A method for producing large-diameter modified polyvinyl alcohol monofilament
Through the heat storage and temperature regulation function of modified polyvinyl alcohol monofilament and urea microcapsule technology, the changes in seawater temperature and pollution problems in seaweed aquaculture are solved, and the stability of the seaweed growth environment and the protection of the seaweed environment are achieved.
Patent Information
- Application Number
- CN202310610263.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2023-04-07
- Filing Date
- 2023-05-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-29
AI Technical Summary
During the seaweed breeding process, seawater inorganic nitrogen pollution is severe, and changes in seawater temperature affect the growth of seaweed, resulting in a failure of breeding. The existing polyvinyl alcohol fibers require a large amount of fertilization and the introduction of foreign fibers, which affects the seawater ecology.
Modified polyvinyl alcohol monofilament is used to combine the technology of paraffin-urea-formaldehyde resin microcapsules and urea microcapsules to impart the polyvinyl alcohol monofilament heat storage and temperature regulation function, and release nutrients through urea microcapsules to reduce the amount of fertilizer applied and protect seawater. environment.
Effectively maintain the temperature stability of the seaweed growth environment, reduce inorganic nitrogen pollution in seaweed, reduce fertilization needs, protect seawater ecology, and improve the success rate of seaweed farming.
Smart Images

Figure BDA0004252245720000151
Abstract
Description
Technical Field
[0001] The invention relates to a production method of modified polyvinyl alcohol monofilament. Background Art
[0002] In nature, substances generally exist in solid, liquid, and gaseous states, and each state of a substance can be called a "phase state". When a substance exchanges heat with the external environment and reaches a certain "special temperature point", its physical state will change from one phase state to another. This phase change is called "phase change", and the special temperature point during the phase change is called "phase change temperature". Materials that can undergo phase change are called "phase change materials (Phase Change Materials)".
[0003] Wang Juan et al. pointed out in the article "Analysis of the Impact of Laver Farming on the Water Quality of Haizhou Bay": Through monitoring and analysis of the two laver farms in Liandao and Qingkou, it was found that laver farming has a great impact on the inorganic nitrogen concentration in seawater. During the laver farming net hanging period and seedling separation period, the inorganic nitrogen concentration in seawater showed a downward trend, and the inorganic nitrogen concentration in seawater increased sharply during the harvest period. The pollution index of inorganic nitrogen was greater than 1. In recent years, with the disorderly expansion of laver farming, the deterioration of seawater quality has intensified.
[0004] Polyvinyl alcohol is a polymer compound with good water solubility, biodegradability and UV resistance, and its application is becoming more and more extensive. Polyvinyl alcohol fiber is the most hygroscopic fiber among synthetic fibers, with strong acid and alkali resistance and strong adsorption. It is particularly suitable for the attachment and growth of seaweed spores. It is an irreplaceable fiber component in cultured mesh curtains. The fiber mixing ratio of domestic cultured mesh curtains is generally 50% polyethylene and 50% vinyl twisted yarn. Although the composition of vinyl yarn is the requirement for cultured seaweed, many fluffy fibers on the surface are easily mixed into laver products, which affects the quality of laver, and the yarn is prone to cause a large number of shell algae to reproduce. And it is troublesome to remove sludge and algae. The Japanese and Korean governments have banned the use of vinylon to cut yarn for seaweed cultivation, and recommend the use of nylon and polyvinyl alcohol coarse denier filaments. In China, polyvinyl alcohol coarse denier filaments have gradually been used to replace vinylon yarns, but the polyvinyl alcohol crude fibers currently used in China are all imported, and the price has remained high.
[0005] In the process of laver cultivation, it is difficult to control the amount of fertilizer due to the flow of seawater and the large sea area. In order to ensure the growth of laver, the amount of fertilizer applied during laver cultivation must be increased, far exceeding the amount required for laver growth, which directly leads to inorganic nitrogen pollution in seawater; at the same time, from late September to November, the seawater temperature is high, exceeding 25°C, which is not conducive to the growth of laver and easily causes large-scale seedling shedding, thus leading to cultivation failure. Summary of the invention
[0006] The purpose of the present invention is to provide a method for producing large-diameter modified polyvinyl alcohol monofilaments which are endowed with the function of heat storage and temperature regulation, and the modified polyvinyl alcohol monofilaments are coated with urea microcapsules to ensure the supply of nutrients to laver during the entire growth and cultivation process and have little pollution to seawater quality.
[0007] The technical solution of the present invention is:
[0008] A method for producing large-diameter modified polyvinyl alcohol monofilaments, characterized in that it comprises the following steps:
[0009] (I) Preparation of paraffin-urea-formaldehyde resin microcapsules
[0010] It mainly includes three stages: prepolymerization, emulsification and encapsulation;
[0011] Urea-formaldehyde resin is a high molecular polymer formed by the self-condensation of urea-formic acid prepolymer. First, formaldehyde reacts with the active hydrogen of the amino group in the urea molecule to form hydroxymethyl, and an addition reaction occurs. The product molecules of the addition reaction dehydrate to form a linear prepolymer. These linear low molecular weight prepolymers are soluble in water and can undergo a polycondensation reaction under the catalytic action of acid or alkali. The prepolymer molecules further remove small molecules (water, etc.) to form a non-water-soluble polycondensate with a cross-linked three-dimensional network structure, and the capsule core is coated to form a microcapsule;
[0012] (II) Preparation of paraffin microcapsule modified polyvinyl alcohol monofilament
[0013] PVA and paraffin microcapsules are added to a certain amount of DMSO, a certain amount of boric acid is added, dissolved and stirred evenly, and then left to stand for degassing to form a uniform spinning solution; the spinning solution is ejected from a spinneret, passes through an air layer and enters ice methanol to solidify, and then is stretched by air and then DMSO is extracted with methanol (100%) at room temperature to obtain primary PVA fibers; drying, and then stretching and shaping the primary PVA fibers in a heat pipe to obtain modified PVA monofilaments;
[0014] (III) Preparation of urea microcapsules
[0015] A certain amount of chitosan is dissolved in a glacial acetic acid (volume fraction is 1%) solution to prepare a chitosan solution with a concentration of 5-10%, and then a certain amount of urea is added, the chitosan-urea solution is used as the aqueous phase, and is placed in a water bath for preheating and dissolution; a liquid paraffin solution containing a certain amount of emulsifier Span80 is prepared as the oil phase, and is placed in a three-necked flask; the chitosan-urea solution is slowly dripped into the oil phase according to a certain proportion, and magnetic stirring is performed while dripping, and after the dripping is completed, the water bath emulsification is continued, and then the three-necked flask is quickly transferred to a refrigeration circulator, and glutaraldehyde (50%) is dripped to solidify and crosslink; after solidification and crosslinking, microcapsules are obtained by suction filtration, and finally the microcapsules are washed with isopropyl alcohol and petroleum ether alternately, and dried;
[0016] (IV) Urea microcapsule coating treatment of modified polyvinyl alcohol monofilament
[0017] A certain amount of urea microcapsules and emulsifier Span80 are evenly dispersed in distilled water to prepare a urea microcapsule solution, which is placed in a dipping and rolling tank; the prepared paraffin microcapsule modified polyvinyl alcohol monofilament is then passed through the dipping and rolling tank, dried in a hot air oven, passed through a drawing roller, and then rolled into a roll.
[0018] The invention adopts dry-wet spinning technology to produce large-diameter coarse-denier polyvinyl alcohol monofilaments; adopts microcapsule technology to modify the large-diameter polyvinyl alcohol monofilaments to obtain phase-change temperature-adjustable polyvinyl alcohol monofilaments capable of slowly releasing urea nutrients.
[0019] The invention firstly adopts a mixture of high and low temperature paraffin to modify the polyvinyl alcohol monofilament, so as to endow the polyvinyl alcohol monofilament with the function of heat storage and temperature regulation, and maintain the temperature between 20-28 DEG C, thereby ensuring that the laver will not be adversely affected in growth due to the change of seawater temperature, and ensuring the normal development of various nutrient elements of the laver; then, the modified polyvinyl alcohol monofilament is subjected to a coating treatment of urea microcapsules, thereby ensuring the supply of nutrient components of the laver in the whole growth and breeding process, without the need for additional large amounts of fertilizers, reducing the workload, and having little pollution to the seawater quality, thereby protecting the ecological environment of the seawater.
[0020] The present invention will be further described below in conjunction with the embodiments. DETAILED DESCRIPTION
[0021] Embodiment 1
[0022] Step 1 Preparation of paraffin-urea-formaldehyde resin microcapsules
[0023] Dissolve 20 parts of urea in 30 parts of formaldehyde aqueous solution, adjust the pH value of the mixed solution to 8 with triethanolamine, and react at a constant temperature of 70°C for 1 hour to prepare a urea-formaldehyde prepolymer for use; stir and mix OP-10 emulsifier and paraffin, wherein the emulsifier content is 20% of the paraffin, and the paraffin is liquid paraffin and n-octadecane, wherein the ratio of the two is 3:2, and then add distilled water, the ratio of distilled water to paraffin is 4, the emulsification temperature is 60°C, the rotation speed is 3000r / min, and the time is After 30 minutes, a stable emulsion is formed; the speed is reduced to 500r / min, the temperature is unchanged, and the prepolymer solution is slowly and uniformly added to the emulsion using a constant pressure dropping funnel. After the addition is completed, the reaction is carried out for 20 minutes; then the final pH value of the solution is adjusted to 3 with 10% citric acid, and the reaction is continued for 1 hour; then the temperature is raised to 90℃ and the reaction is kept warm for 2 hours; after the reaction is completed, the microcapsule emulsion is separated by vacuum filtration; the obtained filter cake is washed with petroleum ether and 60℃ deionized water in turn, and dried to obtain white powder microcapsules.
[0024] Step 2 Preparation of paraffin microcapsule modified polyvinyl alcohol monofilament
[0025] After washing the low molecular weight polymer with 40℃ distilled water, PVA is filtered and dried at 60℃ to remove water. When the mass does not change, it is added to a certain amount of DMSO together with paraffin microcapsules, wherein the mass fraction of PVA is 25%, the mass fraction of paraffin microcapsules is 1%, and a certain amount of boric acid is added, the mass fraction of boric acid is 0.5%, dissolved and stirred evenly at 80℃, and after standing and degassing, a uniform spinning solution is formed. The prepared spinning solution is filtered through a 200-mesh filter screen with nitrogen, and then sprayed from a 6-hole spinneret with a diameter of 0.20mm at 80℃, and enters ice methanol for coagulation through an air layer of about 5cm. The coagulation liquid temperature is -20℃, and the spinneret stretching ratio is -50 times. Then, after air stretching, DMSO is extracted with methanol (100%) at room temperature, and the air stretching ratio is 2.5 times to obtain the primary PVA fiber. After drying, the nascent PVA fiber is stretched in a hot tube at 220° C. with a heat stretching ratio of 8 times, and then subjected to a shaping treatment to finally obtain a modified PVA monofilament.
[0026] Step 3 Preparation of urea microcapsules
[0027] A certain amount of chitosan was dissolved in glacial acetic acid (volume fraction 1%) solution to prepare a chitosan solution with a concentration of 5%, and then a certain amount of urea was added. The chitosan-urea solution was used as the aqueous phase and preheated in a water bath at 60°C to dissolve. A liquid paraffin solution containing a certain amount of emulsifier Span80 was prepared as the oil phase, wherein the mass fraction of the emulsifier Span80 was 2%, and placed in a three-necked flask. According to a certain ratio, the oil-liquid ratio is 5:1, and the chitosan-urea solution is slowly added to the oil phase, while magnetic stirring (500r / min speed, the temperature of the water bath is set to 60°C, and the water bath emulsification is continued for 10 minutes after the addition is completed, and then the three-necked flask is quickly transferred to a refrigeration circulator, and after continuing to stir in an ice water bath at 0°C for 20 minutes, 0.5% volume fraction of glutaraldehyde (50%) is added to solidify and cross-link for 15 minutes. After solidification and cross-linking, microcapsules are obtained by suction filtration, and finally the microcapsules are washed 3 times with isopropanol and petroleum ether alternately, and placed in an oven for drying. The fertilizer loading and encapsulation efficiency of the urea microcapsule slow-release fertilizer prepared under different conditions are determined. The particle size range is 100-150μm.
[0028] Step 4: Urea microcapsule coating treatment to modify polyvinyl alcohol monofilament
[0029] A certain amount of urea microcapsules and emulsifiers are evenly dispersed in distilled water to prepare urea microcapsule solution, which is placed in a padding tank. The prepared paraffin microcapsule modified polyvinyl alcohol monofilament is then passed through the padding tank, the speed of the drafting machine before and after the padding tank is 50m / min, the circulation speed of the urea microcapsule solution in the padding tank is 10ml / min, the length of the padding tank is 3m, and then dried in a hot air oven with a setting temperature of 100℃, and then passed through the third drafting roller at a speed of 50m / min, and then collected into a roll.
[0030] Embodiment 2
[0031] The steps are the same as in Example 1;
[0032] Step 2 Preparation of paraffin microcapsule modified polyvinyl alcohol monofilament
[0033] After washing the low molecular weight polymer with 40℃ distilled water, PVA is filtered and dried at 60℃ to remove water. When the mass does not change, it is added to a certain amount of DMSO together with paraffin microcapsules, wherein the mass fraction of PVA is 25%, the mass fraction of paraffin microcapsules is 6%, and a certain amount of boric acid is added, the mass fraction of boric acid is 0.5%, and dissolved and stirred at 80℃. After standing and degassing, a uniform spinning solution is formed. The prepared spinning solution is filtered through a 200-mesh filter screen with nitrogen, and then sprayed from a 6-hole spinneret with a diameter of 0.20mm at 80℃, and enters ice methanol through an air layer of about 5cm to solidify. The coagulation liquid temperature is -20℃, and the spinneret stretching ratio is -50 times. Then, after air stretching, DMSO is extracted with methanol (100%) at room temperature, and the air stretching ratio is 2.5 times to obtain the nascent PVA fiber. After drying, the nascent PVA fiber is stretched in a hot tube at 220° C. with a heat stretching ratio of 8 times, and then subjected to a shaping treatment to finally obtain a modified PVA monofilament.
[0034] Steps three and four are the same as in Example 1.
[0035] Embodiment 3
[0036] The steps are the same as in Example 1;
[0037] Step 2 Step 2 Preparation of paraffin microcapsule modified polyvinyl alcohol monofilament
[0038] After washing the low molecular weight polymer with 40℃ distilled water, PVA is filtered and dried at 60℃ to remove water. When the mass does not change, it is added to a certain amount of DMSO together with paraffin microcapsules, wherein the mass fraction of PVA is 25%, the mass fraction of paraffin microcapsules is 10%, and a certain amount of boric acid is added, the mass fraction of boric acid is 0.5%, and dissolved and stirred evenly at 80℃. After standing and degassing, a uniform spinning solution is formed. The prepared spinning solution is filtered through a 200-mesh filter screen with nitrogen, and then ejected from a 6-hole spinneret with a diameter of 0.20mm at 80℃, and enters ice methanol for coagulation through an air layer of about 5cm. The coagulation liquid temperature is -20℃, and the spinneret stretching ratio is -50 times. Then, after air stretching, DMSO is extracted with methanol (100%) at room temperature, and the air stretching ratio is 2.5 times to obtain the primary PVA fiber. After drying, the nascent PVA fiber is stretched in a hot tube at 220° C. with a heat stretching ratio of 8 times, and then subjected to a shaping treatment to finally obtain a modified PVA monofilament.
[0039] Steps three and four are the same as in Example 1.
[0040] Embodiment 4
[0041] The steps are the same as in Example 1;
[0042] Step 2 is the same as in Example 2;
[0043] Step 3 Preparation of urea microcapsules
[0044] A certain amount of chitosan was dissolved in glacial acetic acid (volume fraction 1%) solution to prepare a chitosan solution with a concentration of 5-10%, and then a certain amount of urea was added. The chitosan-urea solution was used as the aqueous phase and preheated in a water bath at 60°C to dissolve. A liquid paraffin solution containing a certain amount of emulsifier Span80 was prepared as the oil phase, wherein the mass fraction of the emulsifier Span80 was 4%, and placed in a three-necked flask. According to a certain ratio, the oil-liquid ratio is 5:1, and the chitosan-urea solution is slowly added to the oil phase, while magnetic stirring (500r / min speed, the temperature of the water bath is set to 60°C, and the water bath emulsification is continued for 10 minutes after the addition is completed, and then the three-necked flask is quickly transferred to a refrigeration circulator, and after continuing to stir in an ice water bath at 0°C for 20 minutes, 0.5% volume fraction of glutaraldehyde (50%) is added to solidify and cross-link for 15 minutes. After solidification and cross-linking, microcapsules are obtained by suction filtration, and finally the microcapsules are washed 3 times with isopropanol and petroleum ether alternately, and placed in an oven for drying. The fertilizer loading and encapsulation efficiency of the urea microcapsule slow-release fertilizer prepared under different conditions are determined. The particle size range is 100-150μm.
[0045] Step 4 is the same as in Example 1.
[0046] Embodiment 5
[0047] The steps are the same as in Example 1;
[0048] Step 2 is the same as in Example 2;
[0049] Step 3 Preparation of urea microcapsules
[0050] A certain amount of chitosan was dissolved in glacial acetic acid (volume fraction 1%) solution to prepare a chitosan solution with a concentration of 5-10%, and then a certain amount of urea was added. The chitosan-urea solution was used as the aqueous phase and preheated in a water bath at 60°C to dissolve. A liquid paraffin solution containing a certain amount of emulsifier Span80 was prepared as the oil phase, wherein the mass fraction of the emulsifier Span80 was 6%, and placed in a three-necked flask. According to a certain ratio, the oil-liquid ratio is 5:1, and the chitosan-urea solution is slowly added to the oil phase, while magnetic stirring (500r / min speed, the temperature of the water bath is set to 60°C, and the water bath emulsification is continued for 10 minutes after the addition is completed, and then the three-necked flask is quickly transferred to a refrigeration circulator, and after continuing to stir in an ice water bath at 0°C for 20 minutes, 0.5% volume fraction of glutaraldehyde (50%) is added to solidify and cross-link for 15 minutes. After solidification and cross-linking, microcapsules are obtained by suction filtration, and finally the microcapsules are washed 3 times with isopropanol and petroleum ether alternately, and placed in an oven for drying. The fertilizer loading and encapsulation efficiency of the urea microcapsule slow-release fertilizer prepared under different conditions are determined. The particle size range is 100-150μm.
[0051] Step 4 is the same as in Example 1.
[0052] Embodiment 6
[0053] The steps are the same as in Example 1;
[0054] Step 2 is the same as in Example 2;
[0055] Step 3 Preparation of urea microcapsules
[0056] A certain amount of chitosan was dissolved in glacial acetic acid (volume fraction 1%) solution to prepare a chitosan solution with a concentration of 5-10%, and then a certain amount of urea was added. The chitosan-urea solution was used as the aqueous phase and preheated in a water bath at 60°C to dissolve. A liquid paraffin solution containing a certain amount of emulsifier Span80 was prepared as the oil phase, wherein the mass fraction of the emulsifier Span80 was 6%, and placed in a three-necked flask. According to a certain ratio, the oil-liquid ratio is 6:1, and the chitosan-urea solution is slowly added to the oil phase, while magnetic stirring (500r / min speed, the temperature of the water bath is set to 60°C, and the water bath emulsification is continued for 10 minutes after the addition is completed, and then the three-necked flask is quickly transferred to a refrigeration circulator, and after continuing to stir in an ice water bath at 0°C for 20 minutes, 0.5% volume fraction of glutaraldehyde (50%) is added to solidify and cross-link for 15 minutes. After solidification and cross-linking, microcapsules are obtained by suction filtration, and finally the microcapsules are washed 3 times with isopropanol and petroleum ether alternately, and placed in an oven for drying. The fertilizer loading and encapsulation efficiency of the urea microcapsule slow-release fertilizer prepared under different conditions are determined. The particle size range is 100-150μm.
[0057] Step 4 is the same as in Example 1.
[0058] Embodiment 7
[0059] The steps are the same as in Example 1;
[0060] Step 2 is the same as in Example 2;
[0061] Step 3 Preparation of urea microcapsules
[0062] A certain amount of chitosan was dissolved in glacial acetic acid (volume fraction 1%) solution to prepare a chitosan solution with a concentration of 5-10%, and then a certain amount of urea was added. The chitosan-urea solution was used as the aqueous phase and preheated in a water bath at 60°C to dissolve. A liquid paraffin solution containing a certain amount of emulsifier Span80 was prepared as the oil phase, wherein the mass fraction of the emulsifier Span80 was 6%, and placed in a three-necked flask. According to a certain ratio, the oil-liquid ratio is 8:1, and the chitosan-urea solution is slowly added to the oil phase, while magnetic stirring (500r / min speed, the temperature of the water bath is set to 60°C, and the water bath emulsification is continued for 10 minutes after the addition is completed, and then the three-necked flask is quickly transferred to a refrigeration circulator, and after continuing to stir in an ice water bath at 0°C for 20 minutes, 0.5% glutaraldehyde (50%) is added dropwise for curing and cross-linking for 15 minutes. After curing and cross-linking, microcapsules are obtained by suction filtration, and finally the microcapsules are washed 3 times with isopropanol and petroleum ether alternately, and placed in an oven for drying. The fertilizer loading and encapsulation efficiency of the urea microcapsule slow-release fertilizer prepared under different conditions are determined. The particle size range is 100-150μm.
[0063] Step 4 is the same as in Example 1.
[0064] Embodiment 8
[0065] The steps are the same as in Example 1;
[0066] Step 2 is the same as in Example 2;
[0067] Step 3 Preparation of urea microcapsules
[0068] A certain amount of chitosan was dissolved in glacial acetic acid (volume fraction 1%) solution to prepare a chitosan solution with a concentration of 5-10%, and then a certain amount of urea was added. The chitosan-urea solution was used as the aqueous phase and preheated in a water bath at 60°C to dissolve. A liquid paraffin solution containing a certain amount of emulsifier Span80 was prepared as the oil phase, wherein the mass fraction of the emulsifier Span80 was 6%, and placed in a three-necked flask. According to a certain ratio, the oil-liquid ratio is 6:1, and the chitosan-urea solution is slowly added to the oil phase, while magnetic stirring (500r / min speed, the temperature of the water bath is set to 60°C, and the water bath emulsification is continued for 10 minutes after the addition is completed, and then the three-necked flask is quickly transferred to a refrigeration circulator, and after continuing to stir in an ice water bath at 0°C for 20 minutes, 1.0% glutaraldehyde (50%) is added dropwise for curing and cross-linking for 15 minutes. After curing and cross-linking, microcapsules are obtained by suction filtration, and finally the microcapsules are washed 3 times with isopropanol and petroleum ether alternately, and placed in an oven for drying. The fertilizer loading and encapsulation efficiency of the urea microcapsule slow-release fertilizer prepared under different conditions are determined. The particle size range is 100-150μm.
[0069] Step 4 is the same as in Example 1.
[0070] Embodiment 9
[0071] The steps are the same as in Example 1;
[0072] Step 2 is the same as in Example 2;
[0073] Step 3 Preparation of urea microcapsules
[0074] A certain amount of chitosan was dissolved in glacial acetic acid (volume fraction 1%) solution to prepare a chitosan solution with a concentration of 5-10%, and then a certain amount of urea was added. The chitosan-urea solution was used as the aqueous phase and preheated in a water bath at 60°C to dissolve. A liquid paraffin solution containing a certain amount of emulsifier Span80 was prepared as the oil phase, wherein the mass fraction of the emulsifier Span80 was 6%, and placed in a three-necked flask. According to a certain ratio, the oil-liquid ratio is 6:1, and the chitosan-urea solution is slowly added to the oil phase, while magnetic stirring (500r / min speed, the temperature of the water bath is set to 60°C, and the water bath emulsification is continued for 10 minutes after the addition is completed, and then the three-necked flask is quickly transferred to a refrigeration circulator, and after continuing to stir in an ice water bath at 0°C for 20 minutes, 3.5% glutaraldehyde (50%) is added dropwise for curing and cross-linking for 15 minutes. After curing and cross-linking, microcapsules are obtained by suction filtration, and finally the microcapsules are washed 3 times with isopropanol and petroleum ether alternately, and placed in an oven for drying. The fertilizer loading and encapsulation efficiency of the urea microcapsule slow-release fertilizer prepared under different conditions are determined. The particle size range is 100-150μm.
[0075] Step 4 is the same as in Example 1.
[0076] Embodiment 10
[0077] The steps are the same as in Example 1;
[0078] Step 2 is the same as in Example 2;
[0079] Step 3 Preparation of urea microcapsules
[0080] A certain amount of chitosan was dissolved in glacial acetic acid (volume fraction 1%) solution to prepare a chitosan solution with a concentration of 5-10%, and then a certain amount of urea was added. The chitosan-urea solution was used as the aqueous phase and preheated in a water bath at 60°C to dissolve. A liquid paraffin solution containing a certain amount of emulsifier Span80 was prepared as the oil phase, wherein the mass fraction of the emulsifier Span80 was 6%, and placed in a three-necked flask. According to a certain ratio, the oil-liquid ratio is 6:1, and the chitosan-urea solution is slowly added to the oil phase, while magnetic stirring (500r / min speed, the temperature of the water bath is set to 60°C, and the water bath emulsification is continued for 10 minutes after the addition is completed, and then the three-necked flask is quickly transferred to a refrigeration circulator, and after continuing to stir in an ice water bath at 0°C for 20 minutes, 0.5% glutaraldehyde (50%) is added dropwise for curing and cross-linking for 45 minutes. After curing and cross-linking, microcapsules are obtained by suction filtration, and finally the microcapsules are washed 3 times with isopropanol and petroleum ether alternately, and placed in an oven for drying. The fertilizer loading and encapsulation efficiency of the urea microcapsule slow-release fertilizer prepared under different conditions are determined. The particle size range is 100-150μm.
[0081] Step 4 is the same as in Example 1.
[0082] Embodiment 11
[0083] The steps are the same as in Example 1;
[0084] Step 2 is the same as in Example 2;
[0085] Step 3 Preparation of urea microcapsules
[0086] A certain amount of chitosan was dissolved in glacial acetic acid (volume fraction 1%) solution to prepare a chitosan solution with a concentration of 5-10%, and then a certain amount of urea was added. The chitosan-urea solution was used as the aqueous phase and preheated in a water bath at 60°C to dissolve. A liquid paraffin solution containing a certain amount of emulsifier Span80 was prepared as the oil phase, wherein the mass fraction of the emulsifier Span80 was 6%, and placed in a three-necked flask. According to a certain ratio, the oil-liquid ratio is 6:1, and the chitosan-urea solution is slowly added to the oil phase, while magnetic stirring (500r / min speed, the temperature of the water bath is set to 60°C, and the water bath emulsification is continued for 10 minutes after the addition is completed, and then the three-necked flask is quickly transferred to a refrigeration circulator, and after continuing to stir in an ice water bath at 0°C for 20 minutes, 0.5% glutaraldehyde (50%) is added dropwise for curing and cross-linking for 60 minutes. After curing and cross-linking, microcapsules are obtained by suction filtration, and finally the microcapsules are washed 3 times with isopropanol and petroleum ether alternately, and placed in an oven for drying. The fertilizer loading and encapsulation efficiency of the urea microcapsule slow-release fertilizer prepared under different conditions are measured. The particle size range is 100-150μm.
[0087] Step 4 is the same as in Example 1.
[0088] Comparative Example 1
[0089] The difference from Example 10 is that the mass fraction of the paraffin microcapsules in step 2 is 0.5%.
[0090] Comparative Example 2
[0091] The difference from Example 10 is that the mass fraction of the paraffin microcapsules in step 2 is 15%.
[0092] Comparative Example 3
[0093] The difference from Example 10 is that the mass fraction of the emulsifier Span80 in step 3 is 1%.
[0094] Comparative Example 4
[0095] The difference from Example 10 is that the mass fraction of the emulsifier Span80 in step 3 is 7%.
[0096] Comparative Example 5
[0097] The difference from Example 10 is that the oil-to-liquid ratio in step 3 is 4:1.
[0098] Comparative Example 6
[0099] The difference from Example 10 is that the oil-to-liquid ratio in step 3 is 9:1.
[0100] Comparative Example 7
[0101] The difference from Example 10 is that in step 3, 0.25% by volume of glutaraldehyde (50%) is added dropwise for curing and cross-linking.
[0102] Comparative Example 8
[0103] The difference from Example 10 is that in step 3, 4.0% by volume of glutaraldehyde (50%) is added dropwise for curing and cross-linking.
[0104] Comparative Example 9
[0105] The difference from Example 10 is that step 3 is cross-linked and cured for 10 minutes.
[0106] Comparative Example 10
[0107] The difference from Example 10 is that step 3 is cured and cross-linked for 70 minutes.
[0108]
[0109]
[0110] From the above table, we can see that when blended with polyvinyl alcohol, when the addition amount of paraffin microcapsules is 6%, the phase change enthalpy value is the largest and the heat storage and temperature regulation function is the best. When the mass fraction of emulsifier is 6, the oil-liquid ratio is 6:1, the mass fraction of curing agent is 0.5%, and the curing and cross-linking time is 45 minutes, the chitosan-urea sustained-release microcapsules have the highest fertilizer loading capacity and the highest 48h urea release.
[0111] Test method:
[0112] Test of phase change enthalpy
[0113] Take 4-6 mg of paraffin microcapsules and use differential scanning calorimeter to test the thermal enthalpy of the single fiber. Test conditions: the test temperature range is -20℃-100℃, the heating and cooling rate is 10℃ / min, and nitrogen protection is used.
[0114] Second fertilizer loading test
[0115] The prepared microcapsules are placed in an oven to be fully dried, and then ground into powder. Accurately weigh 0.100g of microcapsules and soak them in 50mL of distilled water. After the microcapsules are allowed to stand and soak for a certain period of time, they are filtered. 10mL of the filtrate is placed in a 50mL volumetric flask, and 10mL of the developer is added to the volumetric flask, and the volume is fixed with distilled water. Using urea standard solution as the standard, a UV-visible spectrophotometer is used to set the band to 420nm to determine the nitrogen content in the solution. The concentration measured by the UV-visible spectrophotometer is multiplied by a certain dilution factor to obtain the urea content in the microcapsules. The fertilizer loading calculation formula is as follows:
[0116] Fertilizer loading = (W c / W m )*100%
[0117] Where: W c is the content of urea encapsulated in the microcapsules, W m is the mass of microcapsules weighed
[0118] 3.48h urea release test
[0119] A certain mass fraction of urea microcapsules is mixed with a certain volume of distilled water to form a solution, which is allowed to stand at room temperature. The nitrogen content in the supernatant is removed at regular intervals and measured.
Claims
1. A method for producing large-diameter modified polyvinyl alcohol monofilaments, Its characteristics are: The following steps are involved: Step 1 Preparation of paraffin-urea-formaldehyde resin microcapsules Dissolve 20 parts of urea in 30 parts of formaldehyde aqueous solution, and adjust the pH value of the mixed solution to 8 with triethanolamine, and react at a constant temperature of 70°C for 1 hour to prepare urea-formaldehyde prepolymer for standby use; stir and mix OP-10 emulsifier and paraffin, wherein the emulsifier content is 20% of the paraffin, and the paraffin is liquid paraffin and n-octadecane, and the ratio of the two is 3:2, and then add distilled water, the ratio of distilled water to paraffin is 4, the emulsification temperature is 60°C, the speed is 3000r / min, and the time is 30min to form a stable emulsion; reduce the speed to 500r / min, keep the temperature unchanged, and slowly and uniformly add the prepolymer solution to the emulsion with a constant pressure dropping funnel, and react for 20min after the addition is completed; Then, the final pH value of the solution was adjusted to 3 with 10% citric acid, and the reaction was continued for 1 hour; then, the temperature was raised to 90°C and the reaction was kept for 2 hours; after the reaction was completed, the microcapsule emulsion was separated by vacuum filtration; the obtained filter cake was washed with petroleum ether and 60°C deionized water in turn, and dried to obtain white powder microcapsules; Step 2 Preparation of paraffin microcapsule modified polyvinyl alcohol monofilament After washing the low molecular weight polymer with 40℃ distilled water, PVA was filtered and dried at 60℃ to remove water. When the mass did not change, it was added to a certain amount of DMSO together with paraffin microcapsules, wherein the mass fraction of PVA was 25%, the mass fraction of paraffin microcapsules was 6%, and a certain amount of boric acid was added, the mass fraction of boric acid was 0.5%, dissolved and stirred evenly at 80℃, and after standing and degassing, a uniform spinning solution was formed; the prepared spinning solution was filtered through a 200-mesh filter with nitrogen, and then heated at 80℃ for 2 hours. The fibers were ejected from a 6-hole spinneret with a diameter of 0.20 mm at 0°C, and solidified in ice methanol after passing through a 5 cm air layer. The solidification liquid temperature was -20°C, and the spinneret stretching ratio was -50 times. After being air stretched, DMSO was extracted with 100% methanol at room temperature. The air stretching ratio was 2.5 times to obtain primary PVA fibers. The fibers were dried, and then stretched in a hot tube at 220°C. The heat stretching ratio was 8 times. The fibers were then shaped to obtain modified PVA monofilaments. Step 3 Preparation of urea microcapsules A certain amount of chitosan was dissolved in a 1% volume fraction glacial acetic acid solution to prepare a chitosan solution with a concentration of 5-10%, and then a certain amount of urea was added. The chitosan-urea solution was used as the aqueous phase and was placed in a 60°C water bath for preheating and dissolution; a liquid paraffin solution containing a certain amount of emulsifier Span80 was prepared as the oil phase, wherein the mass fraction of the emulsifier Span80 was 6%, and was placed in a three-necked flask; the chitosan-urea solution was slowly dripped into the oil phase according to a certain proportion, with an oil-liquid ratio of 6:1, and magnetic stirring was performed while dripping, with a speed of 500 r / min and the temperature of the water bath set to 60°C. After the dripping was completed, the water bath emulsification was continued for 10 min, and then the three-necked flask was quickly transferred to a refrigeration circulator and continued to stir in an ice water bath at 0°C for 20 min. After that, 50% glutaraldehyde with a volume fraction of 0.5% was added dropwise for curing and cross-linking for 45 minutes; after curing and cross-linking, microcapsules were obtained by filtration, and finally the microcapsules were washed with isopropanol and petroleum ether alternately for 3 times, and then placed in an oven for drying; the fertilizer loading and encapsulation efficiency of the urea microcapsule slow-release fertilizer prepared under different conditions were determined; the particle size range was 100-150μm; Step 4: Urea microcapsule coating treatment to modify polyvinyl alcohol monofilament A certain amount of urea microcapsules and emulsifier are uniformly dispersed in distilled water to prepare a urea microcapsule solution, which is then placed in a padding tank; The prepared paraffin microcapsule modified polyvinyl alcohol monofilament is then passed through a dipping tank, the speed of the drawing machine before and after the dipping tank is 50m / min, the circulation flow rate of the urea microcapsule solution in the dipping tank is 10ml / min, the length of the dipping tank is 3m, and then dried in a hot air oven with the temperature set at 100°C, and then passed through a third drawing roller at a speed of 50m / min, and then the wire is collected into a roll.