A nanosheet-assembled micron-spherical monoclinic BiVO prepared by microwave irradiation 4 Materials and preparation methods

The preparation of nanosheets through microwave radiation method assembled microspherical single-climbed phase BiVO4 material is solved, and the problems of high temperature, high pressure and secondary pollution in the preparation of traditional BiVO4 materials are achieved, efficient and environmentally friendly photocatalytic material preparation is achieved, and photocatalytic activity and application are improved. potential.

CN116730386BActive Publication Date: 2024-11-01XIJING UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310002308.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-03
Publication Date
2024-11-01
Estimated Expiration
2043-01-03

AI Technical Summary

Technical Problem

Traditional photocatalytic materials such as TiO2, SnO2 and ZnO have a wide bandwidth, resulting in low solar light utilization, which limits the photocatalytic performance. In addition, the existing BiVO4 material preparation methods require high temperature, high pressure, time-consuming, complex operation and two types of production. Second pollution.

Method used

The nanosheets were prepared by microwave radiation method assembled with microspherical monoclinic phase BiVO4 material, using analytical pure Bi(NO3)3·5H2O and NH4VO3 as raw materials, and cetyl trimethyl ammonium bromide (CTAB) as surfactant. Microwave reaction preparation avoids high temperature and high pressure and acid-base regulation, achieving low energy consumption and simple process operations.

Benefits of technology

The prepared BiVO4 material has good crystallinity, morphological uniformity and large specific surface area, which improves photocatalytic activity, solves the problems of high energy consumption, complex process and pollution in traditional methods, and has a wide range of application prospects in pollutants. Governance and energy conversion fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004034420610000011
    Figure HDA0004034420610000011
  • Figure HDA0004034420610000012
    Figure HDA0004034420610000012
  • Figure HDA0004034420610000021
    Figure HDA0004034420610000021
Patent Text Reader

Abstract

The invention discloses a nanosheet-assembled micron-spherical monoclinic BiVO4 material prepared by a microwave radiation method and a preparation method thereof. The method comprises the following steps: adding analytically pure Bi(NO3)3·5H2O and cetyltrimethylammonium bromide (CTAB) to dissolve in distilled water, stirring and placing in a normal-pressure microwave reactor with a reflux condenser, mixing at a temperature of 85-120 DEG C to obtain solution A; dissolving NH4VO3 in distilled water, stirring until completely dissolved to obtain solution B; adding solution A dropwise into a flask containing solution B under vigorous stirring to obtain solution C; placing solution C in a normal-pressure microwave reactor with a reflux condenser, and reacting at a reaction temperature of 80-120 DEG C by a microwave radiation method to obtain a solid-liquid mixed suspension sample; centrifuging, washing and drying the sample to obtain a micron-spherical monoclinic BiVO4 material assembled by nanosheets; the method has the advantages of simple process operation, fast reaction and short cycle, controllable morphology, energy saving and the like, and the obtained product has uniform morphology and size distribution and high purity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of photocatalytic materials, and in particular to a nanosheet-assembled micron-spherical monoclinic BiVO4 material prepared by a microwave radiation method and a preparation method thereof. Background Art

[0002] Due to the rapid development of industry and agriculture, environmental pollution represented by water pollution and air pollution is particularly prominent. Traditional sewage treatment methods have problems such as high cost, incomplete treatment, and secondary pollution. Semiconductor photocatalytic technology can be used as a new type of environmental pollution control technology because it can directly utilize solar energy and has distinctive characteristics such as environmentally friendly and efficient processes. Photocatalytic technology is based on the energy band theory. When solar energy is irradiated on the semiconductor catalyst, the photocatalyst is excited to produce holes with strong oxidation ability, which can completely decompose the difficult-to-degrade organic pollutants. Therefore, the development of semiconductor photocatalytic technology provides a feasible way for the deep treatment of pollutants in water bodies and the alleviation of current environmental pollution problems; and research has confirmed that photocatalytic technology has broad application prospects in the field of organic pollutant treatment (Xue W, Zhangg, Xu X, et al. Preparation of titania nanotubes doped With cerium and their photocatalytic activity for glyphosate [J]. Chemical Engineering Journal, 2011, 167 (1): 397-402; Chen X, Liu F, Liu B, et al. A novel route to graphite-like carbon supporting SnO2 With high electron transfer and photocatalytic activity [J]. Journal of Hazardous Materials, 2015, 287: 126-132).

[0003] However, the traditional photocatalytic materials represented by TiO2, SnO2 and ZnO have a relatively wide band gap and extremely low utilization rate of sunlight, which affects the photocatalytic performance and limits the development of photocatalytic technology. BiVO4 material is widely used to replace yellow pigments containing toxic heavy metals in the early days because of its non-toxic, bright color, environmental friendliness and stability. In recent years, with the needs of the field of photocatalytic technology, BiVO4 has attracted widespread attention as a photocatalytic material in the degradation of pollutants and decomposition of water due to its narrow band gap of about 2.4eV (Tong H, Ouyang S, Bi Y, et al. Nano-photocatalytic materials: possibilities and challenges [J]. Advanced Materials, 2012, 24 (2): 229-251). BiVO4 has three main crystal structures, namely tetragonal scheelite type, tetragonal zircon type and monoclinic scheelite type. Among them, the bandgap widths of tetragonal and monoclinic scheelite are both about 2.4eV, and that of tetragonal zircon is 2.9eV. Monoclinic and tetragonal scheelite have very similar structures, that is, each BiO8 dodecahedron is surrounded by 8 VO4 tetrahedra, and each O atom connects 2 Bi centers and one V center. But the difference is that the space around Bi and V ions in monoclinic scheelite is more distorted, which increases the local polarization and is conducive to the separation of electron-hole pairs. Therefore, under the same bandgap width, monoclinic BiVO4 has higher catalytic activity (Xie Mingzheng. Modification mechanism and pollutant degradation efficiency of TiO2 and BiVO4-based visible light catalysts [D]. Harbin Institute of Technology, 2015).

[0004] At present, the preparation methods of bismuth vanadate photocatalysts mainly include precipitation method, solid phase method, hydrothermal method, sol-gel method, electrospinning method, etc. However, most of these methods require high temperature, high pressure, and time-consuming reaction conditions, have high requirements for equipment, cumbersome operation, high energy consumption, or have problems such as a large amount of secondary pollution during the reaction, uneven product particle size, and difficult to control morphology. Summary of the invention

[0005] The present invention aims to provide a nanosheet-assembled micron-spherical monoclinic BiVO4 material prepared by a microwave radiation method with low energy consumption, simple process operation and mild preparation reaction conditions, and a preparation method thereof.

[0006] The present invention is implemented by the following scheme:

[0007] A method for assembling micron-spherical monoclinic BiVO4 materials using nanosheets prepared by microwave radiation, comprising the following steps:

[0008] First, weigh 2.0615g analytical pure Bi(NO3)3·5H2O and 0.7745g hexadecyltrimethylammonium bromide (CTAB) and place them in a 250mL beaker, add 115mL distilled water and stir them evenly with magnetic force, then place them in a microwave reactor, set the heating power to 500-2000W, the frequency to 2450MHz, the heating temperature to 80-120℃, mix and stir for 60min to obtain a mixed solution A;

[0009] Second, weigh 0.7457 g NH4VO3 into a 100 mL beaker, add 85 mL distilled water and stir evenly with magnetic force to obtain a homogeneous aqueous solution B;

[0010] Third, the solution B prepared in the second step was transferred to a 500 mL quartz round-bottom flask, and the solution A obtained in the first step was added dropwise to the 500 mL quartz round-bottom flask containing the mixed solution B under vigorous stirring. After the addition was completed, the mixture was stirred continuously to obtain a mixed solution C.

[0011] Fourth, the solution C prepared in the third step is placed in a microwave reactor with a normal pressure reflux cooling device, and the heating power is set to 200-2000 W and the frequency is set to 2450 MHz; the heating temperature is set to 80-120° C. and the reaction time is set to 150 min;

[0012] Fifth, after the reaction is completed, wait for the product in the quartz round-bottom flask to cool to room temperature, transfer the product to a centrifuge, remove the supernatant and take out the lower layer sample, wash it with distilled water and ethanol for many times, and dry it to obtain the nanosheet-assembled micron-spherical monoclinic BiVO4 material.

[0013] Furthermore, in the first step and the second step, the magnetic stirring speed is 800 rpm and the stirring time is 15 min.

[0014] Furthermore, in the fifth step, after centrifugation at 5000 rpm for 2 minutes, the supernatant was removed and the lower layer sample was taken out.

[0015] Furthermore, in the fifth step, the solid sample is washed with distilled water for 3 to 5 times, and then washed with ethanol for 3 to 5 times, and then the washed product is placed in an oven and dried at 70° C. for 24 hours to obtain the target BiVO4 material.

[0016] The invention discloses a nanosheet-assembled micron-spherical monoclinic BiVO4 material, which is assembled from nanosheets into micron-spherical BiVO4, wherein the thickness of the nanosheets is 11.74-35.25 nm, and the diameter of the micron-sphere is 1.24-1.34 μm.

[0017] A nanosheet-assembled micron-spherical monoclinic BiVO4 material, the product space group is I2 / a, and the unit cell parameters are and α=γ=90.0° and β=90.38°, the strongest peak corresponds to the hkl crystal plane index

[0018] Compared with the prior art, the present invention has the following beneficial technical effects:

[0019] The present invention uses analytically pure Bi(NO3)3·5H2O and NH4VO3 as reaction raw materials, distilled water as solvent, and cetyltrimethylammonium bromide (CTAB) as surfactant, and adopts microwave radiation technology to prepare micron-spherical monoclinic BiVO4 material assembled by nanosheets;

[0020] The monoclinic BiVO4 material prepared by the present invention is found through X-ray diffraction results and scanning electron microscope images that the product is a micron-spherical monoclinic BiVO4 with good crystallinity and assembled by nanosheets. The sample has good crystallinity, uniform morphology and size, uniform distribution and a large specific surface area; it has high photocatalytic activity and has important research significance and commercial potential in improving the efficiency of photocatalytic materials.

[0021] The microwave radiation method adopted in the present invention has a preparation process that does not require the use of acid or alkali for pH adjustment, does not require a high-temperature and high-pressure hydrothermal reactor, is simple to operate, does not require high temperature, has mild and controllable reaction conditions, a short time cycle, low cost, rapid controllability, and is green and energy-saving, thereby solving the problems of complex process, long time consumption, and high energy consumption under high temperature reaction caused by the need to use acid and alkali for pH adjustment in the preparation process of monoclinic BiVO4.

[0022] The monoclinic BiVO4 prepared by the present invention is a new type of n-type semiconductor material with narrow band gap, green and non-toxic, and high activity photocatalytic performance with visible light response. It is widely used in the fields of degradation of organic pollutants, decomposition of water to produce hydrogen, disinfection and sterilization; this method is expected to promote the research progress of monoclinic BiVO4 as a photocatalytic material in the fields of pollutant control and energy conversion.

[0023] The synthesis process mechanism of the method of the present invention is as follows: microwave radiation heating is different from the traditional heating method from the outside to the inside. It is a thermal effect caused by dielectric heating caused by the medium under the action of the electromagnetic field. It has a fast heating speed, simple operation and high efficiency. CTAB is a cationic surfactant that can dissociate into C with a hydrophobic group in water. 19 H 42 N + Cations can affect the growth process and structure of BiVO4 through electrostatic and steric effects. 19 H 42 N + The cations easily interact with the VO4 on the surface of the BiVO4 nucleus. 3-Anions attract each other and adhere to the crystal surface to form an ordered hydrophobic film, thereby controlling the growth rate of specific adsorption crystal faces. Therefore, the addition of CTAB will lead to changes in the kinetic deposition process during the growth of the crystal nucleus, promoting the anisotropy of the crystal nucleus growth. Therefore, under the action of microwave radiation, under the experimental parameters such as the specific surfactant CTAB and the concentration of the reactants, temperature, and reaction time, the method of the present invention can efficiently and controllably synthesize nanosheets to assemble micron-spherical monoclinic BiVO4 materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is the X-ray diffraction (XRD) pattern of BiVO4 sample;

[0025] Figure 2 The crystal structure diagram of BiVO4 sample;

[0026] Figure 3 This is a 100k-fold scanning electron microscope (SEM) image of the BiVO4 sample;

[0027] Figure 4 50k times scanning electron microscope (SEM) image of BiVO4 sample;

[0028] Figure 5 25k times scanning electron microscope (SEM) image of BiVO4 sample;

[0029] Figure 6 Schematic diagram of the morphology of BiVO4 sample. DETAILED DESCRIPTION

[0030] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.

[0031] Example 1 Preparation of BiVO4 Sample 1 Using Microwave Radiation Technology

[0032] At room temperature, 2.0615 g of analytical pure Bi(NO3)3·5H2O and 0.7745 g of hexadecyltrimethylammonium bromide (CATB) were weighed and placed in a 250 mL beaker, and 115 mL of distilled water was added. The beaker was placed on a magnetic stirrer at a speed of 800 rpm and stirred at a constant speed for 15 min. After stirring, it was transferred to a 250 mL round-bottom flask and placed in a microwave reactor with a normal pressure reflux cooling device. The model of the microwave reactor was "Midea PJ21C-AU", with a heating power of 1000 W and a frequency of 2450 MHz. The heating temperature was set to 100 ° C. After mixing for 60 min, a mixed solution A was obtained; then, 0.7457 g of NH4VO3 was placed in a 100mL beaker, 85mL of distilled water was added thereto, and the beaker was placed on a magnetic stirrer at a speed of 800rpm and stirred at a uniform speed for 15min to obtain a homogeneous aqueous solution B; then, the mixed solution B was transferred to a 500mL quartz round-bottom flask, and the solution A obtained in the first step was added dropwise to the 500mL quartz round-bottom flask containing the mixed solution B under vigorous stirring. After the addition was completed, stirring was continued for 10min to obtain a mixed solution C; finally, the solution C prepared in the third step was placed in a microwave reactor with a normal pressure reflux cooling device. The model of the microwave reactor is "Midea PJ21C-AU", with a heating power of 1000W and a frequency of 2450MHz; the heating temperature is set to 100°C and the reaction time is 150min; after the reaction is completed, the product in the quartz round-bottom flask is cooled to room temperature, and the product is transferred to a centrifuge, centrifuged at 5000rpm for 2min, the supernatant is removed and the lower layer product is taken out, the lower layer product is washed 3 times with distilled water, and then washed 3 times with ethanol, and then the washed product is placed in an oven, and dried at 70°C for 24h to obtain the target BiVO4 material.

[0033] The X-ray diffraction results of the product are consistent with the JCPDS card number 14-0688 ( Figure 1 ), the strongest peak corresponds to the hkl crystal plane index The product space group is I2 / a, and the unit cell parameters are and α=γ=90.0° and β=90.38°, the crystal structure is shown in the figure Figure 2 shown.

[0034] Scanning electron microscope (SEM) images of the samples Figures 3 to 5 ) shows that the sample morphology is a micron-spherical BiVO4 assembled from nanosheets. The thickness of the nanosheets is measured to be 11.74-35.25 nm, and the diameter of the microspheres is 1.24-1.34 μm. The schematic diagram of the morphology is shown in Figure 6As shown; the X-ray diffraction test results and scanning electron microscope test results of the product both provide strong evidence to confirm that the material is a pure monoclinic bismuth vanadate material, the sample has good crystallinity and uniform morphology and size, and is a very promising photocatalytic functional material.

[0035] Example 2 Preparation of BiVO4 Sample 2 Using Microwave Radiation Technology

[0036] At room temperature, 2.0615 g of analytical pure Bi(NO3)3·5H2O and 0.7745 g of hexadecyltrimethylammonium bromide (CATB) were weighed and placed in a 250 mL beaker, and 115 mL of distilled water was added. The beaker was placed on a magnetic stirrer at a speed of 800 rpm and stirred at a constant speed for 15 min. After stirring, it was transferred to a 250 mL round-bottom flask and placed in a microwave reactor with a normal pressure reflux cooling device. The model of the microwave reactor was "Midea PJ21C-AU", with a heating power of 1200 W and a frequency of 2450 MHz. The heating temperature was set to 95 ° C. After mixing for 60 min, a mixed solution A was obtained; then, 0.7457 g of NH4VO3 was placed in a 100mL beaker, 85mL of distilled water was added, and the beaker was placed on a magnetic stirrer at a speed of 800rpm and stirred at a uniform speed for 15min to obtain a homogeneous aqueous solution B; then, the mixed solution B was transferred to a 500mL quartz round-bottom flask, and the solution A obtained in the first step was added dropwise to the 500mL quartz round-bottom flask containing the mixed solution B under vigorous stirring. After the addition was completed, stirring was continued for 10min to obtain a mixed solution C; finally, the solution C prepared in the third step was placed in a microwave reactor with a normal pressure reflux cooling device. The model of the wave reactor is "Midea PJ21C-AU", with a heating power of 1200W and a frequency of 2450MHz; the heating temperature is set to 95°C and the reaction time is 150min; after the reaction is completed, the product in the quartz round-bottom flask is cooled to room temperature, and the product is transferred to a centrifuge and centrifuged at 5000rpm for 2min. The supernatant is removed and the lower layer product is taken out, and the lower layer product is washed 3 times with distilled water and then washed 3 times with ethanol. The washed product is then placed in an oven and dried at 70°C for 24h to obtain the target BiVO4 material.

[0037] Example 3 Preparation of BiVO4 Sample 3 Using Microwave Radiation Technology

[0038] At room temperature, 2.0615 g of analytical pure Bi(NO3)3·5H2O and 0.7745 g of hexadecyltrimethylammonium bromide (CATB) were weighed and placed in a 250 mL beaker, and 115 mL of distilled water was added. The beaker was placed on a magnetic stirrer at a speed of 800 rpm and stirred at a constant speed for 15 min. After stirring, it was transferred to a 250 mL round-bottom flask and placed in a microwave reactor with a normal pressure reflux cooling device. The model of the microwave reactor was "Midea PJ21C-AU", with a heating power of 1500 W and a frequency of 2450 MHz. The heating temperature was set to 80°C and mixed for 60 min to obtain a mixed solution A. Subsequently, 0.7457 g of NH4VO3 was placed in a 100mL beaker, 85mL of distilled water was added, and the beaker was placed on a magnetic stirrer at a speed of 800rpm and stirred at a uniform speed for 15min to obtain a homogeneous aqueous solution B; then, the mixed solution B was transferred to a 500mL quartz round-bottom flask, and the solution A obtained in the first step was added dropwise to the 500mL quartz round-bottom flask containing the mixed solution B under vigorous stirring. After the addition was completed, stirring was continued for 10min to obtain a mixed solution C; finally, the solution C prepared in the third step was placed in a microwave reactor with a normal pressure reflux cooling device. The model of the wave reactor is "Midea PJ21C-AU", with a heating power of 1500W and a frequency of 2450MHz; the heating temperature is set to 80°C and the reaction time is 150min; after the reaction is completed, the product in the quartz round-bottom flask is cooled to room temperature, and the product is transferred to a centrifuge, centrifuged at 5000rpm for 2min, the supernatant is removed and the lower layer product is taken out, the lower layer product is washed 3 times with distilled water, and then washed 3 times with ethanol, and then the washed product is placed in an oven, and dried at 70°C for 24h to obtain the target BiVO4 material.

[0039] The above are only three embodiments of the present invention, not all embodiments. Any equivalent changes made to the technical solution of the present invention by ordinary technicians in this field after reading the specification of the present invention are covered by the claims of the present invention.

[0040] Comparative Example 1 of Example 1:

[0041] (Ke D, Peng T, Ma L, et al. Effects of hydrothermal temperature on the microstructures of BiVO4 and its photocatalytic O2 evolution activity undervisible light[J]. Inorganic Chemistry, 2009, 48: 4685-4691) Ke et al. used a hydrothermal method to synthesize monoclinic bismuth vanadate materials. The operation was as follows: 2.9100 g Bi(NO3)3·5H2O and 0.7204 g NH4VO3 were dissolved in 30 mL 0.5 M HNO3 under magnetic stirring; then, 30 mL 0.03 M The CTAB solution was added to the above mixture and stirred vigorously; the pH of the above mixture was adjusted to 6.00 with an ammonia solution; after standing for 12 hours, the mixture was transferred to a stainless steel autoclave lined with polytetrafluoroethylene and kept at different temperatures for 72 hours; the solid obtained by the reaction was separated by centrifugation and washed with water and ethanol three times, and then dried in air; subsequently, 0.5000g of the prepared sample was stirred and mixed with 40mL of 0.05M sodium acetate ethanol solution at 40°C for 72 hours for anion exchange treatment; the solid was washed with water and ethanol, and then dried at 60°C to obtain the product; this method requires the use of acid and alkali for pH adjustment, the operation is complicated and time-consuming, the reaction requires high temperature and high energy consumption, and the product particle size is large; the BiVO4 prepared at a hydrothermal temperature of 160°C has a particle size range of 7 to 12μm, which is a mixed crystal composed of tetragonal phase and monoclinic phase; and BiVO4 with pure monoclinic phase needs to be obtained at a higher hydrothermal temperature of 200°C.

[0042] The method, innovation and technical effect disclosed in the present invention are essentially different from those of the comparative example.

[0043] Comparative Example 2 of Example 1:

[0044] (García-Pérez UM, Sepúlveda-Guzmán S, Martínez-De La Cruz A. Nanostructured BiVO4 photocatalysts synthesized via a polymer-assisted coprecipitation method and their photocatalytic properties under visible-light irradiation [J]. Solid State Sciences, 2012, 14 (3): 293-298) García-Pérez et al. used the coprecipitation method to synthesize bismuth vanadate materials as follows: at 70 ° C, 0.03 mol Bi(NO3)3·5H2O was dissolved in 100 mL 4M HNO3 solution to obtain solution A; 0.03 mol NH4VO3 was dissolved in 100 mL 2M NH4OH solution to obtain a homogeneous aqueous solution B; 1.84 g CMC was dissolved in 100 mL of distilled water to obtain solution C; 50 mL of CMC solution C was added to solution A and solution B respectively at room temperature, and the mixture was mixed for 60 minutes under continuous stirring to obtain two transparent solutions D and E; then, the bismuthate CMC mixed solution D was added dropwise to the vanadate CMC mixed solution E under vigorous stirring; after mixing, the pH value of the solution was adjusted to 9 using a 2M NH4OH solution to obtain a yellow suspension, which was stirred for 1 hour; the yellow dispersion was cooled to room temperature and its water content was removed by a freeze-drying process; the obtained orange powder was annealed in air at 350°C for 24 hours, and after cooling, it was washed several times with distilled water to obtain a bismuth vanadate product.

[0045] The method, innovation and technical effect disclosed in the present invention are essentially different from those of the comparative example.

[0046] Comparative Example 3 of Example 1:

[0047] (Wang F, Shao M, Cheng L, et al. The synthesis of monoclinic bismuthvanadate nanoribbons and studies of photoconductive, photoresponse, and photocatalytic properties [J]. Materials Research Bulletin, 2009, 44 (8): 1687-1691) Wang et al. used the hydrothermal method to synthesize the target product as follows: First, weigh 0.047 g of BiCl3 was placed in 40mL of distilled water, the pH value was adjusted to 10 with 0.1mol / L NaOH solution, and stirred for 2h; secondly, 0.018g NH4VO3 was weighed and added to the above solution, and stirred for 30min; then, the stirred solution was transferred to a 50mL stainless steel autoclave and heated at 180℃ for 14h; after the reaction, the yellow precipitate was separated by centrifugation and washed with distilled water and anhydrous ethanol; then the washed product was vacuum dried at 50℃ for 6h to obtain the target product; this method cannot prepare products in which 14-0133, 14-0688 phase BiVO4 and 48-575 phase [Bi6O5(OH)3](NO3)5·3H2O coexist, and the obtained product is a nanotube with a size of 60-80nm.

[0048] The method, innovation and technical effect disclosed in the present invention are essentially different from those of the comparative example.

[0049] Example 4 Preparation of BiVO4 Sample 4 Using Microwave Radiation Technology

[0050] At room temperature, 2.0615 g of analytical pure Bi(NO3)3·5H2O and 0.7745 g of hexadecyltrimethylammonium bromide (CATB) were weighed and placed in a 250 mL beaker, and 115 mL of distilled water was added. The beaker was placed on a magnetic stirrer at a speed of 800 rpm and stirred at a constant speed for 15 min. After stirring, it was transferred to a 250 mL round-bottom flask and placed in a microwave reactor with a normal pressure reflux cooling device. The model of the microwave reactor was "Midea PJ21C-AU", with a heating power of 500 W and a frequency of 2450 MHz. The heating temperature was set to 120 ° C and mixed for 60 min to obtain a mixed solution A. Subsequently, 0.7457 g NH4VO3 was placed in a 100mL beaker, 85mL of distilled water was added, and the beaker was placed on a magnetic stirrer at a speed of 800rpm and stirred at a uniform speed for 15min to obtain a homogeneous aqueous solution B; then, the mixed solution B was transferred to a 500mL quartz round-bottom flask, and the solution A obtained in the first step was added dropwise to the 500mL quartz round-bottom flask containing the mixed solution B under vigorous stirring. After the addition was completed, stirring was continued for 10min to obtain a mixed solution C; finally, the solution C prepared in the third step was placed in a microwave reactor with a normal pressure reflux cooling device. The model of the wave reactor is "Midea PJ21C-AU", with a heating power of 200W and a frequency of 2450MHz; the heating temperature is set to 120℃ and the reaction time is 150min; after the reaction is completed, the product in the quartz round-bottom flask is cooled to room temperature, and the product is transferred to a centrifuge, centrifuged at 5000rpm for 2min, the supernatant is removed and the lower layer product is taken out, the lower layer product is washed 5 times with distilled water, and then washed 4 times with ethanol, and then the washed product is placed in an oven, and dried at 70℃ for 24h to obtain the target BiVO4 material.

[0051] Example 5 Preparation of BiVO4 Sample 5 Using Microwave Radiation Technology

[0052] At room temperature, 2.0615 g of analytical pure Bi(NO3)3·5H2O and 0.7745 g of hexadecyltrimethylammonium bromide (CATB) were weighed and placed in a 250 mL beaker, and 115 mL of distilled water was added. The beaker was placed on a magnetic stirrer at a speed of 800 rpm and stirred at a constant speed for 15 min. After stirring, it was transferred to a 250 mL round-bottom flask and placed in a microwave reactor with a normal pressure reflux cooling device. The model of the microwave reactor was "Midea PJ21C-AU", with a heating power of 2000 W and a frequency of 2450 MHz. The heating temperature was set to 90 ° C. After mixing for 60 min, a mixed solution A was obtained; then, 0.7457 g of NH4VO3 was placed in a 100mL beaker, 85mL of distilled water was added, and the beaker was placed on a magnetic stirrer at a speed of 800rpm and stirred at a uniform speed for 15min to obtain a homogeneous aqueous solution B; then, the mixed solution B was transferred to a 500mL quartz round-bottom flask, and the solution A obtained in the first step was added dropwise to the 500mL quartz round-bottom flask containing the mixed solution B under vigorous stirring. After the addition was completed, stirring was continued for 10min to obtain a mixed solution C; finally, the solution C prepared in the third step was placed in a microwave reactor with a normal pressure reflux cooling device. The model of the wave reactor is "Midea PJ21C-AU", with a heating power of 2000W and a frequency of 2450MHz; the heating temperature is set to 100℃ and the reaction time is 90min; after the reaction is completed, the product in the quartz round-bottom flask is cooled to room temperature, and the product is transferred to a centrifuge and centrifuged at 5000rpm for 2min. The supernatant is removed and the lower layer product is taken out, and the lower layer product is washed 4 times with distilled water and then washed 5 times with ethanol. The washed product is then placed in an oven and dried at 70℃ for 24h to obtain the target BiVO4 material.

Claims

1. A method for preparing nanosheet-assembled micron-spherical monoclinic BiVO4 material by microwave radiation, characterized in that The following steps are involved: First, weigh 2.0615g analytical pure Bi(NO3)3·5H2O and 0.7745g hexadecyltrimethylammonium bromide (CTAB) and place them in a 250mL beaker, add 115mL distilled water and stir them evenly with magnetic force, then place them in a microwave reactor, set the heating power to 500-2000W, the frequency to 2450MHz, and the heating temperature to 80-120℃, mix and stir for 60min to obtain a mixed solution A; Second, weigh 0.7457 g NH4VO3 into a 100 mL beaker, add 85 mL distilled water and stir evenly with magnetic force to obtain a homogeneous aqueous solution B; In the first and second steps, the magnetic stirring speed was 800 rpm and the stirring time was 15 min; Third, the homogeneous aqueous solution B prepared in the second step is transferred to a 500 mL quartz round-bottom flask, and the mixed solution A obtained in the first step is added dropwise to the 500 mL quartz round-bottom flask containing the homogeneous aqueous solution B under vigorous stirring. After the addition is completed, the mixture is stirred continuously to obtain a mixed solution C; Fourth, the mixed solution C prepared in the third step is placed in a microwave reactor with a normal pressure reflux cooling device, and the heating power is set to 200-2000 W and the frequency is set to 2450 MHz; the heating temperature is set to 80-120° C. and the reaction time is set to 150 min; Fifth, after the reaction is completed, wait for the product in the quartz round-bottom flask to cool to room temperature, transfer the product to a centrifuge and centrifuge at 5000 rpm for 2 minutes, remove the supernatant and take out the lower layer sample, wash the solid sample with distilled water for 3 to 5 times, and then wash it with ethanol for 3 to 5 times, then place the washed product in an oven, and dry it at 70°C for 24 hours to obtain a nanosheet-assembled micron-spherical monoclinic BiVO4 material.

2. A nanosheet-assembled micron-spherical monoclinic BiVO4 material prepared by the method according to claim 1, characterized in that: The nanosheets are assembled into micron-shaped spherical BiVO4, with the thickness of the nanosheets ranging from 11.74 to 35.25 nm and the diameter of the microspheres ranging from 1.24 to 1.34 μm.

Citation Information

Patent Citations

  • Bismuth vanadate powder and preparation method thereof

    CN101318700A

  • Surface active agent assisting alcohol-hydrothermal method for preparing anthoid BiVO4