A two-component external cross-linking thickener
By using two-component diplomatic thickener in oil and gas field fracturing and oil production, the rapid crosslinking of aziridine crosslinking agent and polyacrylamide is solved, the slow reaction speed and environmental hazards of traditional high-valent metal ion crosslinking agents are solved. The problem of this method has achieved efficient cross-linking of thickeners and good temperature and salt resistance, which has improved the production increase effect of oil and gas field fracturing.
Patent Information
- Application Number
- CN202310575595.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-19
AI Technical Summary
During oil fracturing and oil production in oil and gas fields, traditional high-priced metal ion crosslinking agents react slowly and are harmful to the environment, resulting in high construction cost of thickeners, poor sand carrying capacity and pressurization effect, and it is difficult to crosslink quickly under environmentally friendly conditions. , affects the fracturing effect.
Using two-component diplomatic thickening agent, the viscosity of the thickening agent is improved by adding aziridine crosslinking agent to the water and the carboxyl group of modified polyacrylamide to rapidly crosslink, thereby enhancing the sand carrying and pressurization properties. And covalent bonds are formed through rapid reaction between aziridine groups and carboxyl groups to achieve efficient crosslinking.
The rapid viscosity-enhancing effect of thickener is achieved, sand carrying and pressurized performance is improved, construction costs are reduced, and the crosslinked thickener has good temperature resistance and salt resistance, which solves the reaction speed of traditional crosslinking agents. Slow and environmental hazards.
Smart Images

Figure BDA0004243991370000021 
Figure BDA0004243991370000081 
Figure BDA0004243991370000091
Abstract
Description
Technical Field
[0001] The invention specifically relates to the technical field of oil and gas field development, and in particular to a two-component external cross-linking thickener suitable for the technical field of fracturing of low-permeability reservoirs in oil and gas fields. Background Art
[0002] In the fracturing and oil production enhancement process of oil and gas fields, a higher viscosity of the thickener solution allows more sand to be carried, showing a better fracturing effect. So far, increasing the concentration of the thickener solution or adding a cross-linking agent are commonly used strategies to quickly increase the viscosity of the thickener solution. Due to the high unit price of the thickener, increasing the viscosity of the fracturing fluid by simply increasing the amount of thickener added will significantly increase the construction cost. Although the unit price of the added cross-linking agent is high, due to the small amount of the added cross-linking agent, the overall cost-effectiveness is high and the viscosity increase effect is significant. The current high-valent ionic cross-linking agents undergo complex hydrolysis, coordination and other reactions in water. Among them, the formation of hydroxyl bridges and coordination reactions after hydrolysis can form a three-dimensional structure and increase the viscosity of the system. Adjusting the pH value of the solution can significantly improve the gelation rate. For example, for every half unit decrease in the pH of the solution, the gelation rate of the system will increase by about 2.2 times (Bhaskar R. Transient Rheological Properties of Chromium / polyacrylamide Solutions Gelling Under Supposed Steady and Oscillatory Shear strains. Kansas: University of Kansas, 1988). When the pH of the solution is low, the high-valent metal ions are rapidly hydrolyzed to form metal ion hydroxyl bridges. The reaction of high-valent metal ions to form hydroxyl bridges is a slow reaction restricted by the pH value, and is the main factor affecting the change rate of the viscosity of the entire thickener aqueous solution from low to high. Therefore, under environmentally friendly conditions (without adjusting the pH value and without adding harmful metal ions), it is still a difficult problem to prepare a fast cross-linking (fast viscosity increase) thickener.
[0003] Polyaziridine compounds are often used in water-based paints to improve the color fixation and chemical resistance of the coating. They can fix the tannins in the wood at the interface between the primer and the wood, and can effectively prevent light-colored topcoats from changing color due to the free migration of tannins in the wood.
[0004] Therefore, the current problems that traditional high-priced metal ion cross-linking agents have slow reaction speeds and are harmful to equipment and the environment, as well as how to effectively reduce the construction cost of thickeners while improving sand carrying capacity, pressurization effect, and salt and temperature resistance are practical problems that need to be solved urgently. Summary of the invention
[0005] The present invention proposes a two-component external cross-linking thickener. After the thickener is dissolved in water, an aziridine cross-linking agent is added to quickly cross-link with the carboxyl group in the modified polyacrylamide, thereby increasing the apparent viscosity of the thickener aqueous solution, improving its sand carrying capacity and pressurizing effect, so that it can meet the requirements of fracturing construction and achieve the effect of increasing production.
[0006] To achieve the above-mentioned object of the invention, the technical solution of the present invention is as follows:
[0007] A two-component external cross-linking thickener, comprising, by weight:
[0008] 40-50 parts of white oil,
[0009] APAM powder 50-60 parts,
[0010] Phase transfer agent 2-5 parts,
[0011] 1-3 parts of viscosity regulator,
[0012] 0.05-0.5 parts of modified aziridine compound;
[0013] Among them, white oil, APAM powder, phase transfer agent, viscosity regulator are basic thickener components, and modified aziridine compound is external crosslinking agent component;
[0014] The modified aziridine compound is at least one of trimethylolpropane-tris[3-(2-methylaziridinyl) propionate], trimethylolpropane-tris(3-aziridinyl propionate), pentaerythritol tris(3-aziridinyl propionate) and pentaerythritol tetrakis(3-aziridinyl propionate);
[0015] The APAM powder is selected from one or more of polymers (I)-(V),
[0016]
[0017] The average diameter of APAM powder is 80-120 μm, and the molecular weight is 1.5×10 7 g / mol-2.8×10 7 g / mol, m:n=1.5~3:1, a, b, o, p, q are positive integers not less than 1, (m+n)≥1000(o+p);
[0018] Furthermore, one or more of the polymers (I)-(V) are prepared according to the following method:
[0019] 1) mixing reactants acrylamide, acrylic acid, p-styrene sulfonic acid and / or polyethylene glycol monoacrylate, or mixing reactants acrylamide and acrylic acid, and then adding 0.05-0.5% of the total mass of the reactants ammonium persulfate-sodium sulfite and 0.05-0.5% of the total mass of the reactants azobisisobutylimidazole; then initiating a copolymerization reaction under stirring, nitrogen atmosphere and 75° C.-85° C. conditions until the reaction is complete, and then drying to constant weight to obtain a polymerization intermediate product,
[0020] The molar ratio of acrylamide to acrylic acid is 1.5 to 3:1, and the molar amount of styrene sulfonic acid and / or polyethylene glycol monoacrylate is not higher than 0.1% of the total molar amount of acrylamide and acrylic acid;
[0021] 2) dissolving the polymerization intermediate product prepared in step 1) in water to prepare a polymerization intermediate aqueous solution with a mass percentage concentration of 10% to 20%;
[0022] 3) Then, sodium hydroxide is added to carry out a neutralization reaction to consume 99% to 99.95% of the total molar amount of the carboxyl groups in the polymerization intermediate product, and then spray-dried, ground, and sieved to obtain a mixture of one or more of the polymers (I) to (V).
[0023] Preferably, the phase transfer agent is at least one of decyl dihydroxyethyl amine oxide, dodecyl dihydroxyethyl amine oxide, tetradecyl dihydroxyethyl amine oxide, hexadecyl dihydroxyethyl amine oxide, octadecyl dihydroxyethyl amine oxide, dodecyl amide propyl amine oxide, myristyl amide propyl amine oxide, hexadecyl amide propyl amine oxide, octadecyl amide propyl amine oxide, isomeric tridecyl alcohol polyoxyethylene ether, octadecyl trimethyl ammonium chloride, hexadecyl trimethyl ammonium chloride, tetradecyl trimethyl ammonium chloride, dodecyl trimethyl ammonium chloride, Tween 20, Tween 40, Tween 65, Tween 80, Tween 81 or Tween 85.
[0024] Preferably, the viscosity regulator is at least one of hydroxymethyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl cellulose, xanthan gum, calcium bentonite, sodium bentonite, and organic bentonite.
[0025] Preferably, the white oil is selected from at least one of No. 3 white oil, No. 5 white oil, No. 7 white oil, No. 10 white oil and No. 15 white oil.
[0026] The present invention provides a method for using a two-component external cross-linking thickener, comprising the following steps:
[0027] (1) adding white oil and viscosity regulator in sequence, and uniformly dispersing phase transfer agent and APAM powder in the white oil in sequence under stirring and at room temperature to 90° C. to obtain a mixed solution; then, cooling the mixed solution to room temperature, filtering and packaging to obtain a basic thickener component;
[0028] (2) filtering the polyaziridine compound or its solution, filling it with inert gas, and packaging it to obtain the external crosslinking agent component of the basic thickener in step 1).
[0029] Preferably, the solvent used to dissolve the polyaziridine compound in step (2) is at least one of tap water, deionized water, distilled water, methanol, ethanol, tetrahydrofuran, dimethylformamide, dimethylacetamide, dimethyl sulfoxide, and 1,4-dioxane.
[0030] The modified aziridine compound needs to be filled with inert gas such as high-purity nitrogen or argon before sealing and packaging.
[0031] It should be noted that the total molar amount of carboxyl and / or sulfonic acid groups in one or more of the polymers (I)-(V) finally prepared by the present invention is 0.05%-1% of the total molar amount of carboxyl and / or sulfonic acid groups contained in the polymer intermediate product before neutralization. This is because the content of carboxyl and / or sulfonic acid groups retained in one or more of the polymers (I)-(V) should not be too much or too little, and must be maintained in the range of 0.05%-0.1%. When the content of carboxyl and / or sulfonic acid groups is lower than 0.05%, the number of groups in polymers (I)-(V) that react with aziridine is too small, the thickening effect of the thickener is not obvious, and the construction requirements cannot be met; when the content of carboxyl and / or sulfonic acid groups is higher than 0.1%, the carboxyl and / or sulfonic acid groups on the APAM molecules that are soluble in water at the periphery of the APAM particles will first react with the aziridine groups to form a chemical cross-linking system, forming a cross-linked shell layer at the periphery of the APAM particles, causing a large number of APAM molecules to be unable to fully dissolve in water, thereby prolonging the thickening time of the thickener or reducing the viscosity of the fracturing fluid.
[0032] Compared with the prior art, the present invention has at least the following beneficial effects:
[0033] The thickener of the present invention is a two-component package, and the aziridine group reacts quickly with the carboxyl group of APAM in an aqueous solution to increase the apparent viscosity of the thickener aqueous solution, thereby obtaining a high-viscosity thickener solution, which improves the sand-carrying and pressurizing performance and is used for fracturing and production increase in oil and gas fields. Moreover, the cross-linked thickener of the present invention has good temperature resistance; at the same time, since the addition reaction of the aziridine group with the carboxyl group or the sulfonic acid group is not affected by the mineralization of water, the aziridine cross-linked thickener solution exhibits good salt resistance.
[0034] Furthermore, the present invention can increase the viscosity of the modified polyacrylamide aqueous solution in a short time, thereby solving the problems of slow reaction speed and certain harm to equipment and environment of the traditional high-valent metal ion cross-linking agent.
[0035] In addition, the aziridine compounds of the present invention have large ring tension and high reaction activity, and can quickly react with the carboxyl groups in the APAM molecules to form a gel without heating or adjusting the pH value of the solution; each cross-linking agent molecule contains multiple aziridine functional groups, allowing a very small amount of cross-linking agent to be added (as low as 50 ppm); furthermore, the aziridine group reacts thoroughly with the carboxyl group, and even if a small amount is added, the reaction can fully occur, and there is a significant viscosity-increasing effect; the reaction between aziridine and carboxyl groups generates a covalent bond, and the APAM molecular gel obtained by cross-linking has good temperature and salt resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 .Viscosities of Example 1 and Comparative Example 1 at different stirring times (solution concentration is 0.5%).
[0037] Figure 2 .Viscosities of Example 2 and Comparative Example 2 at different stirring times (solution concentration is 0.5%).
[0038] Figure 3 .Viscosities of Example 3 and Comparative Example 3 at different stirring times (solution concentration is 0.5%). DETAILED DESCRIPTION
[0039] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0040] It should be noted that one or more of the polymers (I)-(V) in the examples are prepared according to the following method:
[0041] 1) mixing reactants acrylamide, acrylic acid, p-styrene sulfonic acid and / or polyethylene glycol monoacrylate, or mixing reactants acrylamide and acrylic acid, and then adding 0.05-0.5% of the total mass of the reactants ammonium persulfate-sodium sulfite and 0.05-0.5% of the total mass of the reactants azobisisobutylimidazole; then initiating a copolymerization reaction under stirring, nitrogen atmosphere and 75° C.-85° C. conditions until the reaction is complete, and then drying to constant weight to obtain a polymerization intermediate product,
[0042] The molar ratio of acrylamide to acrylic acid is 1.5 to 3:1, and the molar amount of styrene sulfonic acid and / or polyethylene glycol monoacrylate is not higher than 0.1% of the total molar amount of acrylamide and acrylic acid;
[0043] 2) dissolving the polymer intermediate product prepared in step 1) in water to prepare a mass percentage concentration of 10%-
[0044] 20% aqueous solution of polymerization intermediate;
[0045] 3) Then, sodium hydroxide is added to carry out a neutralization reaction to consume 99% to 99.95% of the total molar amount of the carboxyl groups in the polymerization intermediate product, and then spray-dried, ground, and sieved to obtain a mixture of one or more of the polymers (I) to (V).
[0046] The method for preparing the polymer (I) of the APAM powder used in Example 1 comprises the following steps:
[0047] 1) 53.3 g acrylamide, 18.0 g acrylic acid (molar ratio 3:1), 0.18 g ammonium persulfate-sodium sulfite (accounting for 0.25% of the total mass) and 0.18 g azobisisobutylimidazole (accounting for 0.25% of the total mass) were dissolved in 214.5 g deionized water, and copolymerization was carried out under stirring and nitrogen atmosphere conditions at a reaction temperature maintained at 75°C-85°C. Then, the mixture was dried to constant weight to obtain a polymerization intermediate product;
[0048] 2) dissolving the intermediate product in water to prepare an aqueous solution of the polymerization intermediate product with a mass percentage concentration of 20%;
[0049] 3) Then, 9.9 g of sodium hydroxide was added for neutralization reaction to consume 99% of the carboxyl groups in the polymerization intermediate product, and then the product was spray-dried, ground, and passed through an 80-mesh sieve to obtain the polymer (I).
[0050] The preparation of one or more of the polymers (I)-(V) involved in other examples is the same as described above and will not be described in detail here. It is only necessary to appropriately adjust the molar ratio of the reactants and the neutralization reaction rate of sodium hydroxide and the polymerization intermediate to obtain one or more of the corresponding polymers (I)-(V).
[0051] Example 1
[0052] Two-component external cross-linking thickener - the external cross-linking agent component is trimethylolpropane-tris[3-(2-methylaziridinyl) propionate]
[0053] (1) Under stirring and room temperature, 15 parts of No. 3 white oil, 25 parts of No. 15 white oil, 1.8 parts of hydroxyethyl cellulose, 1.2 parts of calcium montmorillonite, 2 parts of dodecyl trimethyl ammonium chloride and 2.8×10 750 parts of g / mol APAM powder (I) (particle size 80 mesh, m:n=3:1, neutralization reaction rate of sodium hydroxide with carboxyl and / or sulfonic acid groups contained in the polymerization intermediate product is 0.99) are added to the reaction kettle. The stirring speed is controlled within the range of 90-120 rpm, stirred for 60 minutes, filtered and packaged to obtain the basic thickener component;
[0054] (2) Filter trimethylolpropane-tris[3-(2-methylaziridinyl)propionate], fill with high-purity nitrogen, and package to obtain an external crosslinking agent component of a thickener. The amount of the external crosslinking agent used is 0.05 parts.
[0055] Comparative Example 1
[0056] Under stirring and room temperature, 15 parts of No. 3 white oil, 25 parts of No. 15 white oil, 1.8 parts of hydroxyethyl cellulose, 1.2 parts of calcium montmorillonite, 2 parts of dodecyl trimethyl ammonium chloride and 2.8×10 7 50 parts of g / mol APAM powder (I) (particle size 80 mesh, m:n=3:1, neutralization reaction rate of sodium hydroxide with carboxyl and / or sulfonic acid groups contained in the polymerization intermediate product is 0.99) are added to the reaction kettle. The stirring speed is controlled within the range of 90-120 rpm, stirred for 60 minutes, filtered and packaged to obtain the basic thickener.
[0057] Performance Test of Example 1 and Comparative Example 1
[0058] The basic thickener was prepared into a standard seawater solution with a mass percentage concentration of 0.5%. After the basic thickener was dissolved for 5 minutes at room temperature and under stirring conditions, an external crosslinking agent was added to the basic thickener of Example 1, and the comparative example 1 was stirred and dissolved continuously. The apparent viscosity of the thickener solution at different dissolution times was tested using a six-speed viscometer (rotor speed was 100 rpm). The test results are shown in FIG. Figure 1 shown.
[0059] When APAM is dissolved in standard seawater for 5 minutes, the viscosity of the basic thickener solution of Example 1 and Comparative Example 1 is about 28 mPa.s. This indicates that when no external crosslinking agent is added, the viscosity of the two sample solutions is equivalent. When an external crosslinking agent is added to the basic thickener solution, the viscosity of the solution of Example 1 rises rapidly. When the stirring time reaches 8 or 9 minutes (or 3-4 minutes after the addition of the crosslinking agent), the viscosity of the APAM solution rises rapidly and gradually reaches a maximum value of about 70 mPa.s. This is because within 3-4 minutes, trimethylolpropane-tris[3-(2-methylaziridinyl) propionate] completes a crosslinking reaction with the carboxyl group on the APAM molecular chain, which rapidly increases the viscosity of the standard seawater solution of the thickener. The viscosity of the solution of Comparative Example 1 does not change much, basically within 30 mPa.s.
[0060] It is shown that after adding the external cross-linking agent, the two-component external cross-linking thickener of the present invention exhibits better viscosity, improves the sand carrying and pressurizing performance, and can be effectively used for fracturing and production increase in oil and gas fields.
[0061] The products of Example 1 and Comparative Example 1 were prepared into a solution with a mass concentration of 0.5% using standard seawater and stirred for 10 minutes. -1 Under the same conditions, the viscosity values at 90°C, 110°C and 130°C were measured respectively. The results are shown in Table 1.
[0062] Table 1. Viscosity of the solutions of Example 1 and Comparative Example 1 at different temperatures
[0063] Test temperature Example 1 Solution Viscosity Comparative Example 1 Solution Viscosity 90℃ 64mPa.s 26mPa.s 110℃ 59mPa.s 22mPa.s 130℃ 53mPa.s 20mPa.s
[0064] It can be seen from Table 1 that the viscosity of the two sample solutions tends to decrease with increasing temperature. For example, at 90°C, the apparent viscosity of the solution of Example 1 is 64mPa·s; at 110°C, the viscosity of the solution is 59mPa·s; at 130°C, the viscosity of the solution is 53mPa·s. The viscosity of the thickener solution of Comparative Example 1 decreases from 26mPa·s to 20mPa·s at 90°C, 110°C and 130°C.
[0065] It shows that the present invention is less affected by temperature and still maintains a relatively high viscosity (about 60 mPa.s) within the range of temperature changes. Furthermore, under the same temperature conditions, the viscosity of the solution of Example 1 is still more than twice that of the solution of Comparative Example 1, and it is maintained at a relatively high viscosity level, indicating that Example 1 has better heat resistance (not greatly affected by temperature) and salt resistance. This is because the three-dimensional cross-linked structure formed by the external cross-linking of the present invention has good strength, which makes up for the local collapse of the hydrated APAM molecular chain.
[0066] Example 2
[0067] Two-component external crosslinking thickener - the external crosslinking agent components are (trimethylolpropane-tris[3-(2-methylaziridinyl) propionate] and pentaerythritol tetrakis(3-aziridinyl propionate))
[0068] (1) Under stirring and 90°C, 50 parts of No. 10 white oil, 1 part of hydroxypropyl cellulose, 5 parts of hexadecyl dihydroxyethyl amine oxide and 1.5×10 7 60 parts of g / mol APAM powder (II) (particle size 120 mesh, m:n=1.5:1, neutralization reaction rate of sodium hydroxide with carboxyl and / or sulfonic acid groups contained in the polymerization intermediate product is 0.9995) are added to the reaction kettle. The stirring speed is controlled within the range of 90-120 rpm, stirred for 60 minutes, filtered and packaged to obtain the basic thickener component;
[0069] (2) Under the protection of high-purity argon, trimethylolpropane-tris[3-(2-methylaziridinyl) propionate] and pentaerythritol tetrakis(3-aziridinyl propionate) were added to the reaction kettle in a mass ratio of 3:2, and deionized water was added to adjust the mass percentage concentration of the polyaziridine crosslinking agent aqueous solution to 30%. Stir for 30 minutes, filter, fill with high-purity argon, and package to obtain the external crosslinking agent component of the thickener. The amount of the external crosslinking agent is 0.5 parts.
[0070] Comparative Example 2
[0071] Under stirring and 90°C, 50 parts of No. 10 white oil, 1 part of hydroxypropyl cellulose, 5 parts of hexadecyl dihydroxyethyl amine oxide and 1.5×10 7 60 parts of g / mol APAM powder (II) (particle size 120 mesh, m:n=1.5:1, neutralization reaction rate of sodium hydroxide with carboxyl and / or sulfonic acid groups contained in the polymerization intermediate product is 0.9995) are added to the reaction kettle. The stirring speed is controlled within the range of 90-120 rpm, stirred for 60 minutes, filtered and packaged to obtain the basic thickener.
[0072] Performance Tests of Example 2 and Comparative Example 2
[0073] The basic thickener was prepared into a standard seawater solution with a mass percentage concentration of 0.5%. After the basic thickener was dissolved for 5 minutes at room temperature and under stirring conditions, the external crosslinking agent was added to Example 2, and the comparative example 2 was stirred and dissolved. The apparent viscosity of the thickener solution at different dissolution times was tested using a six-speed viscometer (rotor speed was 100 rpm). The test results are shown in FIG. Figure 2 shown.
[0074] When APAM was dissolved in standard seawater for 5 minutes, the viscosity of the basic thickener solution of Example 2 and Comparative Example 2 was about 35 mPa.s. This indicates that when no external crosslinking agent is added, the viscosity of the two sample solutions is the same. When a polyaziridine-based crosslinking agent is added, the viscosity of the solution of Example 2 rises rapidly. After 3-4 minutes of reaction between the crosslinking agent and the APAM molecular chain, the viscosity of the solution gradually reaches a maximum value and stabilizes at about 75 mPa.s. Under the same conditions, the viscosity of the solution of Comparative Example 2 does not change much, fluctuating around 35 mPa.s.
[0075] It is shown that after adding the external cross-linking agent, the two-component external cross-linking thickener of the present invention exhibits a better viscosity (about 75 mPa.s), improves the sand carrying and pressurizing performance, and can be effectively used for fracturing and production increase in oil and gas fields.
[0076] The products of Example 2 and Comparative Example 2 were prepared into a solution with a mass concentration of 0.5% using standard seawater and stirred for 10 minutes. -1Under the same conditions, the viscosity values at 90°C, 110°C and 130°C were measured respectively. The results are shown in Table 2.
[0077] Table 2. Viscosity of solution of Example 2 and Comparative Example 2 at different temperatures
[0078]
[0079]
[0080] It can be seen from Table 2 that the viscosity of the two sample solutions tends to decrease with increasing temperature. For example, at 90°C, the apparent viscosity of the solution is 68mPa·s; at 110°C, the viscosity of the solution is 63mPa·s; at 130°C, the viscosity of the solution is 58mPa·s. The viscosity of the thickener solution of Comparative Example 1 decreases from 32mPa·s to 22mPa·s at 90°C, 110°C and 130°C.
[0081] It shows that the present invention is less affected by temperature and still maintains a relatively high viscosity (about 63 mPa.s) within the range of temperature changes. Moreover, under the same temperature conditions, the viscosity of the solution of Example 2 is still more than twice that of the solution of Comparative Example 2, and is maintained at a relatively high viscosity level, indicating that Example 2 has better temperature resistance (not greatly affected by temperature) and salt resistance.
[0082] Example 3
[0083] Two-component external cross-linking thickener - the external cross-linking agent components are trimethylolpropane-tris (3-aziridinyl propionate) and pentaerythritol tris (3-aziridinyl propionate)
[0084] (1) Under stirring and 70°C, 10 parts of No. 5 white oil, 15 parts of No. 7 white oil, 10 parts of No. 10 white oil, 10 parts of No. 15 white oil, 1 part of hydroxyethyl cellulose, 0.5 parts of xanthan gum, 0.5 parts of organic montmorillonite, 0.5 parts of sodium bentonite, 2 parts of decyl dihydroxyethyl amine oxide, 1 part of isomeric tridecanol polyoxyethylene ether, 0.5 parts of Tween 80 phase transfer agent, and 2.1×10 7 g / mol APAM powder (III) (particle size 90 mesh, m:n = 2:1, neutralization reaction rate of sodium hydroxide with carboxyl and / or sulfonic acid groups contained in the polymerization intermediate product is 0.992) 20 parts, molecular weight 1.7×10 7 g / mol APAM powder (IV) (particle size 80 mesh, m:n = 3:1, the neutralization reaction rate of sodium hydroxide with the carboxyl and / or sulfonic acid groups contained in the polymerization intermediate product is 0.9994) 5 parts and molecular weight 2.5×10 730 parts of 100 g / mol APAM powder (V) (particle size 110 mesh, m:n=2.5:1, neutralization reaction rate of sodium hydroxide with carboxyl and / or sulfonic acid groups contained in the polymerization intermediate product is 0.99) are added to the reactor. The stirring speed is controlled within the range of 90-120 rpm, stirred for 60 minutes, filtered and packaged to obtain the basic thickener component; (2) under the protection of high-purity argon, trimethylolpropane-tris (3-aziridine propionate) and pentaerythritol tris (3-aziridine propionate) are added to the reactor in a mass ratio of 4:1, methanol and dimethylformamide are added (mixed in a mass ratio of 9:1), and the mass percentage concentration of the polyaziridine crosslinker solution is adjusted to 80%. Stir for 30 minutes, filter, fill with high-purity nitrogen, and package to obtain the external crosslinker component of the thickener. The amount of the external crosslinker is 0.35 parts.
[0085] Comparative Example 3
[0086] Under stirring and 70 ° C, 10 parts of No. 5 white oil, 15 parts of No. 7 white oil, 10 parts of No. 10 white oil, 10 parts of No. 15 white oil, 1 part of hydroxyethyl cellulose, 0.5 parts of xanthan gum, 0.5 parts of organic montmorillonite, 0.5 parts of sodium bentonite, 2 parts of decyl dihydroxyethyl amine oxide, 1 part of isomeric tridecanol polyoxyethylene ether, 0.5 parts of Tween 80 phase transfer agent, molecular weight 2.1×10 7 g / molAPAM powder (III) (particle size 90 mesh, m:n = 2:1, neutralization reaction rate of sodium hydroxide with carboxyl and / or sulfonic acid groups contained in the polymerization intermediate product is 0.992) 20 parts, molecular weight 1.7×10 7 g / mol APAM powder (IV) (particle size 80 mesh, m:n = 3:1, the neutralization reaction rate of sodium hydroxide with the carboxyl and / or sulfonic acid groups contained in the polymerization intermediate product is 0.9994) 5 parts and molecular weight 2.5×10 7 30 parts of APAM powder (V) with a particle size of 110 mesh, m:n=2.5:1, and a neutralization reaction rate of 0.99 between sodium hydroxide and the carboxyl and / or sulfonic acid groups contained in the polymerization intermediate product are added into the reaction kettle. The stirring speed is controlled within the range of 90-120 rpm, stirred for 60 minutes, filtered and packaged to obtain a basic thickener.
[0087] Performance tests of Example 3 and Comparative Example 3:
[0088] The basic thickener was prepared into a standard seawater solution with a mass percentage concentration of 0.5%. After the basic thickener was dissolved for 5 minutes at room temperature and under stirring conditions, the crosslinking agent was added in Example 3, and the comparative example 3 was stirred and dissolved continuously. The apparent viscosity of the thickener solution at different dissolution times was tested using a six-speed viscometer (rotor speed was 100 rpm). The test results are shown in FIG. Figure 3 shown.
[0089] When APAM was dissolved in standard seawater for 5 minutes, the viscosity of the basic thickener solution of Example 3 and Comparative Example 3 was about 30 mPa.s. This indicates that when no external crosslinking agent is added, the viscosity of the two sample solutions is equivalent. When an external crosslinking agent is added to the thickener solution (Example 3), the viscosity of the solution of Example 3 rises rapidly, and the viscosity of the solution gradually reaches a maximum value of about 65 mPa.s 3-4 minutes after the addition of the crosslinking agent. This is because the crosslinking of the polyaziridine-based crosslinking agent and the carboxyl groups on the APAM molecular chain is completed within 3-4 minutes, and the viscosity of the solution increases rapidly and tends to be constant. The viscosity of the standard seawater solution of Comparative Example 3 does not change much, and is stable at about 30 mPa.s.
[0090] It is shown that the two-component external cross-linking thickener of the present invention exhibits a better viscosity (about 65 mPa.s) after adding an external cross-linking agent.
[0091] The products of Example 3 and Comparative Example 3 were prepared into a solution with a mass concentration of 0.5% using standard seawater and stirred for 10 minutes. -1 Under the same conditions, the viscosity values at 90°C, 110°C and 130°C were measured respectively. The results are shown in Table 3.
[0092] Table 3. Viscosity of solution of Example 3 and Comparative Example 3 at different temperatures
[0093] Test temperature Example 3 Solution Viscosity Comparative Example 3 Solution Viscosity 90℃ 57mPa.s 30mPa.s 110℃ 53mPa.s 27mPa.s 130℃ 48mPa.s 23mPa.s
[0094] It can be seen from Table 3 that the viscosity of the two sample solutions tends to decrease with increasing temperature. For example, at 90°C, the apparent viscosity of the solution is 57mPa·s; at 110°C, the viscosity of the solution is 53mPa·s; at 140°C, the viscosity of the solution is 48mPa·s. The viscosity of the thickener solution of Comparative Example 1 decreases from 30mPa·s to 23mPa·s at 90°C, 110°C and 140°C.
[0095] It shows that the two-component thickener of the present invention is less affected by temperature and still maintains a relatively high viscosity within the range of temperature changes. Furthermore, under the same temperature conditions, the viscosity of the solution of Example 3 is still more than twice that of the solution of Comparative Example 3, and still maintains a relatively high viscosity level, indicating that Example 3 has better temperature resistance (not greatly affected by temperature) and salt resistance.
[0096] The present invention selects a new basic thickener component APAM and a new external crosslinking agent (trimethylolpropane-tris[3-(2-methylaziridinyl) propionate], trimethylolpropane-tris(3-aziridinyl propionate), pentaerythritol tris(3-aziridinyl propionate) and pentaerythritol tetrakis(3-aziridinyl propionate)). Moreover, since the APAM molecular structure contains a small amount of acrylic acid or styrene sulfonic acid structural units (0.05%-1%), after APAM is dissolved in water, the carboxyl or sulfonic acid functional groups and the aziridine groups in the crosslinking agent molecules quickly undergo addition reaction to generate a three-dimensional network structure, which quickly increases the viscosity of the thickener aqueous solution, enhances the sand carrying capacity of the thickener aqueous solution, and improves the fracturing effect. Furthermore, the chemical bond generated by the reaction between the aziridine group and the carboxyl group or the sulfonic acid group is a covalent bond with very stable physicochemical properties. Therefore, the cross-linked thickener has good temperature resistance. At the same time, the addition reaction between the aziridine group and the carboxyl group or the sulfonic acid group is not affected by the mineralization of water. Therefore, the aziridine cross-linked thickener solution exhibits good salt resistance.
[0097] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of equivalent transformations, and these equivalent transformations all belong to the protection scope of the present invention. It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
Claims
1. A two-component external cross-linking thickener, characterized in that The thickener comprises, by weight: 40-50 parts of white oil, APAM powder 50-60 parts, Phase transfer agent 2-5 parts, 1-3 parts of viscosity regulator, 0.05-0.5 parts of modified aziridine compound; Among them, white oil, APAM powder, phase transfer agent, viscosity regulator are basic thickener components, and modified aziridine compound is external crosslinking agent component; The modified aziridine compound is at least one of trimethylolpropane-tris[3-(2-methylaziridinyl) propionate], trimethylolpropane-tris(3-aziridinyl propionate), pentaerythritol tris(3-aziridinyl propionate) and pentaerythritol tetrakis(3-aziridinyl propionate); The APAM powder is selected from one or more of polymers (I)-(V), The average diameter of polymers (I)-(V) is 80-120 μm, and the molecular weight is 1.5×10 7 g / mol-2.8×10 7 g / mol, m:n=1.5~3:1, a, b, o, p, q are positive integers not less than 1, (m+n)≥1000(o+p); Furthermore, one or more of the polymers (I)-(V) are prepared according to the following method: 1) Mixing reactants acrylamide, acrylic acid, p-styrene sulfonic acid and / or polyethylene glycol monoacrylate, or mixing reactants acrylamide and acrylic acid, and then adding 0.05-0.5% of the total mass of the reactants ammonium persulfate-sodium sulfite and 0.05-0.5% of the total mass of the reactants azobisisobutylimidazole, and dissolving them in deionized water; then initiating copolymerization reaction under stirring, nitrogen atmosphere and 75° C.-85° C. conditions until the reaction is complete, and then drying to constant weight to obtain a polymerization intermediate product, The molar ratio of acrylamide to acrylic acid is 1.5 to 3:1, and the molar amount of styrene sulfonic acid and / or polyethylene glycol monoacrylate is not higher than 0.1% of the total molar amount of acrylamide and acrylic acid; 2) dissolving the polymerization intermediate product prepared in step 1) in water to prepare a polymerization intermediate aqueous solution with a mass percentage concentration of 10% to 20%; 3) Then, sodium hydroxide is added to carry out a neutralization reaction to consume 99% to 99.95% of the total molar amount of the carboxyl and / or sulfonic acid groups in the polymerization intermediate product, and then spray-dried, ground, and sieved to obtain a mixture of one or more of the polymers (I) to (V).
2. The thickener according to claim 1, characterized in that The phase transfer agent is at least one of decyl dihydroxyethylamine oxide, dodecyl dihydroxyethylamine oxide, tetradecyl dihydroxyethylamine oxide, hexadecyl dihydroxyethylamine oxide, octadecyl dihydroxyethylamine oxide, dodecyl amide propylamine oxide, myristic amide propylamine oxide, hexadecyl amide propylamine oxide, octadecyl amide propylamine oxide, isomeric tridecyl alcohol polyoxyethylene ether, octadecyl trimethylammonium chloride, hexadecyl trimethylammonium chloride, tetradecyl trimethylammonium chloride, dodecyl trimethylammonium chloride, Tween 20, Tween 40, Tween 65, Tween 80, Tween 81 or Tween 85.
3. The thickener according to claim 1, characterized in that The viscosity regulator is at least one of hydroxymethyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl cellulose, xanthan gum, calcium bentonite, sodium bentonite and organic bentonite.
4. The thickener according to claim 1, characterized in that The white oil is selected from at least one of No. 3 white oil, No. 5 white oil, No. 7 white oil, No. 10 white oil and No. 15 white oil.
5. A method for using the two-component external cross-linking thickener according to claim 1, characterized in that The following steps are involved: (1) adding white oil and viscosity regulator in sequence, and uniformly dispersing phase transfer agent and APAM powder in the white oil in sequence under stirring and at room temperature to 90° C. to obtain a mixed solution; then, cooling the mixed solution to room temperature, filtering and packaging to obtain a basic thickener component; (2) filtering the modified aziridine compound or its solution, filling it with inert gas, and packaging it to obtain the external crosslinking agent component of the basic thickener in step (1).