A composite modified high chromium cast iron and its preparation method
By using Fe-Si alloy, Fe-Nb alloy, Fe-Ti alloy and rare earth elements composite deteriorating agent in high chromium cast iron, the carbide morphology and distribution are changed, and the brittleness and resistance of high chromium cast iron under impact conditions is solved. The problem of insufficient wearability has achieved the improvement of high toughness and wear resistance of the castings.
Patent Information
- Application Number
- CN202310710145.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-06-15
AI Technical Summary
The existing high-chromium cast iron has insufficient brittleness and material toughness under impact conditions, mainly due to the poor carbide morphology and distribution, which leads to insufficient brittleness and wear resistance of the material in its application.
Using a highly chromium cast iron metamorphic agent, including Fe-Si alloy, Fe-Nb alloy, Fe-Ti alloy and mixed rare earth elements, the carbide morphology and distribution are changed through composite metamorphic treatment, and the formation and heterogeneity of high melting point carbides are promoted. Growth of quaternary nucleus to improve the toughness and wear resistance of castings.
By improving the carbide morphology and distribution, the toughness and wear resistance of high-chromium cast iron are improved. The structure of the casting is eutectic M7C3 carbide and submicron-scale particulate carbide precipitates, with a hardness of 58~63HRC and an impact toughness of 8 ~12J/m2, significantly improving the performance of the material.
Smart Images

Figure CN116732404B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal smelting, and relates to a high-chromium cast iron and a preparation method thereof, and specifically relates to a modifier for high-chromium cast iron, high-chromium cast iron subjected to composite modification treatment using the modifier and a preparation method thereof. Background Art
[0002] The good wear resistance of high chromium cast iron comes from the high content and high hardness of M7C3 carbides in its structure, but the increase in the content of these carbides will drastically reduce the toughness of the alloy, especially the needle-shaped pro-eutectic M7C3 carbides will seriously destroy the continuity of the good matrix structure, so that when the casting is subjected to impact, the buffering effect of the matrix on stress concentration is weakened, and the brittleness of the material is significantly increased, which limits the application of high chromium cast iron in some large impact conditions. Therefore, how to improve the morphology and distribution of carbides is the key to improving the toughness of high chromium cast iron.
[0003] Modification can change the structure and distribution of cast iron, and improve the toughness and wear resistance of high chromium cast iron. Domestic and foreign studies have reported that the use of K, Na or rare earth elements to modify wear-resistant alloy cast iron can refine the structure and improve the toughness and wear resistance of cast iron to a certain extent. However, K, Na and other elements added in the form of salts are prone to produce pores in the casting, and the melt absorption rate is low, and the actual application effect is unstable, which limits its scope of use to a certain extent.
[0004] Therefore, whether a new type of deteriorating agent can be designed to overcome the above-mentioned defects has become a technical problem that needs to be solved urgently by those skilled in the art. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a high chromium cast iron modifier and high chromium cast iron prepared by using the modifier. The high chromium cast iron modifier provided by the present invention performs a composite modification treatment on the melt during the preparation process, which can improve the morphology and distribution of carbides and improve the toughness of the high chromium cast iron.
[0006] To achieve this object, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a high chromium cast iron modifier, wherein the high chromium cast iron modifier comprises, by mass percentage:
[0008] Fe-Si alloy 5% to 10%;
[0009] Fe-Nb alloy 10%~15%;
[0010] Fe-Ti alloy 10%~15%;
[0011] The balance is mixed rare earth.
[0012] In the present invention, the high chromium cast iron modifier contains elements such as Ce, La, Nb, Ti, Fe, Si, etc., and the rare earth elements therein can reduce inclusions, purify molten iron, change, refine and stabilize carbide morphology, refine grains, and purify grain boundaries; at the same time, the modifier can chemically interact with other atoms in the cast iron raw material, and can preferentially generate high melting point carbides during solidification, which can promote the growth of eutectic carbides with heterogeneous nucleation; these rare earth elements can also increase the activity of carbon in cast iron, and are insoluble in γ-Fe, have a high melt absorption rate, and are strongly adsorbed on the surface of eutectic carbides to form an adsorption film to prevent the growth of eutectic carbides. The modifier provided by the present invention can carry out composite metamorphism of the melt, change the cast iron organizational morphology and distribution so that the organizational structure of the casting prepared by the obtained high chromium cast iron is eutectic M7C3 carbide and tempered martensite characterized by submicron-sized particle carbide precipitates, thereby improving the toughness and wear resistance of the high chromium cast iron.
[0013] The high chromium cast iron modifier of the present invention includes 5% to 10% of Fe-Si alloy, for example, 5%, 6%, 7%, 8%, 9% or 10%; 10% to 15% of Fe-Nb alloy, for example, 10%, 11%, 12%, 13%, 14% or 15%; 10% to 15% of Fe-Ti alloy, for example, 10%, 11%, 12%, 13%, 14% or 15%.
[0014] As a preferred technical solution of the present invention, the mass percentage of Si in the Fe-Si alloy is 70% to 80%, for example, it can be 70%, 72%, 75%, 78%, 79% or 80%.
[0015] Preferably, the mass percentage of Nb in the Fe-Nb alloy is 50% to 65%, for example, it may be 50%, 52%, 55%, 58%, 60%, 62% or 65%.
[0016] Preferably, the mass percentage of Ti in the Fe-Ti alloy is 2% to 35%, for example, it can be 2%, 5%, 8%, 10%, 15%, 20%, 22%, 25%, 28%, 30%, 33% or 35%.
[0017] Preferably, the mixed rare earth is a cerium-rich mixed rare earth, wherein the weight percentage of Ce is 50% to 60%, for example, it can be 50%, 52%, 55%, 58%, 59% or 60%.
[0018] The present invention does not specifically limit the particle size of the high chromium cast iron modifier, and generally the millimeter-level particle size is sufficient. In actual application, the raw materials are crushed and ground using a crushing or grinding machine to form particles with uniform particle size. As a preferred technical solution of the present invention, the average particle size of the Fe-Si alloy is 5 to 20 mm, for example, 5 mm, 8 mm, 10 mm, 12 mm, 15 mm, 16 mm, 18 mm or 20 mm, etc.
[0019] Preferably, the average particle size of the Fe-Nb alloy is 5 to 20 mm, for example, 5 mm, 8 mm, 10 mm, 12 mm, 15 mm, 16 mm, 18 mm or 20 mm.
[0020] Preferably, the average particle size of the Fe-Ti alloy is 5 to 20 mm, for example, 5 mm, 8 mm, 10 mm, 12 mm, 15 mm, 16 mm, 18 mm or 20 mm.
[0021] Preferably, the average particle size of the mixed rare earth is 5 to 20 mm, for example, 5 mm, 8 mm, 10 mm, 12 mm, 15 mm, 16 mm, 18 mm or 20 mm.
[0022] In a second aspect, the present invention further provides a high chromium cast iron subjected to a composite modification treatment, wherein the high chromium cast iron is modified by adding the modifier as described in the first aspect before melt pouring.
[0023] As a preferred technical solution of the present invention, the amount of the modifier added is greater than or equal to 0.5% of the mass of the high chromium cast iron raw material, preferably 0.5% to 1.5% of the mass of the high chromium cast iron raw material; for example, it can be 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.3%, 1.4% or 1.5%. In the present invention, the amount of the modifier added is at least 0.5% of the mass of the high chromium cast iron raw material. If it is less than 0.5%, it will not have a modifier effect; and when it is higher than 1.5%, the modifier effect is equivalent when the addition amount is 1.5% and 2.0%. In order to reduce waste, the preferred addition amount is 0.5% to 1.5%.
[0024] As a preferred technical solution of the present invention, the high chromium cast iron contains the following components in mass percentage before melt pouring: 2.5% to 3.2% C, 0.5% to 1.5% Si, 1.2% to 1.5% Mn, 0.7% to 1.0% Ni, 18% to 22% Cr, 0.4% to 0.8% Mo, and the balance is Fe.
[0025] As a preferred technical solution of the present invention, the hardness of the casting prepared by using the high chromium cast iron is 58-63HRC.
[0026] The impact toughness of the casting prepared by using the high chromium cast iron is 8-12 J / m 2 .
[0027] As a preferred technical solution of the present invention, the microstructure of the casting prepared by using the high chromium cast iron is: eutectic M7C3 carbide and tempered martensite characterized by submicron-sized carbide precipitates. The casting with this characteristic structure has finer grains and better toughness; more precipitated phases, higher hardness and strength.
[0028] In a third aspect, the present invention provides a method for preparing the high chromium cast iron as described in the second aspect, the method comprising the steps of batching, smelting, modification, pouring, mold opening, sample processing and heat treatment;
[0029] Wherein, the modification treatment is to add the modifier as described in the first aspect to the melt obtained after smelting.
[0030] As a preferred technical solution of the present invention, the heat treatment step is: heating the casting obtained after sample processing for the first time, quenching after heat preservation, cooling to room temperature, heating again, tempering, and air cooling to room temperature.
[0031] Generally speaking, the temperature cannot be lower than 900°C. Preferably, the temperature of the first addition and insulation is 950°C to 1000°C, for example, it can be 950°C, 960°C, 970°C, 980°C, 990°C or 1000°C; the time is 2h to 5h, for example, it can be 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h.
[0032] Preferably, the reheating and tempering temperature is 450°C to 550°C, for example, it can be 450°C, 460°C, 480°C, 500°C, 510°C, 520°C, 530°C or 550°C; the time is 2h to 6h, for example, it can be 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h or 6h.
[0033] Preferably, the room temperature is 25°C to 30°C, for example, it may be 25°C, 26°C, 27°C, 28°C, 29°C or 30°C.
[0034] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] (1) The present invention reasonably improves the ratio of each component of the high chromium cast iron modifier, so that the obtained high chromium cast iron modifier can chemically interact with other atoms in the cast iron raw material, preferentially generates high melting point carbides during solidification, and can promote the growth of eutectic carbides with heterogeneous nucleation; the rare earth elements therein can reduce inclusions, purify molten iron, change, refine and stabilize the morphology of carbides, refine grains, and purify grain boundaries;
[0037] (2) The modifier can also increase the activity of carbon in cast iron, strongly adsorb on the surface of eutectic carbide, and has a high melt absorption rate, that is, a high utilization rate, and the usage amount can reach 0.5% of the melt mass; through reasonable smelting, casting, heat treatment and other processing processes, the strength, toughness and wear resistance of the casting are improved. The microstructure of the casting prepared by using the high chromium cast iron is eutectic M7C3 carbide and tempered martensite characterized by submicron-sized particle carbide precipitates, with a hardness of 58 to 63 HRC and an impact toughness of 8 to 12 J / m 2 . BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is the as-cast metallographic structure of high chromium cast iron sample 3 subjected to modification treatment in Application Example 2.
[0039] Figure 2 This is the as-cast metallographic structure of the high chromium cast iron of Sample 4 in Application Example 2 after no modification treatment.
[0040] Figure 3 It is the precipitation phase of the heat-treated matrix of the high chromium cast iron of sample 5 which was modified in application example 3.
[0041] Figure 4 It is the precipitation phase of the matrix of the high chromium cast iron heat-treated state of sample 6 which has not been modified in application example 3. DETAILED DESCRIPTION
[0042] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following examples are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0043] In the following examples, unless otherwise specified, all reagents and consumables used were purchased from conventional reagent manufacturers in the field; unless otherwise specified, all experimental methods and technical means used were conventional methods and means in the field.
[0044] Example 1
[0045] This embodiment provides a modifier for high chromium cast iron.
[0046] The modifier comprises: 5% Fe-Si alloy, 10% Fe-Nb alloy, 12% Fe-Ti alloy, and the balance is mixed rare earth, and the average particle size of the modifier is 5mm;
[0047] The mass percentage of Si in the Fe-Si alloy is 80%, the mass percentage of Nb in the Fe-Nb alloy is 50%, and the mass percentage of Ti in the Fe-Ti alloy is 10%;
[0048] The weight percentage of Ce in the mixed rare earth is 50%, and the total weight of Ce, La, Nd and Pr in the mixed rare earth is not less than 90% of the weight of the mixed rare earth.
[0049] Example 2
[0050] This embodiment provides a modifier for high chromium cast iron.
[0051] The modifier comprises: 8% Fe-Si alloy, 15% Fe-Nb alloy, 15% Fe-Ti alloy, and the balance is mixed rare earth. The average particle size of the modifier is 5 mm.
[0052] The remaining features remain the same as those of Example 1.
[0053] Example 3
[0054] This embodiment provides a modifier for high chromium cast iron.
[0055] The modifier includes: 10% Fe-Si alloy, 10% Fe-Nb alloy, 10% Fe-Ti alloy, and the balance is mixed rare earth, and the average particle size of the modifier is 10 mm. The mass percentage of Si in the Fe-Si alloy is 70%, and the other features are consistent with Example 1.
[0056] Example 4
[0057] This embodiment provides a modifier for high chromium cast iron.
[0058] The modifier includes: 5% Fe-Si alloy, 12% Fe-Nb alloy, 12% Fe-Ti alloy, and the balance is mixed rare earth, and the average particle size of the modifier is 20 mm. The mass percentage of Ce in the mixed rare earth is 60%, and the other features are consistent with Example 1.
[0059] Comparative Example 1
[0060] This comparative example provides a modifier for high chromium cast iron, which is different from Example 2 in that the modifier does not contain Fe-Nb alloy.
[0061] The modifier includes: 13% Fe-Si alloy, 25% Fe-Ti alloy, and the balance is mixed rare earth. The average particle size of the modifier is 5 mm, and the other characteristics are consistent with those of Example 1.
[0062] Comparative Example 2
[0063] This comparative example provides a modifier for high chromium cast iron, which is different from Example 2 in that the modifier does not contain Fe-Ti alloy.
[0064] The modifier includes: 13% Fe-Si alloy, 25% Fe-Nb alloy, and the balance is mixed rare earth. The average particle size of the modifier is 5 mm, and the other features are consistent with those of Example 1.
[0065] Comparative Example 3
[0066] This comparative example provides a modifier for high chromium cast iron, which is different from Example 2 in that the Fe-Nb alloy is replaced by potassium chloride in the modifier.
[0067] The modifier includes: the modifier includes: 8% Fe-Si alloy, 15% potassium chloride, 15% Fe-Ti alloy, and the balance is mixed rare earth. The other features are consistent with Example 1.
[0068] Comparative Example 4
[0069] This comparative example provides a modifier for high chromium cast iron, which is different from Example 2 in that the Fe-Nb alloy in the modifier is replaced by rare earth ferrosilicon.
[0070] The modifier includes: the modifier includes: 8% Fe-Si alloy, 15% rare earth ferrosilicon, 15% Fe-Ti alloy, and the balance is mixed rare earth; the weight of the rare earth in the rare earth ferrosilicon is 20% of the weight of the rare earth ferrosilicon, and the other characteristics are consistent with Example 1.
[0071] Application Example 1
[0072] This application example uses the high chromium cast iron modifier provided in Example 1 to prepare a high chromium cast iron subjected to composite modification.
[0073] The chemical composition (mass percentage) of the high chromium cast iron raw material is: 2.5% C, 0.5% Si, 1.2% Mn, 0.9% Ni, 18% Cr, 0.6% Mo, and the rest is Fe.
[0074] The production process is as follows:
[0075] (1) Ingredients: Prepare the raw materials according to the above ingredients.
[0076] (2) Smelting: The smelting is divided into two groups, one of which is subjected to modification and the other is not. Both groups are heated to 1450°C in a 25kg medium frequency induction furnace to completely melt the ingredients.
[0077] (3) Modification treatment: After complete melting, a modifier accounting for about 0.5% of the total weight of the molten iron is added (the modifier composition of Example 1: 5% Fe-Si alloy, 10% Fe-Nb alloy, 12% Fe-Ti alloy, and the balance is mixed rare earth) for modification treatment.
[0078] (4) Pouring: The modifier is completely dissolved in the molten steel and poured immediately. The mold is a cavity of Φ50×100mm.
[0079] (5) Mold opening: After the pouring is completed and cooled to room temperature, the mold is opened.
[0080] (6) Sample processing: The riser is removed and the remaining material is processed by wire cutting to form an impact specimen of 20×20×110 mm.
[0081] (7) Heat treatment: Under argon atmosphere, keep at 1000°C for 3 hours, air quench to room temperature, keep at 500°C for 5 hours and then air cool to room temperature.
[0082] The obtained casting after modification is marked as sample 1, and the casting without modification is marked as sample 2.
[0083] Application Example 2
[0084] This application example uses the high chromium cast iron modifier provided in Example 2 to prepare a high chromium cast iron subjected to composite modification.
[0085] The chemical composition (mass percentage) of the high chromium cast iron raw material is: 2.8% C, 1.2% Si, 1.3% Mn, 1.0% Ni, 20% Cr, 0.5% Mo, and the rest is Fe.
[0086] The production process is as follows:
[0087] (1) Ingredients: Prepare the raw materials according to the above ingredients.
[0088] (2) Smelting: The smelting is divided into two groups, one of which is subjected to modification treatment and the other is not. Both groups are heated to 1450°C in a 50kg medium frequency induction furnace to completely melt the ingredients.
[0089] (3) Modification treatment: After complete melting, a modifier accounting for about 1.0% of the total weight of the molten iron is added (the modifier composition of Example 2: 8% Fe-Si alloy, 15% Fe-Nb alloy, 15% Fe-Ti alloy, and the balance is mixed rare earth) for modification treatment.
[0090] (4) Pouring: The modifier is completely dissolved in the molten steel and poured immediately. The mold is a cavity of Φ100×200mm.
[0091] (5) Mold opening: After the pouring is completed and cooled to room temperature, the mold is opened.
[0092] (6) Sample processing: The riser is removed and the remaining material is processed by wire cutting to form an impact specimen of 20×20×110 mm.
[0093] (7) Heat treatment: Under argon atmosphere, keep at 950°C for 5 hours, air quench to room temperature, keep at 500°C for 5 hours and then air cool to room temperature.
[0094] The resulting modified casting is marked as sample 3. The high chromium cast iron as-cast metallographic structure of sample 3 is as follows: Figure 1 As shown; the casting obtained without modification is marked as sample 4, and the high chromium cast iron as-cast metallographic structure of sample 4 is as shown Figure 2 As shown in the figure, it can be seen from the comparison between the two figures that the grains of the crystal phase in sample 3 are finer, and finer grains indicate that the toughness of the obtained sample is better.
[0095] Application Example 3
[0096] This application example also uses the high chromium cast iron modifier provided in Example 2 to prepare a high chromium cast iron subjected to composite modification.
[0097] The chemical composition (mass percentage) of the high chromium cast iron raw material is: 3.2% C, 1.5% Si, 1.3% Mn, 0.8% Ni, 22% Cr, 0.8% Mo, and the rest is Fe.
[0098] The production process is as follows:
[0099] (1) Ingredients: Prepare the raw materials according to the above ingredients.
[0100] (2) Smelting: The smelting is divided into two groups, one of which is subjected to modification and the other is not. Both groups are heated to 1450°C in a 60kg medium frequency induction furnace to completely melt the ingredients.
[0101] (3) Modification treatment: After complete melting, a modifier accounting for about 1.5% of the total weight of the molten iron is added (the modifier composition of Example 2: 8% Fe-Si alloy, 15% Fe-Nb alloy, 15% Fe-Ti alloy, and the balance is mixed rare earth) for modification treatment.
[0102] (4) Pouring: The modifier is completely dissolved in the molten steel and poured immediately. The mold is a cavity of Φ100×200mm.
[0103] (5) Mold opening: After the pouring is completed and cooled to room temperature, the mold is opened.
[0104] (6) Sample processing: The riser is removed and the remaining material is processed by wire cutting to form an impact specimen of 20×20×110 mm.
[0105] (7) Heat treatment: Under argon atmosphere, keep at 950°C for 3 hours, air quench to room temperature, keep at 500°C for 3 hours and then air cool to room temperature.
[0106] The resulting modified casting is marked as sample 5. The high chromium cast iron as-cast metallographic structure of sample 5 is as follows: Figure 3 As shown; the casting obtained without modification is marked as sample 6, and the high chromium cast iron as-cast metallographic structure of sample 6 is as shown Figure 4 As shown in the figure, it can be seen from the comparison between the two figures that the precipitated phase in sample 5 is more and denser, which also indicates that the hardness and strength of the obtained sample are higher.
[0107] The remaining examples 3 to 4 were cast according to the method described in application example 2, including a modification step; the samples obtained in examples 3 to 4 were marked as samples 7 to 8, and the samples obtained in comparative examples 1 to 4 were marked as samples 9 to 12. The hardness and impact toughness of the castings obtained from samples 1 to 13 (tested according to the description in "GB / T 229-2007 Charpy pendulum impact test method for metal materials") are shown in Table 1 below:
[0108] Table 1
[0109] sample Hardness(HRC) <![CDATA[Impact toughness (J / m 2 )]]> Sample 1 58 10.6 Sample 2 22 5.4 Sample 3 60 12.0 Sample 4 25 4.6 Sample 5 63 11.8 Sample 6 19 5.7 Sample 7 60 9.7 Sample 8 58 8.4 Sample 9 42 7.5 Sample 10 49 6.6 Sample 11 55 7.9 Sample 12 57 8.0
[0110] According to the test results, compared with samples 7 to 8, it can be seen that the content of each component of the modifier of sample 3 prepared in the present invention has the best effect and is the optimal content;
[0111] It can be seen from the comparison between Sample 3 and Samples 9-10 and Samples 11-12 that if any component of the modifier described in the present invention is deleted or replaced, although the total content remains unchanged, the hardness and impact toughness of the obtained sample are greatly reduced, indicating that the modifier provided by the present invention has the best effect achieved by its combination, in which each element component interacts with the elements in the high chromium cast iron, and none of them can be missing.
[0112] In addition, it should be noted that the heat treatment step described in the present invention is an essential step in the casting manufacturing process. The present invention has been tested to find that the heat treatment temperature provided is the most suitable temperature, which is most conducive to the modification of the high chromium cast iron by the modifier provided by the present invention, and is more conducive to the interaction between atoms, so that the resulting casting has finer grains, more and denser precipitated phases, and better performance.
[0113] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A modifier for high chromium cast iron, characterized in that: The high chromium cast iron modifier is composed of the following components by mass percentage: Fe-Si alloy 5% to 10%; Fe-Nb alloy 10%~15%; Fe-Ti alloy 10%~15%; The balance is mixed rare earth, wherein the mixed rare earth is cerium-rich mixed rare earth, wherein the weight percentage of Ce is 50% to 60%; Wherein, the mass percentage of Si in the Fe-Si alloy is 70% to 80%; The mass percentage of Nb in the Fe-Nb alloy is 50% to 65%; The mass percentage of Ti in the Fe-Ti alloy is 2% to 35%.
2. A high chromium cast iron subjected to composite modification treatment, characterized in that: The high chromium cast iron is modified by adding the modifier as claimed in claim 1 before melt pouring.
3. The high chromium cast iron according to claim 2, characterized in that: The addition amount of the modifier is 0.5% to 1.5% of the mass of the high chromium cast iron raw material.
4. The high chromium cast iron according to claim 2, characterized in that: The high chromium cast iron is composed of the following components in mass percentage before melt pouring: 2.5% to 3.2% C, 0.5% to 1.5% Si, 1.2% to 1.5% Mn, 0.7% to 1.0% Ni, 18% to 22% Cr, 0.4% to 0.8% Mo, and the balance is Fe.
5. The high chromium cast iron according to claim 2, characterized in that: The hardness of the casting prepared by using the high chromium cast iron is 58-63HRC; The impact toughness of the casting prepared by using the high chromium cast iron is 8-12 J / m 2 .
6. The high chromium cast iron according to claim 2, characterized in that: The microstructure of the casting prepared by using the high chromium cast iron is: eutectic M7C3 carbide and tempered martensite characterized by submicron-sized particle carbide precipitates.
7. A method for preparing high chromium cast iron according to any one of claims 2 to 6, characterized in that: The preparation method comprises the steps of batching, smelting, modification, pouring, mold opening, sample processing and heat treatment; Wherein, the modification treatment is to add the modifier as claimed in claim 1 to the melt obtained after smelting.
8. The preparation method according to claim 7, characterized in that: The heat treatment steps are: The casting obtained after sample processing is heated for the first time, kept warm, then quenched, cooled to room temperature, heated again, tempered, and air-cooled to room temperature; The temperature of the first addition and heat preservation is 950° C. to 1000° C., and the time is 2 h to 5 h; The reheating and tempering temperature is 450°C to 550°C, and the time is 2h to 6h; The room temperature is 25°C to 30°C.