A construction method for a rolling-resistant, wear-resistant and corrosion-resistant coating material for a heavy-load deck
By using a composite coating system of anti-corrosion primer, wear-resistant intermediate paint and wear-resistant topcoat on the heavy-duty deck of the ship, combined with surface treatment and specific coating processes, the problem of ship decks in rolling and seawater environments is solved It reduces wear and corrosion problems, improves rolling resistance and wear resistance, extends coating life and reduces maintenance costs.
Patent Information
- Application Number
- CN202310731979.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-20
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-06-20
AI Technical Summary
Heavy-duty decks of ships are prone to wear and corrosion under long-term rolling and seawater environments. Existing construction methods of rolling-resistant coating materials have shortcomings and are difficult to meet the increasingly stringent coating environment requirements.
It adopts three coating compound systems of anti-corrosion primer, wear-resistant middle layer paint and wear-resistant topcoat. Through surface treatment, double-layer coating of anti-corrosion primer, multi-layer trowel coating and silk screen laying of the wear-resistant middle layer, The aggregate spreading process forms a high-performance anti-rolling, wear-resistant and anti-corrosion coating material.
Significantly improves the deck's crushing resistance, wear resistance, impact resistance, media resistance and corrosion resistance, extends the service life of the coating material, reduces maintenance costs, and meets the requirements of the ship's long-term transportation of large hovercraft and heavy tracked vehicles. need.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coating construction for heavy-load decks, and more particularly to a construction method of a rolling-resistant, wear-resistant and corrosion-resistant coating material for heavy-load decks. Background Art
[0002] Dock ships, amphibious ships, heavy trestle ships and other ships are responsible for the loading and transfer of heavy tracked vehicles and wheeled vehicles. Their docks, large cabins, vehicle warehouses, driving channels, anchor chain lockers, etc. are loaded with large hovercraft and heavy tracked vehicles. The operating deck is subjected to the combined effects of long-term rolling of heavy loads of vehicles and alternating dry and wet environments of seawater. Ordinary protective coatings are very easy to wear and fall off, which in turn causes corrosion of the metal substrate. The use of rolling-resistant, wear-resistant and anti-corrosion coating materials can significantly improve the rolling resistance of the deck, effectively reduce the later maintenance costs, improve the loading and transfer efficiency of ships, and thus increase the ship's sailing rate.
[0003] In recent years, new amphibious ships, dock ships, and heavy-duty trestle ships have been gradually put into use in shipping. The loading and transfer forces are gradually shifting from light wheeled vehicles to heavy tracked vehicles, and the demand for heavy-duty deck anti-rolling and wear-resistant protective coatings is growing. At the same time, the research and development of anti-rolling coating materials has also made positive progress accordingly. However, the construction method of anti-rolling, wear-resistant, and anti-corrosion coating materials is still a shortcoming. Therefore, the development of new construction methods for anti-rolling, wear-resistant, and anti-corrosion coating materials for heavy-duty decks of ships to meet the increasingly stringent coating environment requirements is an important direction in my country's current ship coating field. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a construction method of a rolling-resistant, wear-resistant and anti-corrosion coating material for heavy-load decks. The construction method of the present invention can significantly improve the performance of the rolling-resistant, wear-resistant and anti-corrosion coating material for heavy-load decks such as large cabins, dock cabins, vehicle garages, and driving passages of dock ships, amphibious ships, heavy trestle ships, etc., effectively prevent the wear and damage to the working deck caused by long-term rolling of heavy tracked vehicles and wheeled vehicles, improve the loading and transportation efficiency of ships, reduce maintenance costs, and extend service life.
[0005] Specifically, the present invention provides a construction method of a rolling-resistant, wear-resistant and corrosion-resistant coating material for a heavy-load deck, the construction method comprising the following steps:
[0006] S1. Surface treatment of metal substrates: remove welding slag, oil stains, dust and rust from the surface of metal substrates;
[0007] S2, coating of anti-corrosion primer, coating the surface of the metal substrate treated in step S1 with anti-corrosion primer, the total dry film thickness of the anti-corrosion primer being 95 to 105 μm;
[0008] S3. Coating of wear-resistant intermediate layer
[0009] Applying a wear-resistant intermediate layer on the anti-corrosion primer applied in step S2, wherein the wear-resistant intermediate layer is provided with a wear-resistant wire mesh and wear-resistant aggregate, the wear-resistant wire mesh is evenly distributed at the bottom of the wear-resistant intermediate layer, and the wear-resistant aggregate is evenly distributed in the wear-resistant intermediate layer;
[0010] S4, applying a wear-resistant topcoat, applying a wear-resistant topcoat on the surface of the wear-resistant intermediate layer applied in step S3, the total dry film thickness of the wear-resistant topcoat being 95-105 μm.
[0011] Furthermore, in step S1, the substrate of the heavy-duty deck is mainly a metal substrate, and is mainly made of steel or aluminum. When treating the surface of the metal substrate, the treatment methods of substrates with different usage levels or substrates in different parts should also be different. For example:
[0012] For substrates that have been in contact with seawater, they must be rinsed with fresh water first, and the water-logged areas must be blown dry. Then the substrate must be sandblasted, shot blasted, or electrically derusted to Sa2.5, or manually derusted to St3.
[0013] For new substrates, directly perform sandblasting, shot blasting or electric rust removal to Sa2.5 level, or manual rust removal to St3 level;
[0014] For substrates coated with shop primer, secondary rust removal shall be performed on the damaged and / or rusted areas of the paint film to Sa2.5 or St3 level;
[0015] For the substrate of the shop primer that has produced zinc salt, the zinc salt should be removed by spraying or high-pressure fresh water, and then the substrate should be sandblasted, shot blasted or electrically derusted to Sa2.5 level, or manually derusted to St3 level;
[0016] For the surface of welds or burned parts, sandblasting, shot blasting or electric rust removal to Sa2.5 level, or manual rust removal to St3 level;
[0017] After the above substrates or parts are polished, the debris needs to be cleaned up and the surface needs to be wiped clean with a rag dipped in epoxy thinner to more thoroughly clean the fine dust and rust caused by polishing.
[0018] Furthermore, in step S2, the coating method of the anticorrosive primer is:
[0019] The anti-corrosion primer must be applied to the surface of the metal substrate within 8 hours after the surface treatment of the metal substrate is completed. Use a brush dipped in paint to apply to the weld area, and then roll or spray it on the surface of the substrate. The anti-corrosion primer needs to be applied twice. After the first coat of anti-corrosion primer is completely dry, the second coat of anti-corrosion primer is applied. The coating methods of the first and second coats of anti-corrosion primer are the same. The total dry film thickness of the anti-corrosion primer is 95-105μm.
[0020] Preferably, the anticorrosive primer comprises an anticorrosive primer main material and an anticorrosive primer curing agent. More preferably, the anticorrosive primer comprises an anticorrosive primer main material, an anticorrosive primer curing agent and an anticorrosive primer diluent.
[0021] Preferably, the main ingredient of the anti-corrosion primer is a mixture of epoxy resin, mica iron oxide, mica powder, defoamer, wetting dispersant and diluent; the anti-corrosion primer curing agent is a modified alicyclic amine curing agent; the anti-corrosion primer diluent is an organic solvent; more preferably xylene. The anti-corrosion primer diluent can reduce the viscosity of the paint and facilitate coating.
[0022] Preferably, the preparation method of the anticorrosive primer is:
[0023] Add the anti-corrosion primer curing agent and or without the anti-corrosion primer thinner to the main material of the anti-corrosion primer, stir for 3 to 5 minutes, and mature for 15 to 20 minutes before painting.
[0024] Preferably, the mass ratio of the anticorrosive primer main material to the anticorrosive primer curing agent is 3:1 to 5:1, and the amount of the anticorrosive primer diluent is less than 10% of the amount of the anticorrosive primer main material.
[0025] Furthermore, in step S3, before the wear-resistant intermediate layer is coated, the mooring holes and the deck equipment area need to be separated by rubber strips to prevent the wear-resistant intermediate layer material from penetrating into the holes.
[0026] Specifically, the coating method of the wear-resistant intermediate layer is:
[0027] On the surface of the anti-corrosion primer, apply the first coat of wear-resistant intermediate layer paint with a width of 1.1-1.2m and a thickness of 1.5-1.6mm at intervals of 25-30cm, press it into the wear-resistant wire mesh, and after the first coat of wear-resistant intermediate layer paint is completely dry, apply the second coat of wear-resistant intermediate layer paint on the entire area of the anti-corrosion primer, and evenly spread the wear-resistant aggregate at the same time. After the second coat of wear-resistant intermediate layer paint is completely dry, apply the third coat of wear-resistant intermediate layer paint on top of the second coat of wear-resistant intermediate layer paint, and evenly spread the wear-resistant aggregate at the same time.
[0028] More specifically, the coating method of the wear-resistant intermediate layer is:
[0029] At intervals of 25 to 30 cm, evenly trowel the surface of the anti-corrosion primer with a first wear-resistant intermediate layer paint of 1.1 to 1.2 m width and 1.5 to 1.6 mm thickness, lay the wear-resistant wire mesh on the first wear-resistant intermediate layer paint, and cover it with a plastic sheet of 1 to 1.2 m width, compact the wear-resistant wire mesh with the plastic sheet, and evenly press the wear-resistant wire mesh into the first wear-resistant intermediate layer paint, squeeze out the air between the plastic sheet and the first wear-resistant intermediate layer paint, and after the first wear-resistant intermediate layer paint is completely dry, remove the covering plastic sheet, and polish and remove the protruding and / or loosely adhered wear-resistant wire mesh. Then apply the second wear-resistant intermediate layer paint on the entire area of the anti-corrosion primer, and evenly spread the wear-resistant aggregate at the same time. Use a defoaming roller to roll the surface of the second wear-resistant intermediate layer paint with the wear-resistant aggregate evenly. After the second wear-resistant intermediate layer paint is completely dry, use an angle grinder to grind off the loosely adhered and / or accumulated wear-resistant aggregate. After cleaning, apply the third wear-resistant intermediate layer paint on the second wear-resistant intermediate layer paint. The coating method of the third wear-resistant intermediate layer paint is the same as that of the second wear-resistant intermediate layer paint. The total dry film thickness of the wear-resistant intermediate layer is 3.5 to 3.7 mm.
[0030] Preferably, the plastic sheet is made of PE material.
[0031] Preferably, the amount of wear-resistant aggregate spread in the second wear-resistant intermediate layer of paint is 1.5-2 kg / m 2 .
[0032] Preferably, the amount of wear-resistant aggregate spread in the third wear-resistant intermediate layer of paint is 0.5-1 kg / m 2 .
[0033] Preferably, the wear-resistant intermediate layer paint is composed of a wear-resistant intermediate layer paint main material and a wear-resistant intermediate layer paint curing agent as raw materials.
[0034] Preferably, the main material of the wear-resistant intermediate layer paint is a mixture of polyurethane-modified epoxy resin, aluminum oxide, mica powder, aluminum powder, defoamer and wetting dispersant; and the wear-resistant intermediate layer curing agent is a modified alicyclic amine curing agent.
[0035] Preferably, the preparation method of the wear-resistant intermediate layer paint is:
[0036] Add the wear-resistant middle layer curing agent to the wear-resistant middle layer main material, stir for 3 to 5 minutes, and mature for 15 to 20 minutes before coating.
[0037] Preferably, the mass ratio of the main material of the wear-resistant intermediate layer to the curing agent of the wear-resistant intermediate layer is 1.5:1 to 3:1.
[0038] Preferably, the wear-resistant wire mesh is 304L stainless steel wire mesh (20 mesh, wire diameter 0.5mm), 310S stainless steel wire mesh (20 mesh, wire diameter 0.5mm), 321 stainless steel wire mesh (20 mesh, wire diameter 0.5mm), 316L stainless steel wire mesh (20 mesh, wire diameter 0.5mm), galvanized wire mesh (10 mesh, wire diameter 0.32mm), galvanized wire mesh (5 mesh, wire diameter 0.32mm), nylon wire mesh (10 mesh, wire diameter 0.8mm), polyester wire mesh (10 mesh, wire diameter 0.8mm), glass fiber wire mesh (300g / m 2 ) or a combination of .
[0039] Preferably, the wear-resistant aggregate is one or a combination of 15-mesh polyurethane particles, 30-mesh polyurethane particles, 15-mesh silicon carbide particles, 30-mesh silicon carbide particles, 15-mesh quartz sand particles, 30-mesh quartz sand particles, and 50-mesh quartz sand particles.
[0040] Further, in step S4, the coating method of the wear-resistant topcoat is:
[0041] The wear-resistant topcoat must be applied to the surface of the wear-resistant intermediate layer within 8 hours after the wear-resistant intermediate layer is dry, and the wear-resistant topcoat is applied twice by roller coating or spraying. After the first coat of wear-resistant topcoat is completely dry, the second coat of wear-resistant topcoat is applied. The coating methods of the first and second coats of wear-resistant topcoat are the same, and the total dry film thickness of the wear-resistant topcoat is 95 to 105 μm.
[0042] Preferably, the wear-resistant topcoat comprises a main material of the wear-resistant topcoat and a wear-resistant topcoat curing agent. More preferably, the wear-resistant topcoat comprises a main material of the wear-resistant topcoat, a wear-resistant topcoat curing agent and a wear-resistant topcoat thinner.
[0043] Preferably, the main ingredient of the wear-resistant topcoat is a mixture of polyurethane modified epoxy resin, aluminum oxide, mica powder, defoamer, wetting dispersant and diluent; the wear-resistant topcoat curing agent is a modified alicyclic amine curing agent; the wear-resistant topcoat diluent is an organic solvent; preferably xylene, the wear-resistant topcoat diluent can reduce the viscosity of the paint and facilitate coating.
[0044] Preferably, the preparation method of the wear-resistant topcoat is:
[0045] Add the wear-resistant topcoat curing agent and or without the wear-resistant topcoat thinner to the main material of the wear-resistant topcoat, stir for 3 to 5 minutes, and then paint after aging for 15 to 20 minutes.
[0046] Preferably, the mass ratio of the main material of the wear-resistant topcoat to the curing agent of the wear-resistant topcoat is 2.5:1 to 4:1, and the amount of the thinner of the wear-resistant topcoat is less than 10% of the main material of the wear-resistant topcoat.
[0047] Compared with the prior art, the beneficial effects of the present invention are:
[0048] 1. The present invention adopts a three-coating compound system of anti-corrosion primer, wear-resistant intermediate layer paint and wear-resistant topcoat, and adopts different coating construction processes according to the different properties of the three coating materials to form an excellent performance of rolling-resistant, wear-resistant and anti-corrosion coating material, thereby improving the deck's rolling resistance, wear resistance, impact resistance, medium resistance and corrosion resistance.
[0049] 2. The present invention arranges a wear-resistant middle layer in the area of the ship's operating deck that is subjected to heavy loads and prone to wear for a long time, and evenly presses a layer of wear-resistant wire mesh into the wear-resistant middle layer, while spreading wear-resistant aggregates, which significantly improves the deck coating's rolling resistance and wear resistance, and meets the actual transportation needs of the ship for long-term carrying of large hovercraft and heavy tracked vehicles; in addition, by controlling the spreading amount of wear-resistant aggregates, while effectively improving the coating material's wear resistance and rolling resistance, it also takes into account the coating's anti-slip performance and aesthetic effect.
[0050] 3. The present invention selects wear-resistant wire mesh of specific specifications. Through the laying of the wire mesh, the synergistic effect of the wear-resistant aggregate and the wear-resistant coating material, the rolling resistance of the coating material system is greatly improved, which solves the problem that the traditional rolling resistance coating is prone to local cracks, breakage and falling off due to high stress. The coating material is significantly more resistant to the number of times it is rolled over by heavy tracked vehicles, which extends the service life of the coating material and effectively protects the heavy-loaded deck of the ship.
[0051] 4. The construction method provided by the present invention is simple, efficient and has good applicability. While improving the rolling and wear resistance requirements of the heavy-loaded deck of the ship, it also greatly reduces the later maintenance cost of the protective coating material of the heavy-loaded deck. It has a broad prospect for promotion and application, and can also be used in the coating construction of parts on other ships with pressure resistance and wear resistance requirements. DETAILED DESCRIPTION
[0052] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.
[0053] Example 1
[0054] This example is used to illustrate the construction method of rolling-resistant, wear-resistant and anti-corrosion coating materials for heavy-load decks. The specific steps are as follows:
[0055] S1. Surface treatment of metal substrate
[0056] First, remove welding slag, oil stains, dust and other debris on the surface of the substrate, and then remove rust. Rinse the substrate in contact with seawater with fresh water, dry the water-logged area with a heater, and perform shot blasting and rust removal on the steel substrate to Sa2.5 level. Clean up iron filings and sand shots, and wipe the surface with a rag dipped in epoxy thinner.
[0057] S2. Application of anti-corrosion primer
[0058] The anticorrosive primer is applied to the surface of the substrate after rust removal within 3 hours. The weld is painted with a brush, and then the surface of the metal substrate is sprayed. After the first coat of anticorrosive primer is completely dry, the second coat of anticorrosive primer is applied. The coating method of the second coat of anticorrosive primer is the same as the coating method of the first coat of anticorrosive primer. In this embodiment, the total dry film thickness of the anticorrosive primer is 97 μm.
[0059] Among them, in this embodiment, the anticorrosive primer is prepared by adding an anticorrosive primer curing agent and an anticorrosive primer diluent to the main material of the anticorrosive primer, stirring for 3 minutes, and aging for 15 minutes. The mass ratio of the added anticorrosive primer main material and the anticorrosive primer curing agent is 3:1, and the amount of the anticorrosive primer diluent is 8% of the amount of the anticorrosive primer main material. The main material of the anticorrosive primer is a mixture of epoxy resin, mica iron oxide, mica powder, defoamer BYK-085, wetting dispersant BYK-354 and xylene (the mass ratio of each component in the mixture is: 50:20:20:0.2:0.2:20); the anticorrosive primer curing agent is a modified alicyclic amine curing agent; the anticorrosive primer diluent is xylene.
[0060] S3. Coating of wear-resistant intermediate layer
[0061] Separate the mooring holes and deck equipment areas with rubber strips to prevent the wear-resistant intermediate layer material from penetrating into the holes. At intervals of 25cm, evenly trowel a first layer of wear-resistant intermediate layer paint with a width of 1.1m and a thickness of 1.5mm. Lay the wear-resistant wire mesh on the first layer of wear-resistant intermediate layer paint and cover it with a layer of 1m wide PE plastic sheet. Use the plastic sheet to compact the wear-resistant wire mesh, that is, press the wear-resistant wire mesh evenly into the first layer of wear-resistant intermediate layer paint, squeeze out the air between the plastic sheet and the first layer of wear-resistant intermediate layer paint, and after the first layer of wear-resistant intermediate layer paint is completely dry, remove the covering plastic sheet and polish away the protruding and unadhered parts. A firm wear-resistant wire mesh is installed, and then the second wear-resistant intermediate layer paint is troweled on the whole. At the same time, wear-resistant aggregate is evenly spread. The surface of the second wear-resistant intermediate layer paint after spreading the wear-resistant aggregate is rolled evenly with a defoaming roller. After the second wear-resistant intermediate layer paint is completely dry, use an angle grinder to grind off the loosely adhered and accumulated wear-resistant aggregate. After cleaning, the third wear-resistant intermediate layer paint is troweled on. The coating method of the third wear-resistant intermediate layer paint is the same as that of the second wear-resistant intermediate layer paint. The total dry film thickness of the wear-resistant intermediate layer is 3.7mm.
[0062] Among them, in this embodiment, the wear-resistant intermediate layer paint is prepared by adding the wear-resistant intermediate layer curing agent to the wear-resistant intermediate layer main material, stirring for 3 minutes, and aging for 15 minutes, and the mass ratio of the added wear-resistant intermediate layer main material to the wear-resistant intermediate layer curing agent is 1.5:1. The wear-resistant intermediate layer main material is a mixture of polyurethane modified epoxy resin, aluminum oxide, mica powder, aluminum powder, defoamer BYK-085 and wetting dispersant BYK-354 (the mass ratio of each component in the mixture is: 55:10:10:5:0.5:0.5); the wear-resistant intermediate layer curing agent is a modified alicyclic amine curing agent.
[0063] In this embodiment, the wear-resistant wire mesh is 321 stainless steel wire mesh (20 mesh, wire diameter 0.5 mm); the wear-resistant aggregate spread in the wear-resistant middle layer paint is 15 mesh polyurethane particles, and the spread amount is 1.8 kg / m 2 The wear-resistant aggregate in the wear-resistant topcoat is 15 mesh polyurethane particles, and the amount of the particles is 0.5 kg / m 2 ;
[0064] S4. Application of wear-resistant topcoat
[0065] The surface of the dried wear-resistant intermediate layer is coated with a wear-resistant topcoat within 8 hours. Then the wear-resistant topcoat is applied to the surface of the wear-resistant intermediate layer by spraying. After the first coat of the wear-resistant topcoat is completely dry, the second coat of the wear-resistant topcoat is applied. The coating method of the second coat of the wear-resistant topcoat is the same as the coating method of the first coat of the wear-resistant topcoat. In this embodiment, the total dry film thickness of the wear-resistant topcoat is 100 μm.
[0066] Among them, in this embodiment, the wear-resistant topcoat is prepared by adding a wear-resistant topcoat curing agent and a wear-resistant topcoat thinner to the main material of the wear-resistant topcoat, stirring for 3 minutes, and aging for 15 minutes. The mass ratio of the added wear-resistant topcoat main material and the wear-resistant topcoat curing agent is 2:1, and the amount of the wear-resistant topcoat thinner is 8% of the amount of the wear-resistant topcoat main material. The main material of the wear-resistant topcoat is a mixture of polyurethane modified epoxy resin, aluminum oxide, mica powder, defoamer BYK-085, wetting dispersant BYK-354 and xylene (the mass ratio of each component in the mixture is: 45:10:10:0.5:0.5:10); the wear-resistant topcoat curing agent is a modified alicyclic amine curing agent; and the wear-resistant topcoat thinner is xylene.
[0067] After the construction was completed, the deck coating material had excellent rolling resistance. After 40 months of use on the actual ship, the coating was not damaged or peeled off, and the surface condition was good. There was only a small amount of wear and tear from the tracks of heavy vehicles, which met the use requirements well.
[0068] Example 2
[0069] This example is used to illustrate the construction method of rolling-resistant, wear-resistant and anti-corrosion coating materials for heavy-load decks. The specific steps are as follows:
[0070] S1. Surface treatment of metal substrate
[0071] First, remove welding slag, oil stains, dust and other debris on the surface of the substrate, and then remove rust. Rinse the substrate in contact with seawater with fresh water, dry the water-logged area with a heater, and perform shot blasting and rust removal on the steel substrate to Sa2.5 level. Clean up iron filings and sand shots, and wipe the surface with a rag dipped in epoxy thinner.
[0072] S2. Application of anti-corrosion primer
[0073] The anticorrosive primer is applied to the surface of the substrate after rust removal within 5 hours. The weld is painted with a brush, and then the surface of the metal substrate is sprayed. After the first coat of anticorrosive primer is completely dry, the second coat of anticorrosive primer is applied. The coating method of the second coat of anticorrosive primer is the same as the coating method of the first coat of anticorrosive primer. In this embodiment, the total dry film thickness of the anticorrosive primer is 100 μm.
[0074] Among them, in this embodiment, the anticorrosive primer is prepared by adding an anticorrosive primer curing agent and an anticorrosive primer diluent to the main material of the anticorrosive primer, stirring for 3 minutes, and aging for 20 minutes. The mass ratio of the added anticorrosive primer main material and the anticorrosive primer curing agent is 5:1, and the amount of the anticorrosive primer diluent is 7% of the amount of the anticorrosive primer main material. The main material of the anticorrosive primer is a mixture of epoxy resin, mica iron oxide, mica powder, defoamer BYK-085, wetting dispersant BYK-354 and xylene (the mass ratio of each component in the mixture is: 50:20:20:0.2:0.2:20); the anticorrosive primer curing agent is a modified alicyclic amine curing agent; the anticorrosive primer diluent is xylene.
[0075] S3. Coating of wear-resistant intermediate layer
[0076] Separate the mooring holes and deck equipment areas with rubber strips to prevent the wear-resistant intermediate layer material from penetrating into the holes. At intervals of 30cm, evenly trowel a first layer of wear-resistant intermediate layer paint with a width of 1.2m and a thickness of 1.5mm. Lay the wear-resistant wire mesh on the first layer of wear-resistant intermediate layer paint and cover it with a layer of 1m wide PE plastic sheeting. Use the plastic sheeting to compact the wear-resistant wire mesh, that is, press the wear-resistant wire mesh evenly into the first layer of wear-resistant intermediate layer paint, squeeze out the air between the plastic sheeting and the first layer of wear-resistant intermediate layer paint, and after the first layer of wear-resistant intermediate layer paint is completely dry, remove the covering plastic sheeting and polish to remove the protruding, For the wear-resistant wire mesh that is not firmly adhered, then apply the second wear-resistant middle layer paint on the whole, and at the same time evenly spread the wear-resistant aggregate. Use a defoaming roller to roll the surface of the second wear-resistant middle layer paint after spreading the wear-resistant aggregate. After the second wear-resistant middle layer paint is completely dry, use an angle grinder to grind off the wear-resistant aggregate that is not firmly adhered and accumulated. After cleaning, apply the third wear-resistant middle layer paint. The coating method of the third wear-resistant middle layer paint is the same as that of the second wear-resistant middle layer paint. The total dry film thickness of the wear-resistant intermediate layer is 3.6mm.
[0077] Among them, in this embodiment, the wear-resistant intermediate layer paint is prepared by adding the wear-resistant intermediate layer curing agent to the wear-resistant intermediate layer main material, stirring for 3 minutes, and aging for 15 minutes, and the mass ratio of the added wear-resistant intermediate layer main material and the wear-resistant intermediate layer curing agent is 2:1. The main material of the wear-resistant intermediate layer paint is a mixture of polyurethane modified epoxy resin, aluminum oxide, mica powder, aluminum powder, defoamer BYK-085 and wetting dispersant BYK-354 (the mass ratio of each component in the mixture is: 55:10:10:5:0.5:0.5); the wear-resistant intermediate layer curing agent is a modified alicyclic amine curing agent.
[0078] In this embodiment, the wear-resistant wire mesh is galvanized wire mesh (10 mesh, wire diameter 0.32 mm); the wear-resistant aggregate spread in the wear-resistant middle layer paint is 30 mesh silicon carbide, and the spreading amount is 2 kg / m 2 The wear-resistant aggregate spread in the wear-resistant topcoat is 30 mesh silicon carbide, and the spreading amount is 0.8kg / m 2 ;
[0079] S4. Application of wear-resistant topcoat
[0080] The surface of the dried wear-resistant intermediate layer is coated with a wear-resistant topcoat within 8 hours. Then the wear-resistant topcoat is sprayed on the surface of the wear-resistant intermediate layer. After the first coat of the wear-resistant topcoat is completely dry, the second coat of the wear-resistant topcoat is applied. The coating method of the second coat of the wear-resistant topcoat is the same as the coating method of the first coat of the wear-resistant topcoat. In this embodiment, the total dry film thickness of the wear-resistant topcoat is 99 μm.
[0081] Among them, in this embodiment, the wear-resistant topcoat is prepared by adding a wear-resistant topcoat curing agent and a wear-resistant topcoat thinner to the main material of the wear-resistant topcoat, stirring for 3 minutes, and aging for 15 minutes. The mass ratio of the added wear-resistant topcoat main material and the wear-resistant topcoat curing agent is 3:1, and the amount of the wear-resistant topcoat thinner is 8% of the amount of the wear-resistant topcoat main material. The main material of the wear-resistant topcoat is a mixture of polyurethane modified epoxy resin, aluminum oxide, mica powder, defoamer BYK-085, wetting dispersant BYK-354 and xylene (the mass ratio of each component in the mixture is: 45:10:10:0.5:0.5:10); the wear-resistant topcoat curing agent is a modified alicyclic amine curing agent; and the wear-resistant topcoat thinner is xylene.
[0082] After the construction was completed, the deck coating material had excellent crushing resistance. After 47 months of use on the actual ship, the coating was not damaged or peeled off, and the surface condition was good. There was only a small amount of wear and tear from the tracks of heavy vehicles, which effectively met the use requirements.
[0083] Example 3
[0084] This example is used to illustrate the construction method of rolling-resistant, wear-resistant and anti-corrosion coating materials for heavy-load decks. The specific steps are as follows:
[0085] S1. Surface treatment of metal substrate
[0086] First, remove welding slag, oil stains, dust and other debris on the surface of the substrate, and then remove rust. Rinse the substrate in contact with seawater with fresh water, dry the water-logged area with a heater, and manually polish and remove rust on the aluminum substrate to St3 level. Clean up iron filings and wipe the surface with a rag dipped in epoxy thinner.
[0087] S2. Application of anti-corrosion primer
[0088] The anti-corrosion primer is applied to the surface of the substrate within 3 hours after rust removal. The weld is painted with a brush, and then the surface of the metal substrate is sprayed. After the first coat of anti-corrosion primer is completely dry, the second coat of anti-corrosion primer is applied. The coating method of the second coat of anti-corrosion primer is the same as the coating method of the first coat of anti-corrosion primer. In this embodiment, the total dry film thickness of the anti-corrosion primer is 95 μm.
[0089] Among them, in this embodiment, the anticorrosive primer is prepared by adding an anticorrosive primer curing agent and an anticorrosive primer diluent to the main material of the anticorrosive primer, stirring for 3 minutes, and aging for 15 minutes. The mass ratio of the added anticorrosive primer main material and the anticorrosive primer curing agent is 4:1, and the amount of the anticorrosive primer diluent is 7% of the amount of the anticorrosive primer main material. The main material of the anticorrosive primer is a mixture of epoxy resin, mica iron oxide, mica powder, defoamer BYK-085, wetting dispersant BYK-354 and xylene (the mass ratio of each component in the mixture is: 50:20:20:0.2:0.2:20); the anticorrosive primer curing agent is a modified alicyclic amine curing agent; the anticorrosive primer diluent is xylene.
[0090] S3. Coating of wear-resistant intermediate layer
[0091] Separate the mooring holes and deck equipment areas with rubber strips to prevent the wear-resistant intermediate layer material from penetrating into the holes. At intervals of 30cm, evenly trowel a first layer of wear-resistant intermediate layer paint with a width of 1.1m and a thickness of 1.6mm. Lay the wear-resistant wire mesh on the first layer of wear-resistant intermediate layer paint and cover it with a layer of 1m wide PE plastic sheet. Use the plastic sheet to compact the wear-resistant wire mesh, that is, press the wear-resistant wire mesh evenly into the first layer of wear-resistant intermediate layer paint, squeeze out the air between the plastic sheet and the first layer of wear-resistant intermediate layer paint, and after the first layer of wear-resistant intermediate layer paint is completely dry, remove the covering plastic sheet, and polish and remove the protruding, For the wear-resistant wire mesh that is not firmly adhered, then apply the second wear-resistant middle layer paint on the whole, and at the same time evenly spread the wear-resistant aggregate. Use a defoaming roller to roll the surface of the second wear-resistant middle layer paint after spreading the wear-resistant aggregate. After the second wear-resistant middle layer paint is completely dry, use an angle grinder to grind off the wear-resistant aggregate that is not firmly adhered and accumulated. After cleaning, apply the third wear-resistant middle layer paint. The coating method of the third wear-resistant middle layer paint is the same as that of the second wear-resistant middle layer paint. The total dry film thickness of the wear-resistant intermediate layer is 3.5mm.
[0092] Among them, in this embodiment, the wear-resistant intermediate layer paint is prepared by adding the wear-resistant intermediate layer curing agent to the wear-resistant intermediate layer main material, stirring for 3 minutes, and aging for 15 minutes, and the mass ratio of the added wear-resistant intermediate layer main material and the wear-resistant intermediate layer curing agent is 3:1. The main material of the wear-resistant intermediate layer paint is a mixture of polyurethane modified epoxy resin, aluminum oxide, mica powder, aluminum powder, defoamer BYK-085 and wetting dispersant BYK-354 (the mass ratio of each component in the mixture is: 55:10:10:5:0.5:0.5); the wear-resistant intermediate layer curing agent is a modified alicyclic amine curing agent.
[0093] In this embodiment, the wear-resistant wire mesh is 304L stainless steel wire mesh (20 mesh, wire diameter 0.5mm); the wear-resistant aggregate spread in the wear-resistant middle layer paint is 30 mesh polyurethane particles, and the spreading amount is 1.8kg / m 2The wear-resistant aggregate in the wear-resistant topcoat is 30 mesh polyurethane particles, and the amount of the particles is 0.6 kg / m 2 ;
[0094] S4. Application of wear-resistant topcoat
[0095] The surface of the dried wear-resistant intermediate layer is coated with a wear-resistant topcoat within 8 hours. Then the wear-resistant topcoat is sprayed on the surface of the wear-resistant intermediate layer. After the first coat of the wear-resistant topcoat is completely dry, the second coat of the wear-resistant topcoat is applied. The coating method of the second coat of the wear-resistant topcoat is the same as the coating method of the first coat of the wear-resistant topcoat. In this embodiment, the total dry film thickness of the wear-resistant topcoat is 98 μm.
[0096] Among them, in this embodiment, the wear-resistant topcoat is prepared by adding a wear-resistant topcoat curing agent and a wear-resistant topcoat thinner to the main material of the wear-resistant topcoat, stirring for 3 minutes, and aging for 15 minutes. The mass ratio of the added wear-resistant topcoat main material and the wear-resistant topcoat curing agent is 4:1, and the amount of the wear-resistant topcoat thinner is 5% of the amount of the wear-resistant topcoat main material. The main material of the wear-resistant topcoat is a mixture of polyurethane modified epoxy resin, aluminum oxide, mica powder, defoamer BYK-085, wetting dispersant BYK-354 and xylene (the mass ratio of each component in the mixture is: 45:10:10:0.5:0.5:10); the wear-resistant topcoat curing agent is a modified alicyclic amine curing agent; and the wear-resistant topcoat thinner is xylene.
[0097] After the construction was completed, the deck coating material had excellent crushing resistance. After 36 months of use on the actual ship, the coating was not damaged or peeled off, and the surface condition was good. There was only a small amount of wear and tear from the tracks of heavy vehicles, which effectively met the use requirements.
[0098] Comparative Example 1
[0099] This comparative example is used to illustrate the construction method of the rolling-resistant, wear-resistant and anti-corrosion coating material for heavy-load decks. The specific steps are as follows:
[0100] S1. Surface treatment of metal substrate
[0101] First, remove welding slag, oil stains, dust and other debris on the surface of the substrate, and then remove rust. Rinse the substrate in contact with seawater with fresh water, dry the water-logged area with a heater, and manually grind and remove rust on the steel substrate to St3 level. Clean up iron filings and wipe the surface with a rag dipped in epoxy thinner.
[0102] S2. Application of anti-corrosion primer
[0103] After rust removal, the surface of the substrate is coated with an anticorrosive primer within 3 hours. Use a brush dipped in paint to paint the weld area, and then use a roller to paint the surface of the metal substrate. After the first coat of anticorrosive primer is completely dry, the second coat of anticorrosive primer is applied. The coating method of the second coat of anticorrosive primer is the same as the coating method of the first coat of anticorrosive primer. In this embodiment, the total dry film thickness of the anticorrosive primer is 100 μm.
[0104] Among them, in this embodiment, the anticorrosive primer is prepared by adding an anticorrosive primer curing agent and an anticorrosive primer diluent to the main material of the anticorrosive primer, stirring for 3 minutes, and aging for 15 minutes. The mass ratio of the added anticorrosive primer main material and the anticorrosive primer curing agent is 4:1, and the amount of the anticorrosive primer diluent is 7% of the amount of the anticorrosive primer main material. The main material of the anticorrosive primer is a mixture of epoxy resin, mica iron oxide, mica powder, defoamer BYK-085, wetting dispersant BYK-354 and xylene (the mass ratio of each component in the mixture is: 50:20:20:0.2:0.2:20); the anticorrosive primer curing agent is a modified alicyclic amine curing agent; the anticorrosive primer diluent is xylene.
[0105] S3. Coating of wear-resistant intermediate layer
[0106] Separate the mooring hole and the deck equipment area with rubber strips to prevent the wear-resistant intermediate layer material from penetrating into the hole. Then, the wear-resistant intermediate paint is applied to the surface of the anti-corrosion primer by trowel coating. After the first coat of the wear-resistant intermediate paint is completely dry, the second coat of the wear-resistant intermediate paint is applied. The coating method of the second coat of the wear-resistant intermediate paint is the same as that of the first coat of the wear-resistant intermediate paint. In this embodiment, the total dry film thickness of the wear-resistant intermediate paint is 95 μm;
[0107] Among them, in this embodiment, the wear-resistant intermediate layer paint is prepared by adding the wear-resistant intermediate layer curing agent to the wear-resistant intermediate layer main material, stirring for 3 minutes, and aging for 15 minutes, and the mass ratio of the added wear-resistant intermediate layer main material and the wear-resistant intermediate layer curing agent is 3:1. The main material of the wear-resistant intermediate layer paint is a mixture of polyurethane modified epoxy resin, aluminum oxide, mica powder, aluminum powder, defoamer BYK-085 and wetting dispersant BYK-354 (the mass ratio of each component in the mixture is: 55:10:10:5:0.5:0.5); the wear-resistant intermediate layer curing agent is a modified alicyclic amine curing agent.
[0108] S4. Application of wear-resistant topcoat
[0109] The surface of the dried wear-resistant intermediate paint is coated with a wear-resistant topcoat within 8 hours. Then the wear-resistant topcoat is sprayed on the surface of the wear-resistant intermediate layer. After the first coat of the wear-resistant topcoat is completely dry, the second coat of the wear-resistant topcoat is applied. The coating method of the second coat of the wear-resistant topcoat is the same as the coating method of the first coat of the wear-resistant topcoat. In this embodiment, the total dry film thickness of the wear-resistant topcoat is 100 μm.
[0110] Among them, in this embodiment, the wear-resistant topcoat is prepared by adding a wear-resistant topcoat curing agent and a wear-resistant topcoat thinner to the main material of the wear-resistant topcoat, stirring for 3 minutes, and aging for 15 minutes. The mass ratio of the added wear-resistant topcoat main material and the wear-resistant topcoat curing agent is 4:1, and the amount of the wear-resistant topcoat thinner is 5% of the amount of the wear-resistant topcoat main material. The main material of the wear-resistant topcoat is a mixture of polyurethane modified epoxy resin, aluminum oxide, mica powder, defoamer BYK-085, wetting dispersant BYK-354 and xylene (the mass ratio of each component in the mixture is: 45:10:10:0.5:0.5:10); the wear-resistant topcoat curing agent is a modified alicyclic amine curing agent; and the wear-resistant topcoat thinner is xylene.
[0111] After the construction was completed, it was verified through 36 months of use on the actual ship that the coating was severely damaged at the track rolling point and could not meet the use requirements.
Claims
1. A construction method of a rolling-resistant, wear-resistant and corrosion-resistant coating material for a heavy-load deck, characterized in that: The following steps are involved: S1. Surface treatment of metal substrate The surface of the metal substrate is treated with welding slag, oil stains, dust and rust removal; after the metal substrate is polished, the debris is cleaned and the surface is wiped clean with epoxy thinner; S2. Application of anti-corrosion primer Applying an anti-corrosion primer on the surface of the metal substrate treated in step S1, wherein the total dry film thickness of the anti-corrosion primer is 95 to 105 μm; The anticorrosive primer is composed of raw materials including an anticorrosive primer main material and an anticorrosive primer curing agent; The main material of the anticorrosive primer is a mixture of epoxy resin, mica iron oxide, mica powder, defoamer, wetting dispersant and diluent; The anticorrosive primer curing agent is a modified alicyclic amine curing agent; S3. Coating of wear-resistant intermediate layer Applying a wear-resistant intermediate layer on the anti-corrosion primer applied in step S2, wherein the wear-resistant intermediate layer is provided with a wear-resistant wire mesh and wear-resistant aggregate, wherein the wear-resistant wire mesh is evenly distributed at the bottom of the wear-resistant intermediate layer, and the wear-resistant aggregate is evenly distributed in the wear-resistant intermediate layer; The coating method of the wear-resistant intermediate layer is: On the surface of the anticorrosive primer, apply the first wear-resistant intermediate layer paint with a width of 1.1 to 1.2 m and a thickness of 1.5 to 1.6 mm at intervals of 25 to 30 cm, press into the wear-resistant wire mesh, wait for the first wear-resistant intermediate layer paint to dry completely, apply the second wear-resistant intermediate layer paint on the entire area of the anticorrosive primer, and evenly spread the wear-resistant aggregate at the same time, wait for the second wear-resistant intermediate layer paint to dry completely, apply the third wear-resistant intermediate layer paint on the second wear-resistant intermediate layer paint, and evenly spread the wear-resistant aggregate at the same time; The wear-resistant intermediate layer paint is composed of raw materials including a main material of the wear-resistant intermediate layer paint and a wear-resistant intermediate layer paint curing agent; The main material of the wear-resistant intermediate layer paint is a mixture of polyurethane modified epoxy resin, aluminum oxide, mica powder, aluminum powder, defoamer and wetting dispersant; The wear-resistant intermediate layer curing agent is a modified alicyclic amine curing agent; The wear-resistant wire mesh is one or a combination of stainless steel wire mesh, galvanized wire mesh, nylon wire mesh, polyester wire mesh, and glass fiber wire mesh; The wear-resistant aggregate is one or a combination of polyurethane particles, silicon carbide particles, and quartz sand particles; The amount of the wear-resistant aggregate spread in the second wear-resistant intermediate layer of paint is 1.5-2 kg / m 2 ; The amount of the wear-resistant aggregate spread in the third wear-resistant intermediate layer of paint is 0.5-1 kg / m 2 ; S4. Application of wear-resistant topcoat Applying a wear-resistant topcoat on the surface of the wear-resistant intermediate layer applied in step S3, wherein the total dry film thickness of the wear-resistant topcoat is 95 to 105 μm; The wear-resistant topcoat is composed of raw materials including a main material of the wear-resistant topcoat and a curing agent for the wear-resistant topcoat; The main material of the wear-resistant topcoat is a mixture of polyurethane-modified epoxy resin, aluminum oxide, mica powder, defoamer, wetting dispersant and diluent; The wear-resistant topcoat curing agent is a modified alicyclic amine curing agent.
2. The construction method of the rolling-resistant, wear-resistant and corrosion-resistant coating material for heavy-load decks according to claim 1 is characterized in that: In the step S1, The metal substrate is one of steel and aluminum; The metal substrate is derusted to Sa2.5 or St3 level, and after polishing, the surface is cleaned with epoxy thinner.
3. The construction method of the rolling-resistant, wear-resistant and corrosion-resistant coating material for heavy-load decks according to claim 2 is characterized in that: In the step S2, the method of applying the anticorrosive primer is: Within 8 hours, the surface of the metal substrate treated in step S1 is coated with the anticorrosive primer, and the anticorrosive primer is coated twice. After the first coat of the anticorrosive primer is completely dry, the second coat of the anticorrosive primer is coated.
4. The construction method of the rolling-resistant, wear-resistant and corrosion-resistant coating material for heavy-load decks according to claim 3 is characterized in that: In the step S2, The anticorrosive primer is composed of raw materials including an anticorrosive primer main material, an anticorrosive primer curing agent and an anticorrosive primer diluent; The anticorrosive primer diluent is an organic solvent.
5. The construction method of the rolling-resistant, wear-resistant and corrosion-resistant coating material for heavy-load decks according to claim 4 is characterized in that: The anticorrosive primer thinner is xylene.
6. The construction method of the rolling-resistant, wear-resistant and corrosion-resistant coating material for heavy-load decks according to claim 4 is characterized in that: The preparation method of the anticorrosive primer is: Add the anti-corrosion primer curing agent and / or the anti-corrosion primer thinner to the main material of the anti-corrosion primer, stir for 3 to 5 minutes, and mature for 15 to 20 minutes before painting.
7. The construction method of the rolling-resistant, wear-resistant and corrosion-resistant coating material for heavy-load decks according to claim 4 is characterized in that: The mass ratio of the anticorrosive primer main material to the anticorrosive primer curing agent is 3:1-5:1, and the amount of the anticorrosive primer diluent is less than 10% of the amount of the anticorrosive primer main material.
8. The construction method of the rolling-resistant, wear-resistant and corrosion-resistant coating material for heavy-load decks according to claim 1 is characterized in that: The preparation method of the wear-resistant intermediate layer paint is: Add the wear-resistant middle layer curing agent to the wear-resistant middle layer main material, stir for 3 to 5 minutes, and mature for 15 to 20 minutes before coating.
9. The construction method of the rolling-resistant, wear-resistant and corrosion-resistant coating material for heavy-load decks according to claim 1 is characterized in that: The mass ratio of the main material of the wear-resistant intermediate layer to the curing agent of the wear-resistant intermediate layer is 1.5:1 to 3:
1.
10. The construction method of the rolling-resistant, wear-resistant and corrosion-resistant coating material for heavy-load decks according to claim 1 is characterized in that: In the step S3, the particle size of the wear-resistant aggregate ranges from 15 to 50 meshes.
11. The construction method of the rolling-resistant, wear-resistant and corrosion-resistant coating material for heavy-load decks according to claim 1 is characterized in that: In the step S4, the coating method of the wear-resistant topcoat is: Within 8 hours, the surface of the wear-resistant intermediate layer treated in step S3 is coated with a wear-resistant topcoat, and the wear-resistant topcoat is coated twice. After the first coat of the wear-resistant topcoat is completely dry, the second coat of the wear-resistant topcoat is coated.
12. The construction method of the rolling-resistant, wear-resistant and corrosion-resistant coating material for heavy-load decks according to claim 11 is characterized in that: In the step S4, The wear-resistant topcoat is composed of raw materials including a main material of the wear-resistant topcoat, a wear-resistant topcoat curing agent and a wear-resistant topcoat diluent; The wear-resistant topcoat thinner is an organic solvent.
13. The construction method of the rolling-resistant, wear-resistant and corrosion-resistant coating material for heavy-load decks according to claim 12 is characterized in that: The wear-resistant topcoat thinner is xylene.
14. The construction method of the rolling-resistant, wear-resistant and corrosion-resistant coating material for heavy-load decks according to claim 12, characterized in that: The preparation method of the wear-resistant topcoat is: Add the wear-resistant topcoat curing agent and / or the wear-resistant topcoat thinner to the main material of the wear-resistant topcoat, stir for 3 to 5 minutes, and mature for 15 to 20 minutes before coating.
15. The construction method of the rolling-resistant, wear-resistant and corrosion-resistant coating material for heavy-load decks according to claim 14 is characterized in that: The mass ratio of the main material of the wear-resistant topcoat to the curing agent of the wear-resistant topcoat is 2.5:1-4:1, and the amount of the thinner of the wear-resistant topcoat is less than 10% of the main material of the wear-resistant topcoat.