree is 20%. The precursor MIL-88B (Fe) prepared in this comparative example has an octahedral shape and a size of about 1200 nm (such as Figure 3 ). According to the above adsorption experimental method, the prepared Fe3O4@C was subjected to adsorption of Pb 2+ The adsorption efficiency of pollutants is less than 60% (such as Fig.13 ).

[0065] Comparative Example 2

[0066] The preparation method is the same as that of Example 1, except that the calcination temperature is 600°C. According to the above adsorption experimental method, the prepared Fe3O4@C is subjected to adsorption of Pb 2+ Low adsorption efficiency of pollutants (such as Fig.14 ) and the heavy metal ion Pb after 5 cycles under pH = 7 2+ Poor removal effect and recyclability (such as Fig.15 ).

[0067] Comparative Example 3

[0068] The preparation method is the same as that of Example 1, except that the calcination time is 3 h. According to the above adsorption experimental method, the prepared Fe3O4@C is subjected to adsorption of Pb in a wide pH range. 2+ Low adsorption efficiency of pollutants (such as Fig.16 ) and the heavy metal ion Pb after 5 cycles under pH = 7 2+ Poor removal effect and recyclability (such as Fig.17 ).

[0069] The above description is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several modifications and improvements without departing from the inventive concept, which all belong to the protection scope of the present invention.

Claims

1. A method for adsorbing heavy metal ions Pb in comprehensive wastewater from garbage power plants 2+ A method for preparing a Fe3O4@C composite material derived from multi-sized octahedral MIL-88B (Fe), characterized in that: The following steps are involved: (1) dissolving ferric chloride hexahydrate in N,N-dimethylformamide solvent, and stirring magnetically until the solution is uniform and transparent, thereby obtaining solution A, wherein the concentration of ferric chloride hexahydrate is 0.092 to 0.138 mol / L; dissolving terephthalic acid in N,N-dimethylformamide solvent, and stirring magnetically until the solution is uniform and transparent, thereby obtaining solution B; (2) adding solution A dropwise into solution B while continuously stirring under magnetic stirring, wherein the molar ratio of ferric chloride hexahydrate to terephthalic acid is 1-2:1-2, and after complete addition, continuing magnetic stirring until the solution is uniform, thereby obtaining solution C; (3) Solvent thermal reaction of solution C, after the reaction is completed, the solid is separated by centrifugation, washed and dried to obtain a pink powder, namely MIL-88B (Fe), the solvent thermal reaction temperature is 100-120°C, and the reaction time is 20-30h; (4) using the MIL-88B(Fe) obtained in step (3) as a precursor, calcining under N2 to undergo carbonization and graphitization, and finally obtaining a multi-sized octahedral MIL-88B(Fe)-derived Fe3O4@C composite material, wherein the calcination is carried out in a quartz tube furnace, the heating rate during calcination is 2 to 10°C / min, the calcination temperature is 700 to 900°C, and the time is 0.5 to 2h; The obtained multi-sized octahedral MIL-88B (Fe) derived Fe3O4@C composite material is octahedral in shape, with a side length of 40 to 900 nm and a size concentrated in the range of 400 to 700 nm. The small size effect of nano-scale materials is beneficial to increasing the specific surface area of ​​the material and promoting full contact between the material and the comprehensive wastewater of the garbage power plant. The large-sized octahedron at the micron level can provide more pores to adsorb heavy metal ions. The multi-sized particles work together to greatly promote the material's adsorption of heavy metal ions in the comprehensive wastewater of the garbage power plant.

2. The preparation method according to claim 1, characterized in that: The concentration of ferric chloride hexahydrate is 0.092-0.11 mol / L.

3. The preparation method according to claim 1, characterized in that: The molar ratio of ferric chloride hexahydrate to terephthalic acid is 1-1.5:1-1.

5.

4. The preparation method according to claim 1, characterized in that: The drying in step (3) is vacuum drying, the drying temperature is 50 to 70° C., and the drying time is 12 to 24 hours.